A carbon material / metal modified doped diamond particle integrated sensor and its preparation method and application
By depositing a polycrystalline doped diamond film on the surface of the carrier particles and providing a carbon material or metal modification layer, optimized doped diamond particles are formed, which solves the problems of uneven resistance and impurities in the existing boron-doped diamond electrodes, and achieves a variety of The high sensitivity and conductivity of substance detection reduce production costs.
Patent Information
- Application Number
- CN202111084124.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-15
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-09-15
AI Technical Summary
Existing boron-doped diamond electrodes have problems such as uneven resistance, metal impurities affecting quality, poor corrosion resistance, high thermal expansion coefficient, low electrocatalytic activity, poor selectivity and sensitivity, and difficulty in mass production, and the sensor can only detect a single substance. .
Integrated sensors using carbon material/metal modified doped diamond particles are used to form optimized doped diamond particles by depositing a polycrystalline doped diamond film on the surface of the carrier particle and setting a carbon material or metal modification layer on its surface. For the detection of various electroactive substances.
It realizes the detection of a variety of electroactive substances, has good linear response and high detection sensitivity, excellent conductive properties, chemically inert surface, and low cost.
Smart Images

Figure CN113777142B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of diamond electrode preparation, and in particular relates to a carbon material / metal-modified doped diamond particle integrated sensor and a preparation method and application thereof. Background Art
[0002] Artificial diamond is a superhard material, but it has very few applications in other areas. After boron doping, the resistance of diamond can be greatly reduced. At present, the boron-doped diamond mainly includes single crystal and polycrystalline boron-containing diamond particles, as well as boron-doped diamond films. Among them, boron-containing gold diamond particles are mainly prepared by high temperature and high pressure method. The particles prepared by this method are mainly single crystal diamond, which has the problems of uneven B concentration distribution and low B concentration. In addition, because metals such as Ni and Fe are needed as catalysts in the preparation process, the prepared particle electrodes contain more metal impurities, which to some extent affects the quality of BDD particles.
[0003] Although the existing BDD film has advantages such as wide potential window, good chemical stability and weak surface adsorption, most of the existing BDD materials are based on metal or silicon wafers, but as a substrate material for BDD, there are some fatal defects. The metal matrix has the advantages of high strength, good toughness and strong plasticity, but as the matrix of the electrode, it has the problems of poor corrosion resistance and high thermal expansion coefficient. In addition, the existing BDD electrode has the disadvantages of low electrocatalytic activity, poor selectivity and sensitivity, and difficulty in large-scale production, which limits its application. In addition, the current sensor based on the BDD electrode can only detect a single substance. Summary of the invention
[0004] In view of the deficiencies in the prior art, the object of the present invention is to provide a carbon material / metal modified doped diamond particle integrated sensor and a preparation method thereof and a preparation method and application thereof.
[0005] In order to achieve the above object, the present invention adopts the following technical solution.
[0006] The present invention discloses a carbon material / metal modified doped diamond particle integrated sensor, comprising a working electrode, a counter electrode, a reference electrode, and a substrate. The working electrode is composed of at least one doped diamond particle. The doped diamond particle comprises a carrier particle, a coating layer, and a modification layer from the inside to the outside. The carrier particle is a boron-containing diamond particle or a pure diamond particle. The coating layer is a doped diamond film. The doping element is selected from one or more of boron, nitrogen, and phosphorus, preferably boron. The modification layer is selected from at least one of carbon material modification and metal modification.
[0007] The present invention provides a carbon material / metal modified doped diamond particle integrated sensor, which can be provided with a plurality of working electrodes on a substrate, and any one of the working electrodes can realize the detection of a variety of electroactive substances through different modification methods.
[0008] In a preferred embodiment, the carrier particles are of a single crystal structure, and the doped diamond film is of a polycrystalline structure.
[0009] The inventors have found that using single-crystal boron-containing diamond particles or diamond particles as carrier particles and then depositing a polycrystalline doped diamond film on their surface can greatly improve the conductivity of the boron-containing diamond particles or diamond particles.
[0010] In the present invention, the carrier particles used can be natural or artificially synthesized, and are preferably prepared by high temperature and high pressure to reduce costs.
[0011] In a preferred embodiment, the concentration of the doping element in the doped diamond film is greater than 10 21 cm -3 , preferably 10 21 cm -3~ 10 22 cm -3 .
[0012] When the content of the doped diamond film is controlled within the above range, the performance of the finally obtained doped diamond particles is optimal. This is because when the doping concentration is greater than 10 18 cm -3 When the insulating diamond has semiconductor properties, when it is greater than 10 21 cm -3 When the doping element is too high, metal-like properties can be obtained. However, due to the different lattice coefficients of the doping element and diamond, excessive doping will cause the diamond lattice to be destroyed and produce impurity phases (such as sp 2 )), resulting in the loss of some excellent properties of diamond such as high hardness, high strength and inert surface. Controlling the doping concentration in the doped diamond film within the above range will achieve optimal performance in collaboration with the carrier particles.
[0013] Preferably, the doping method of the doped diamond film includes one or more combinations of constant doping, multi-layer variable doping, and gradient doping.
[0014] In a preferred solution, the particle size of the carrier particles is 100 nm-500 μm, preferably 100 nm-300 μm, and more preferably 100 nm-100 μm, and the thickness of the doped diamond film is 5 μm-20 μm.
[0015] The inventors have found that by setting the thickness of the doped diamond film within the above range, completely uniformly coated doped diamond particles with the best performance can be obtained.
[0016] In a preferred embodiment, the doped diamond film is a doped diamond film with a porous structure, and the diameter of the holes in the doped diamond film is 10 nm-200 nm.
[0017] Providing micropores on the surface of the doped diamond film can further increase the specific surface area of the particles and improve their performance.
[0018] In the present invention, there are no excessive restrictions on the setting of the multiple holes, such as metal etching treatment, high temperature atmosphere etching treatment, and plasma etching in the prior art.
[0019] In a preferred embodiment, the carbon material in the carbon material modification is selected from at least one of microcrystalline graphite, carbon nanotubes, carbon nanofibers, and graphene, and the metal in the metal modification is selected from at least one of iron, copper, platinum, silver, and gold.
[0020] In a preferred embodiment, the reference electrode is Ag / AgCl, and the counter electrode is Au nanoparticles.
[0021] In the present invention, the working electrode is connected to the Au nanoparticles on the substrate through conductive silver glue or metal welding, and epoxy resin is used as a conductive glue to be coated on the edge of the electrode for fixing.
[0022] In a preferred embodiment, the material of the substrate is selected from one of silicon and germanium semiconductors, polyimide (PI), polydimethylsiloxane (PDMS), and polyethylene terephthalate (PET).
[0023] The present invention provides a method for preparing a carbon material / metal-modified doped diamond particle integrated sensor, comprising the following steps:
[0024] Step 1 Preparation of doped diamond particles
[0025] First, nano-diamond seed crystals are planted on the surface of carrier particles, and then the carrier particles planted with diamond seed crystals are subjected to chemical vapor deposition to grow doped diamond films, and a carbon material modification layer and / or a metal modification layer are arranged on the surface of the doped diamond film to obtain doped diamond particles;
[0026] Step 2: Sensor assembly
[0027] First, the substrate is exposed to UV light, and the electrode layout on the substrate surface is constructed through a mask. Then, Au nanoparticles are deposited on the substrate surface by chemical plating. Then, silver paste is applied to the substrate surface and heated. The substrate coated with silver paste is immersed in a solution containing chloride ions to form an Ag / AgCl reference electrode on the substrate surface. Finally, at least one doped diamond particle is fixed on the substrate and connected to the Au nanoparticles to obtain an integrated sensor.
[0028] In the step 1 of the present invention, during the preparation of the doped diamond particles, since the carrier particles and the doped diamond film have similar structures and are easy to nucleate, conventional chemical vapor deposition methods can be used to grow excellent boron-doped diamond films. However, the inventors have found that the carrier particles can be better coated by cooling down every 3-6 hours of growth, taking out the carrier particles, and then heating up to the target temperature and growing them in multiple times, so that the performance of the doped diamond particles finally obtained is optimal.
[0029] In a preferred embodiment, in step 1, the process of planting nano-diamond seed crystals on the surface of the carrier particles is as follows: immersing the carrier particles in a suspension containing nano-diamonds and ultrasonically vibrating for ≥30 minutes, and finally washing and drying. The mass fraction of nano-diamonds in the suspension containing nano-diamonds is 0.01-0.1wt%.
[0030] In a preferred embodiment, in step 1, the process of chemical vapor deposition growth of doped diamond film is as follows: the mass flow ratio of the gas is hydrogen: methane: doping gas source = 98:2:0.3-0.6, the growth pressure is 2-5Kpa, the growth temperature is 800-850°C, the number of growths is 2-6 times, preferably 5 times, each time the growth is performed, the carrier particles are taken out, the carrier particles are shaken, and then the growth is continued, and the single growth time is 3-6h, and the doping gas source is selected from at least one of ammonia, phosphine, and borane;
[0031] Further preferably, the chemical vapor deposition is hot wire chemical vapor deposition, and the temperature of the hot wire is 2500-2700°C.
[0032] In a preferred embodiment, in step one, the process of setting the carbon material modification layer is as follows: first, a metal nickel layer is deposited on the surface of the doped diamond film by magnetron sputtering; the thickness of the metal nickel layer is 2-22 nm; then, the doped diamond particles covered with the metal nickel layer are thermally catalyzed to grow carbon material on the surface of the doped diamond film to form a carbon material modification layer; the carbon material includes one or more of microcrystalline graphite, carbon nanotubes, carbon nanofibers, and graphene.
[0033] Further preferably, the magnetron sputtering process is: using a nickel target with a purity of ≥99.99%, a distance between the substrate and the target of 10-12 cm, an argon atmosphere, a deposition pressure of 0.4-0.6 Pa, a sputtering power of 150 W, and a deposition time of 60 s.
[0034] Further preferably, when the carbon material is selected from microcrystalline graphite, the thermal catalytic process is: introducing 97-100 sccm of hydrogen, the thermal catalytic temperature is 750-800°C, the thermal catalytic gas pressure is 9-11 kPa, the thermal catalytic time is 1-1.2h, the heating rate is 18-22°C / min, and the cooling rate is 18-22°C / min;
[0035] When the carbon material is selected from carbon nanotubes, the thermal catalysis process is as follows: introducing 28.5 sccm of hydrogen and 1.5-2.0 sccm of methane, the thermal catalysis temperature is 750-800°C, the thermal catalysis pressure is 10 kPa, the thermal catalysis time is 35-40 min, the heating rate is 195-205°C / min, and the cooling rate is 195-205°C / min;
[0036] When the carbon material is selected from carbon nanofibers, the thermal catalysis process is as follows: introducing 28.5 sccm of hydrogen and 1.5-2.0 sccm of methane, the thermal catalysis temperature is 950-1000°C, the thermal catalysis pressure is 10 kPa, the thermal catalysis time is 30-40 min, the heating rate is 195-205°C / min, and the cooling rate is 195-205°C / min;
[0037] When the carbon material is selected from graphene, the thermal catalysis process is: introducing 98 sccm of hydrogen, the thermal catalysis temperature is 750-800°C, the thermal catalysis gas pressure is 10 kPa, the thermal catalysis time is 5 minutes, the heating rate is 195-205°C / min, and the cooling rate is 195-205°C / min.
[0038] In a preferred embodiment, in step 1, the process of setting the metal modification layer is as follows: a metal layer is deposited on the surface of the doped diamond film by magnetron sputtering; the thickness of the metal layer is 2-22 nm; the process of the magnetron sputtering is as follows: the purity of the target material is ≥99.9%, the target material is selected from at least one of iron, copper, platinum, silver and gold, the distance between the substrate and the target material is 10-15 cm, an argon atmosphere is adopted, the deposition pressure is 0.6-2 Pa, the sputtering power is 150-300 W, and the deposition time is 60-120 s; the doped diamond particles after sputtering are placed in a heat pipe furnace for heat treatment, so that the metal layer is spheroidized into nanoparticle clusters with a grain size of 20-500 nm, the gas pressure is maintained at 15-20 kPa, the heat treatment temperature is 900° C., the heat treatment time is 4-5 h, and the mass flow ratio of the introduced atmosphere is H2:Ar=1.5-3.
[0039] In the preferred embodiment, in step 2, the process of depositing Au nanoparticles on the substrate surface is as follows: the substrate with the electrode layout is aminated in an amination solution containing ethylenediamine (0.4 M) and EDC (50 mM) for 180 min, and then the substrate is ammoniated with HAuCl in a dark environment. 4 The substrate was treated with a 1 mM solution for 80-200 min, and then treated with NaBH 4 The PET substrate was treated with a 0.1M solution for 5-50 min, and then the substrate was ultrasonically treated in a KSCN (0.5M) solution for 1 h. 2 SO 3 , 0.6 M formaldehyde and 8 mM Na 3 Au(SO 3 ) 2 The Au plating solution was placed in the solution for 120 min, rinsed with deionized water and washed with N 2 Dry substrate.
[0040] In a preferred embodiment, in step 2, the heating treatment is performed for 60 minutes at a temperature of 60°C.
[0041] In the preferred embodiment, in step 2, the substrate coated with silver paste is immersed in 30 μL 0.1 M FeCl 3 After 60 s in the solution, a Ag / AgCl reference electrode was formed on the substrate surface.
[0042] The present invention also provides an application of a carbon material / metal-modified doped diamond particle integrated sensor, and the carbon material / metal-modified doped diamond particle integrated sensor is used for electrochemical detection.
[0043] In actual application, when the working electrode is a single particle, it can detect a single active molecule, such as modified Au to detect -DA molecules. When the working electrode is a plurality of doped diamond particles with different modifications, it can detect multiple active molecules at the same time. For example, carrying Ni-modified doped diamond particles and Au-modified doped diamond particles at the same time can detect glucose and dopamine at the same time.
[0044] Beneficial Effects
[0045] The carbon material / metal modified doped diamond particle integrated sensor provided by the present invention can be provided with multiple working electrodes on a substrate, and any one of the working electrodes can detect a variety of electroactive substances through different modification methods, and has good linear response and high detection sensitivity.
[0046] The present invention is the first to use diamond particles or boron-containing diamond particles synthesized at high temperature and high pressure as carrier particles, and grow polycrystalline doped diamond films on their surfaces. The resulting doped diamond particles have excellent conductivity, high specific surface area, and are non-toxic to the environment and have a high signal-to-noise ratio. In addition, because commercial particle electrodes contain impurities such as Fe and Ni, they are easy to adsorb substances. The polycrystalline film produced is mainly composed of sp 3 The diamond phase has a saturated structure, so the surface is chemically inert and does not easily adsorb other substances.
[0047] The present invention adopts the method of vapor deposition in the growth process. Taking boron-doped diamond film as an example, the vapor deposition method for preparing polycrystalline diamond is to use methane (CH 4 ), acetylene and other hydrocarbons, hydrogen (H 2 ) and borane are introduced into the reaction chamber, the gas concentration is adjustable and the ratio is uniform, so the boron-doped diamond film prepared by the vapor deposition method has high B doping uniformity and is easy to prepare highly doped films. The present invention adopts a multiple growth method and effectively controls the crystal structure, the thickness of the film, and the doping amount, and ultimately makes the performance of the obtained doped diamond particles the best.
[0048] The preparation method of the invention is simple and controllable, and the carrier particles used are diamond particles or boron-containing diamond particles with a single crystal structure synthesized under high temperature and high pressure, which are commercially available as carrier particles, and are inexpensive and low in cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 The microstructure of the boron-doped diamond particles prepared in Example 1, wherein Figure 1 (a) is a SEM image of a single-crystal boron-containing diamond coated with a polycrystalline B-doped diamond film. (b) is a magnified image of a polycrystalline boron-doped diamond film. (c) is a Raman spectrum of a polycrystalline diamond film.
[0050] Figure 2 The microstructure of the boron-doped diamond particles prepared in Example 2, wherein Figure 1 (a) is a SEM image of a single-crystal boron-containing diamond coated with a polycrystalline B-doped diamond film. (b) is a magnified image of a polycrystalline boron-doped diamond film. (c) is a Raman spectrum of a polycrystalline diamond film.
[0051] Figure 3 The microstructure of the boron-doped diamond particles prepared in the comparative example.
[0052] Figure 4 Schematic diagram of the sensor, in which: 1. doped diamond particles; 2. Au nanoparticles; 3. Ag / AgCl; 4. substrate.
[0053] Figure 5 Schematic diagram of Ni-modified doped diamond particles (the blue dots are Ni).
[0054] Figure 6 Au modified particle BDD electrode (yellow dots are Au). DETAILED DESCRIPTION
[0055] Example 1
[0056] Preparation of Boron-doped Diamond Particles
[0057] (1) First, the boron-containing diamond particles with an average particle size of 150 μm are cleaned.
[0058] (2) Immersing in a suspension containing nano-diamonds and ultrasonically vibrating for 30 minutes, cleaning and drying. The nano-diamonds are placed in the suspension containing nano-diamonds, and the mass fraction of the nano-diamonds is 0.01 wt%.
[0059] (3) A boron-doped diamond film was deposited by hot-wire CVD, and the deposition process parameters were as follows: hot-wire distance 6 mm, growth temperature 800-850°C, hot-wire temperature 2200°C, deposition pressure 3 KPa, and a diamond film thickness of 50 μm was obtained by controlling the deposition time; during the chemical vapor deposition, the mass flow ratio of the gas was hydrogen: methane: borane = 98:2:0.3, the growth pressure was 2 KPa, and the number of growths was 2 times. After each growth, the carrier particles were taken out, and the carrier particles were shaken before continuing to grow. The single growth time was 6 hours.
[0060] Figure 1 (a) is the SEM image of a single crystal B-doped diamond coated with a polycrystalline B-doped diamond film. (b) is the magnified image of the polycrystalline film. (c) is the Raman peak of the polycrystalline diamond film with a high B-doping degree, showing a typical B peak (479 cm -1 and 1200cm -1 ), less graphite phase (G peak: 1530cm -1 ), and the concentration of B is greater than 10 21 cm -1 , indicating that it is a heavily B-doped material.
[0061] Preparation of Au-modified boron-doped diamond particles
[0062] A metal Au layer is deposited on the surface of a boron-doped diamond layer by magnetron sputtering; the thickness of the metal Au layer is 2-22 nm; the process of the magnetron sputtering is as follows: an Au target with a purity of ≥99.99%, a distance between a substrate and a target material of 10-15 cm, an argon atmosphere, a deposition pressure of 0.6 Pa, a sputtering power of 150 W, and a deposition time of 60 s.
[0063] The sputtered electrode is placed in a heat tube furnace for heat treatment to spheroidize the metal Au layer into nanoparticle clusters with a grain size of 20-500nm. The gas pressure is maintained at 15kpa, the heat treatment temperature is 900℃, the heat treatment time is 4h, and the mass flow ratio of the introduced atmosphere is H2:Ar=1.5.
[0064] Sensor Assembly
[0065] (1) A clean PET sheet (5 cm × 5 cm, 0.05-0.5 mm thick) was used as a flexible substrate at 9 mW / cm 2 The substrate was exposed to UV light (254 nm) for 240 min, and the electrode layout on the substrate surface was constructed through a mask.
[0066] (2) The substrate was aminated in an amination solution containing ethylenediamine (0.4 M) and EDC (50 mM) for 180 min.
[0067] (3) Using HAuCl 4 (1 mM) and NaBH 4 The PET substrate was treated with a 0.1M solution to adsorb Au nanoparticles. The treatment time of the former was 80-200 min in a dark environment, while the treatment time of the latter was 5-50 min.
[0068] (4) Ultrasonic treatment in KSCN (0.5 M) solution for 1 h to eliminate nonspecific adsorption.
[0069] (5) Place the activated PET substrate in a 0.125M Na 2 SO 3 , 0.6 M formaldehyde and 8 mM Na 3 Au(SO 3 ) 2 The Au plating solution was kept for about 120 minutes.
[0070] (6) Rinse with deionized water and N 2 After drying the substrate, silver paste was applied to the reference electrode to prepare for the subsequent preparation of the Ag / AgCl reference electrode.
[0071] (7) Before use, the prepared substrate was heated at 60°C for about 60 minutes.
[0072] After each of the above processes, rinse with deionized water and 2 dry
[0073] Immerse the Ag-coated electrode in 30 μL of 0.1 M FeCl 3 The Ag / AgCl reference electrode was prepared in the solution for 60 s.
[0074] The doped diamond particles containing the gold modification layer are connected to the Au on the substrate through conductive silver glue or metal welding, and epoxy resin is used as a conductive glue to be coated on the edge of the electrode for fixing.
[0075] The electrochemical potential window of the Au-modified boron-doped diamond microelectrode obtained in this example is as high as 3.3V; it has a good linear response in the concentration range of 0.05-100μM for dopamine detection, and the detection sensitivity is as high as 135μA·μM-1·cm-2. The Ni-modified boron-doped diamond microelectrode obtained in this example has a good linear response in the concentration range of 0.05-13μM for glucose detection, and the detection sensitivity is as high as 330μA·μM-1·cm-2.
[0076] Example 2
[0077] (1) First, the boron-containing diamond particles with an average particle size of 300 μm are cleaned.
[0078] (2) Immersing in a suspension containing nano-diamonds and ultrasonically vibrating for 30 minutes, cleaning and drying. Putting into the suspension containing nano-diamonds, the mass fraction of nano-diamonds is 0.1wt%.
[0079] (3) Boron-doped diamond film was deposited by hot wire CVD. The deposition process parameters were as follows: hot wire distance 6 mm, growth temperature 800-850°C, hot wire temperature 2200°C, deposition pressure 4 KPa, gas ratio hydrogen: methane: borane = 98:2:0.5. By controlling the deposition time, the diamond film thickness of 10 μm was obtained. The number of growths was 4 times. After each growth, the carrier particles were taken out and shaken before continuing to grow. The single growth time was 4 hours.
[0080] Figure 2 (a) is the SEM image of a single crystal B-doped diamond coated with a polycrystalline B-doped diamond film. (b) is the magnified image of the polycrystalline film. (c) is the Raman peak of the polycrystalline diamond film, where the typical B peak (479 cm -1 and 1200cm -1 ), the graphite phase is less (G peak: 1530cm-1), and the B concentration is greater than 10 after fitting. 21 cm -1 , indicating that it is a heavily B-doped material.
[0081] Preparation of Au-modified boron-doped diamond particles
[0082] A metal Au layer is deposited on the surface of a boron-doped diamond layer by magnetron sputtering; the thickness of the metal Au layer is 2-22 nm; the process of the magnetron sputtering is as follows: an Au target with a purity of ≥99.99%, a distance between a substrate and a target material of 10-15 cm, an argon atmosphere, a deposition pressure of 0.6 Pa, a sputtering power of 150 W, and a deposition time of 60 s.
[0083] The sputtered electrode is placed in a heat tube furnace for heat treatment to spheroidize the metal Au layer into nanoparticle clusters with a grain size of 20-500nm. The gas pressure is maintained at 15kpa, the heat treatment temperature is 900℃, the heat treatment time is 4h, and the mass flow ratio of the introduced atmosphere is H2:Ar=1.5.
[0084] Preparation of Ni-modified boron-doped diamond particles
[0085] A metal Au layer is deposited on the surface of a boron-doped diamond layer by magnetron sputtering; the thickness of the metal Ni layer is 2-22 nm; the process of the magnetron sputtering is as follows: a Ni target with a purity of ≥99.99%, a distance between a substrate and a target material of 13 cm, an argon atmosphere, a deposition pressure of 0.7 Pa, a sputtering power of 200 W, and a deposition time of 30 s.
[0086] The sputtered electrode is placed in a heat tube furnace for heat treatment to spheroidize the metal Au layer into nanoparticle clusters with a grain size of 20-500nm. The gas pressure is maintained at 10kpa, the heat treatment temperature is 900℃, the heat treatment time is 4h, and the mass flow ratio of the introduced atmosphere is H2:Ar=1.5.
[0087] Sensor Assembly
[0088] (1) A clean PET sheet (5 cm × 5 cm, 0.05-0.5 mm thick) was used as a flexible substrate at 9 mW / cm 2 The substrate was exposed to UV light (254 nm) for 240 min, and the electrode layout on the substrate surface was constructed through a mask.
[0089] (2) The substrate was aminated in an amination solution containing ethylenediamine (0.4 M) and EDC (50 mM) for 180 min.
[0090] (3) Using HAuCl 4 (1 mM) and NaBH 4 The PET substrate was treated with a 0.1M solution to adsorb Au nanoparticles. The treatment time of the former was 80-200 min in a dark environment, while the treatment time of the latter was 5-50 min.
[0091] (4) Ultrasonic treatment in KSCN (0.5 M) solution for 1 h to eliminate nonspecific adsorption.
[0092] (5) Place the activated PET substrate in a 0.125M Na 2 SO 3 , 0.6 M formaldehyde and 8 mM Na 3 Au(SO 3 ) 2 The Au plating solution was kept for about 120 minutes.
[0093] (6) Rinse with deionized water and N 2 After drying the substrate, silver paste was applied to the reference electrode to prepare for the subsequent preparation of the Ag / AgCl reference electrode.
[0094] (7) Before use, the prepared substrate was heated at 60°C for about 60 minutes.
[0095] After each of the above processes, rinse with deionized water and 2 dry
[0096] Immerse the Ag-coated electrode in 30 μL of 0.1 M FeCl 3 The Ag / AgCl reference electrode was prepared in the solution for 60 s.
[0097] The doped diamond particles containing a gold modification layer and the doped diamond particles containing a nickel modification layer are connected to the Au on the substrate through conductive silver glue or metal welding, and epoxy resin is used as a conductive glue to be coated on the edge of the electrode for fixing.
[0098] The electrochemical potential window of the Au-modified boron-doped diamond microelectrode obtained in this example is as high as 3.2V; it has a good linear response in the concentration range of 0.1-120μM with a detection sensitivity of up to 140μA·μM-1·cm-2 when used for dopamine detection. The Ni-modified boron-doped diamond microelectrode obtained in this example has a good linear response in the concentration range of 0.05-18μM with a detection sensitivity of up to 210μA·μM-1·cm-2 when used for glucose detection.
[0099] Example 3
[0100] (1) First, the boron-containing diamond particles with an average particle size of 300 μm are cleaned.
[0101] (2) Immersing in a suspension containing nano-diamonds and ultrasonically vibrating for 30 minutes, cleaning and drying. Putting into the suspension containing nano-diamonds, the mass fraction of nano-diamonds is 0.1wt%.
[0102] (3) Boron-doped diamond film was deposited by hot-filament CVD. The deposition process parameters were as follows: hot-filament distance 6 mm, growth temperature 800-850°C, hot-filament temperature 2200°C, deposition pressure 4 KPa, gas ratio hydrogen: methane: borane = 98:2:0.6. By controlling the deposition time, a diamond film thickness of 10 μm was obtained. The number of growths was 5 times. After each growth, the carrier particles were taken out and shaken before continuing the growth. The single growth time was 3 h.
[0103] Preparation of Carbon Modified Boron-doped Diamond Particles
[0104] A nickel layer is deposited on the surface of boron-doped diamond by magnetron sputtering. During the deposition process, a high-purity nickel target with a purity of 99.99% is used, the distance between the substrate and the target is 10 cm, an argon atmosphere is used, the deposition pressure is 0.5 Pa, the sputtering power is 150 W, the deposition time is 60 s, and the nickel layer deposition thickness is 20-22 nm.
[0105] Step 4: Microcrystalline graphite phase catalysis: During the catalytic process of microcrystalline graphite, 98 sccm of hydrogen was introduced, the thermal catalytic temperature was 800°C, the thermal catalytic gas pressure was 10 kPa, the thermal catalytic time was 1 h, the heating rate was 20°C / min, and the cooling rate was 20°C / min.
[0106] Sensor Assembly
[0107] (1) A clean PET sheet (5 cm × 5 cm, 0.05-0.5 mm thick) was used as a flexible substrate at 9 mW / cm 2 The substrate was exposed to UV light (254 nm) for 240 min, and the electrode layout on the substrate surface was constructed through a mask.
[0108] (2) The substrate was aminated in an amination solution containing ethylenediamine (0.4 M) and EDC (50 mM) for 180 min.
[0109] (3) Using HAuCl 4 (1 mM) and NaBH 4 The PET substrate was treated with a 0.1M solution to adsorb Au nanoparticles. The treatment time of the former was 80-200 min in a dark environment, while the treatment time of the latter was 5-50 min.
[0110] (4) Ultrasonic treatment in KSCN (0.5 M) solution for 1 h to eliminate nonspecific adsorption.
[0111] (5) Place the activated PET substrate in a 0.125M Na 2 SO 3 , 0.6 M formaldehyde and 8 mM Na 3 Au(SO3 ) 2 The Au plating solution was kept for about 120 minutes.
[0112] (6) Rinse with deionized water and N 2 After drying the substrate, silver paste was applied to the reference electrode to prepare for the subsequent preparation of the Ag / AgCl reference electrode.
[0113] (7) Before use, the prepared substrate was heated at 60°C for about 60 minutes.
[0114] After each of the above processes, rinse with deionized water and 2 dry
[0115] Immerse the Ag-coated electrode in 30 μL of 0.1 M FeCl 3 The Ag / AgCl reference electrode was prepared in the solution for 60 s.
[0116] The carbon-modified boron-doped diamond particles are connected to the Au on the substrate through conductive silver glue or metal welding, and epoxy resin is used as a conductive glue to be coated on the edge of the electrode for fixation.
[0117] The electrochemical potential window of the Au-modified boron-doped diamond microelectrode obtained in this example is as high as 3.3V; it has a good linear response in the concentration range of 0.1-150μM, and the detection sensitivity is as high as 243μA·μM-1·cm-2 when used for dopamine detection. The Ni-modified boron-doped diamond microelectrode obtained in this example is used for glucose detection: it has a good linear response in the concentration range of 0.05-20μM, and the detection sensitivity is as high as 410μA·μM-1·cm-2.
[0118] Comparative Example 1
[0119] (1) Diamond particles with an average particle size of 150 μm are cleaned.
[0120] (2) Immersing in a suspension containing nano-diamonds and ultrasonically vibrating for 30 minutes, cleaning and drying. The nano-diamonds are placed in the suspension containing nano-diamonds, and the mass fraction of the nano-diamonds is 0.01 wt%.
[0121] (3) Boron-doped diamond film was deposited by hot-filament CVD. The deposition process parameters were as follows: hot-filament distance 7 mm, growth temperature 800-900°C, hot-filament temperature 2200°C, deposition pressure 3 KPa, gas mass flow ratio of hydrogen:methane:borane = 98:2:0.3, growth pressure 2 KPa, and continuous growth for 6 h.
[0122] Figure 3This is a SEM image of diamond particles coated with polycrystalline B-doped diamond film. Due to the lack of continuous growth, some areas on the surface are not completely coated.
Claims
1. A method for preparing a carbon material / metal modified doped diamond particle integrated sensor, characterized in that: The steps include: Step 1 Preparation of doped diamond particles First, nano-diamond seed crystals are planted on the surface of carrier particles, and then the carrier particles planted with diamond seed crystals are subjected to chemical vapor deposition to grow doped diamond films, and a carbon material modification layer and / or a metal modification layer are arranged on the surface of the doped diamond film to obtain doped diamond particles; The process of chemical vapor deposition growth of doped diamond film is as follows: the mass flow ratio of the gas is hydrogen: methane: doping gas source = 98: 2: 0.3-0.6, the growth pressure is 2-5Kpa, the growth temperature is 800-850°C, the growth times are 2-6 times, after each growth, the carrier particles are taken out, the carrier particles are shaken, and then the growth is continued, the single growth time is 3-6h, and the doping gas source is selected from at least one of ammonia, phosphine, and borane; Step 2: Sensor assembly First, the substrate is exposed to UV light, and the electrode layout on the substrate surface is constructed through a mask. Then, Au nanoparticles are deposited on the substrate surface by chemical plating. Then, silver paste is applied to the substrate surface, and heat treatment is performed. Then, the substrate coated with silver paste is immersed in a solution containing chloride ions to form an Ag / AgCl reference electrode on the substrate surface. Finally, at least one doped diamond particle is fixed on the substrate and connected to the Au nanoparticle to obtain an integrated sensor. The integrated sensor comprises a working electrode, a counter electrode, a reference electrode, and a substrate. The working electrode is composed of at least one doped diamond particle. The doped diamond particle comprises a carrier particle, a coating layer, and a modification layer from the inside to the outside. The carrier particle is a boron-containing diamond particle. The coating layer is a doped diamond film. The doping element is selected from one or more of boron, nitrogen, and phosphorus. The modification layer is selected from at least one of carbon material modification and metal modification. The carrier particles are of a single crystal structure, and the doped diamond film is of a polycrystalline structure; The doping concentration in the doped diamond film is 10 21 cm -3 ~10 22 cm -3 ; When the working electrode is a single doped diamond particle, detection of a single active molecule is achieved; when the working electrode is a plurality of doped diamond particles with different modification layers, detection of multiple active molecules is achieved simultaneously.
2. The method for preparing a carbon material / metal-modified doped diamond particle integrated sensor according to claim 1, characterized in that: In step 1, the process of planting nano-diamond seed crystals on the surface of the carrier particles is as follows: immersing the carrier particles in a suspension containing nano-diamonds and ultrasonically vibrating for ≥30 minutes, and finally washing and drying. The mass fraction of nano-diamonds in the suspension containing nano-diamonds is 0.01-0.1wt%; In step 1, the chemical vapor deposition is hot wire chemical vapor deposition, and the temperature of the hot wire is 2500-2700°C.
3. The method for preparing a carbon material / metal-modified doped diamond particle integrated sensor according to claim 1, characterized in that: In step 1, the process of setting the carbon material modification layer is as follows: first, a metal nickel layer is deposited on the surface of the doped diamond film by magnetron sputtering; the thickness of the metal nickel layer is 2-22 nm; then, the doped diamond particles covered with the metal nickel layer are thermally catalyzed to grow carbon material on the surface of the doped diamond film to form a carbon material modification layer; the carbon material includes one or more of microcrystalline graphite, carbon nanotubes, carbon nanofibers, and graphene; The magnetron sputtering process is as follows: a nickel target with a purity of ≥99.99% is used, the distance between the substrate and the target is 10-12 cm, an argon atmosphere is used, the deposition pressure is 0.4-0.6 Pa, the sputtering power is 150 W, and the deposition time is 60 s; When the carbon material is selected from microcrystalline graphite, the thermal catalysis process is: introducing 97-100 sccm of hydrogen, the thermal catalysis temperature is 750-800°C, the thermal catalysis pressure is 9-11 kPa, the thermal catalysis time is 1-1.2 h, the heating rate is 18-22°C / min, and the cooling rate is 18-22°C / min; When the carbon material is selected from carbon nanotubes, the thermal catalysis process is: introducing 28.5 sccm of hydrogen, 1.5-2.0 sccm of methane, a thermal catalytic temperature of 750-800°C, a thermal catalytic gas pressure of 10 kPa, a thermal catalytic time of 35-40 min, a heating rate of 195-205°C / min, and a cooling rate of 195-205°C / min; When the carbon material is selected from carbon nanofibers, the thermal catalysis process is: introducing 28.5 sccm of hydrogen, 1.5-2.0 sccm of methane, a thermal catalytic temperature of 950-1000°C, a thermal catalytic gas pressure of 10 kPa, a thermal catalytic time of 30-40 min, a heating rate of 195-205°C / min, and a cooling rate of 195-205°C / min; When the carbon material is graphene, the thermal catalysis process is: introducing 98 sccm of hydrogen, the thermal catalysis temperature is 750-800°C, the thermal catalysis pressure is 10 kPa, the thermal catalysis time is 5 min, the heating rate is 195-205°C / min, and the cooling rate is 195-205°C / min.
4. The method for preparing a carbon material / metal-modified doped diamond particle integrated sensor according to claim 1, characterized in that: In step 1, the process of setting the metal modification layer is: depositing a metal layer on the surface of the doped diamond film by magnetron sputtering; the thickness of the metal layer is 2-22nm; the process of the magnetron sputtering is: the purity of the target material is ≥99.9%, the target material is selected from at least one of iron, copper, platinum, silver and gold, the distance between the substrate and the target material is 10-15 cm, an argon atmosphere is adopted, the deposition pressure is 0.6-2 Pa, the sputtering power is 150-300W, and the deposition time is 60-120 s; the doped diamond particles after sputtering are placed in a hot tube furnace for heat treatment, so that the metal layer is spheroidized into nanoparticle clusters with a grain size of 20-500nm, the gas pressure is maintained at 15-20kpa, the heat treatment temperature is 900°C, the heat treatment time is 4-5h, and the mass flow ratio of the atmosphere is H2:Ar=1.5-3.
5. The method for preparing a carbon material / metal-modified doped diamond particle integrated sensor according to claim 1, characterized in that: In step 2, the process of depositing Au nanoparticles on the surface of the substrate is as follows: the substrate with the electrode layout set is aminated in an amination solution containing 0.4 M ethylenediamine and 50 mM EDC for 180 min, and the substrate is first treated with 1 mM HAuCl4 solution for 80-200 min under dark conditions, and then the PET substrate is treated with 0.1 M NaBH4 solution for 5-50 min, and then the substrate is placed in a 0.5 M KSCN solution for ultrasonic treatment for 1 h, and then the substrate is placed in an Au plating solution containing 0.125 M Na2SO3, 0.6 M formaldehyde and 8 mM Na3Au(SO3)2 for 120 min, and the substrate is rinsed with deionized water and dried with N2; In step 2, the substrate coated with silver paste was immersed in 30 μL 0.1 M FeCl3 solution for 60 s to form a Ag / AgCl reference electrode on the substrate surface.
6. The method for preparing a carbon material / metal-modified doped diamond particle integrated sensor according to claim 1, characterized in that: The particle size of the carrier particles is 100nm-500μm, and the thickness of the doped diamond film is 5μm-20μm; The doping method of the doped diamond film includes one or more combinations of constant doping, multi-layer variable doping, and gradient doping.
7. The method for preparing a carbon material / metal-modified doped diamond particle integrated sensor according to claim 1, characterized in that: The doped diamond film is a doped diamond film with a porous structure, and the pore diameter of the pores in the doped diamond film is 10nm-200nm; The carbon material in the carbon material modification is selected from at least one of microcrystalline graphite, carbon nanotubes, carbon nanofibers, and graphene, and the metal in the metal modification is selected from at least one of iron, copper, platinum, silver, and gold. The reference electrode is Ag / AgCl, and the counter electrode is Au nanoparticles.
8. The method for preparing a carbon material / metal-modified doped diamond particle integrated sensor according to claim 1, characterized in that: The material of the substrate is selected from one of silicon and germanium semiconductors, polyimide, polydimethylsiloxane, and polyethylene terephthalate.
9. Application of a carbon material / metal-modified doped diamond particle integrated sensor prepared by the preparation method according to any one of claims 1 to 8, characterized in that: Carbon material / metal-modified doped diamond particles integrated sensor for electrochemical detection.
Citation Information
Patent Citations
Methods for integrating electrodes on diamond anvil cells
CN102288844A
Preparation method of boron-nitrogen co-doped nano-based oriented diamond film
CN103938182A
Single particle layer nano-diamond film and preparation method thereof
CN104762607A
Boron-doped single-particle-layer nano-diamond film and preparation method thereof
CN105316648A
Preparation method of electrochemical alanine biosensor based on boron-doped diamond microelectrode and application thereof
CN108362751A