Graphene-based nanosheet array composite supported palladium cluster catalyst and preparation method

By loading captopril-protected water-soluble ultrafine palladium nanoclusters on nanosheet array hybrid support, the problem of large particle size and uneven distribution of traditional Pd catalysts is solved, and efficient catalytic activity and environmentally friendly catalysts are achieved Preparation, suitable for catalytic reduction and degradation of aromatic nitro compounds and anionic azo dyes.

CN113786844BActive Publication Date: 2024-12-03BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111194114.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-13
Publication Date
2024-12-03
Estimated Expiration
2041-10-13

AI Technical Summary

Technical Problem

In the existing supported Pd catalysts, the Pd particle size is large and the distribution is uneven, and the active site is insufficient, resulting in low catalytic activity. The traditional impregnation method uses a large amount of organic solvents to cause environmental pollution problems.

Method used

Captopril-protected water-soluble ultrafine palladium nanoclusters (Pd-Capt) were prepared by simple chemical reduction method, and nanosheet array hybrid carrier M1M2-LDH/rGO was prepared by aqueous co-precipitation method, and electrostatic adsorption was adjusted using pH. The Pd-Capt nanocluster was loaded on a support and moderately calcined in a nitrogen atmosphere to obtain the supported Pd nanocluster catalyst x-PdNCs/M1M2(O)/rGO-T.

Benefits of technology

The high dispersion and uniform distribution of Pd nanoclusters were achieved, which significantly improved the catalytic activity, and showed excellent catalytic reduction and degradation performance for aromatic nitro compounds and anionic azo dyes, and the process was clean and green and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113786844B_ABST
    Figure CN113786844B_ABST
Patent Text Reader

Abstract

A graphene-based nanosheet array composite supported palladium cluster catalyst and a preparation method thereof belong to the technical field of supported palladium nanocluster catalysts. The expression is x-PdNCs / M1M2(O) / rGO-T, wherein x is the mass loading of Pd, which is 0.1-0.5wt%; M1M2(O) is a composite metal oxide obtained by topological transformation of layered double hydroxide; rGO is reduced graphene oxide; and T is the calcination temperature. The captopril-protected water-soluble palladium nanoclusters prepared by a simple chemical reduction method are loaded on a pre-prepared LDH / rGO hybrid by a pH-adjusted electrostatic adsorption method and subsequently calcined in a nitrogen atmosphere. In the obtained nanosheet array-type catalyst, ultrafine palladium nanoclusters (1.3-1.8nm) are highly dispersed at the edge of the oxide nanosheet. The advantage is that it has excellent catalytic reduction of nitro compounds and degradation of organic dyes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of supported palladium nanocluster catalysts, and in particular provides a graphene-based nanosheet array composite metal oxide supported ultrafine palladium nanocluster (PdNCs) catalyst and a preparation method thereof. Technical Background

[0002] Supported Pd catalysts are a typical type of heterogeneous catalysts, widely used in the fields of fine chemicals and environmental protection. The regulation of the size and dispersion of the active component Pd plays a vital role in the catalytic activity. The preparation of ultrafine and highly uniformly dispersed supported Pd catalysts is extremely beneficial to the improvement of their catalytic activity. However, the Pd particle size in the Pd-based catalyst prepared by the traditional impregnation method is relatively large (>2nm) and unevenly distributed. Therefore, a simple and green synthesis method is designed to directly anchor the prefabricated ultrafine Pd nanoclusters of uniform size on the carrier to obtain highly dispersed ultrafine Pd nanocluster catalysts.

[0003] Chen et al. (XHGao, W.Chen, Chem. Commun., 2017, 53, 9733-9736) used PdCl2 as palladium source, tetraoctylammonium bromide as phase transfer agent, 1-dodecanethiol as protective ligand and reducing agent, and synthesized oil-soluble atomic precision Pd6 (SC 12 H 25 ) 12 Clusters. The catalyst obtained by depositing it on activated carbon and calcining it in vacuum at 200°C showed excellent catalytic activity in the HER reaction. In another study, Chen et al. (ZH Zhuang, Q. Yang, W. Chen, ACS Sustainable Chem. Eng., 2019, 7, 2916-2923.) used Pd(acac)2 as a precursor, 1-dodecanethiol as a protective ligand and reducing agent, and oleylamine as a solvent to synthesize oil-soluble atomic precision Pd6(C 12 H 25 S) 11 Clusters. It was deposited on carbon black and moderately calcined to obtain a highly active Pd nanocluster catalyst with a Pd cluster size of <1 nm. The 0.2 mg catalyst can completely degrade 0.25 μmol 4-nitrophenol (4-NP) in just 0.5 minutes (100% conversion rate). Farrag et al. (Mostafa Farrag, Mrinmoy K. Das, Michael Moody, M. Samy El-Shall, Chem. Phys. Chem., 2021, 22, 312-322.) prepared a water-soluble Pd nanocluster catalyst using potassium hexachloropalladate as a palladium source, L-cysteine ​​as a protective ligand, and sodium borohydride as a reducing agent.n (L-Cys) m Nanoclusters. It is then loaded on metal oxides by an impregnation method to prepare a Pd nanocluster catalyst, in which the Pd size is about 2nm. The effect of ligands on catalytic activity was investigated in the CO oxidation reaction. However, most of the supported Pd nanocluster catalysts reported in the literature are prepared using oil-soluble nanoclusters as precursors, and the use of a large amount of organic solvents during the loading process will inevitably cause environmental pollution problems. Therefore, the preparation of clean, green, and environmentally friendly water-soluble Pd nanoclusters is crucial. At the same time, considering the dispersion and exposure of Pd active sites in supported Pd catalysts and metal-support interactions, the properties of the support may also greatly affect the catalytic reaction performance. Zhang et al. (LGDou, H.Zhang, J.Mater.Chem.A, 2016, 4, 18990-19002; ZJWei, YGLi, LGDou, M.Ahmad, H.Zhang, ACS Appl.Nano Mater.2019, 2, 2383-2396.) prepared nanosheet array hybrids Cu by aqueous coprecipitation. x Mg(Ni) 3-x Al-LDH / rGO (LDH: layered double hydroxide, rGO: reduced graphene oxide) exhibits excellent catalytic reduction performance for 4-NP. The high specific surface area and rich mesoporous structure of the LDH / rGO nanosheet arrays, as well as the controllable atomically dispersed metal cations in the LDH layer sheets, are very conducive to the anchoring of ultrafine Pd nanoclusters.

[0004] Therefore, the present invention intends to prepare water-soluble ultrafine palladium nanoclusters (Pd-Capt) protected by captopril (Capt) by a simple chemical reduction method, prepare a nanosheet array type hybrid carrier M1M2-LDH / rGO by an aqueous phase coprecipitation method, and then use a pH adjustment electrostatic adsorption method to immobilize the Pd-Capt nanoclusters on the M1M2-LDH / rGO hybrid carrier, and then moderately calcine in a nitrogen atmosphere to obtain a supported Pd nanocluster catalyst x-PdNCs / M1M2(O) / rGO-T. The catalytic reduction of 4-NP to p-aminophenol (4-AP) is used as a probe reaction to explore the catalytic activity of the obtained catalyst. So far, there has been no report on water-soluble captopril-protected Pd nanoclusters, and there has been no report on the synthesis of a multi-level structure carrier-supported water-soluble Pd nanocluster catalyst. Summary of the invention

[0005] The purpose of the present invention is to provide a graphene-based nanosheet array composite metal oxide supported captopril protected water-soluble ultrafine palladium nanocluster (PdNCs) catalyst and a preparation method thereof, which solves the problems of relatively large size, uneven distribution and less exposure of active sites of Pd nanoparticles prepared by traditional impregnation reduction method, thereby greatly improving the activity of supported ultrafine palladium nanocluster catalyst. In the catalyst, ultrafine PdNCs are highly dispersed at the edge of M1M2(O) composite oxide nanosheets. It exhibits excellent activity in the room temperature NaBH4 catalytic reduction of 4-NP reaction, and also exhibits excellent catalytic reduction and degradation performance for a variety of aromatic nitro compounds and anionic azo dyes. Among them, aromatic nitro compounds include o-nitrophenol, m-nitrophenol, 2,4-dinitrotoluene, 4-nitrobenzaldehyde and 4-nitroaniline; organic dyes include methyl orange, acid orange 7, rhodamine B, methylene blue, Congo red and acid black.

[0006] The catalyst of the present invention is obtained by loading Capt-protected water-soluble ultrafine Pd nanoclusters (Pd-Capt) (1.3±0.5nm) prepared by a simple chemical reduction method on a nanosheet array-type M1M2-LDH / rGO hybrid carrier by a pH-adjusted electrostatic adsorption method, and then moderately calcining in a nitrogen atmosphere. The catalyst is expressed as x-PdNCs / M1M2(O) / rGO-T, wherein x represents the mass loading of Pd, which is 0.1-0.5wt%; M1M2(O) represents a composite metal oxide obtained by topological transformation of a layered double hydroxide (LDH) precursor, and M1 is Ni 2+ 、Co 2+ and Mg 2+ Any one or two of the divalent metal cations, M2 is Al 3+ and Ce 3+ Any one or two of trivalent metal cations, and the molar ratio of M1 to M2 is 3:1; rGO is reduced graphene oxide; T is the calcination temperature, which is 250-320°C, and the calcination atmosphere is nitrogen; the obtained catalyst has a multi-level nanosheet array morphology, wherein the M1M2(O) nanosheets are 55-75nm in size and 8-12nm in thickness, and are vertically oriented and grown on both sides of the rGO sheets, and Pd NCs with a size of 1.3-1.8nm are highly dispersed at the edges of the M1M2(O) nanosheets.

[0007] The catalyst preparation of the present invention comprises the following steps:

[0008] (1) Preparation of water-soluble ultrafine palladium nanoclusters (Pd-Capt)

[0009] Captopril (Capt) protected water-soluble palladium nanoclusters (Pd-Capt) were prepared by a simple chemical reduction method. The specific preparation steps are as follows: 1g Na2PdCl4 was dissolved in 50mL methanol to 100mL to obtain a stock solution with a mass concentration of 10mg / mL. At 25±1℃, 5.88mL Na2PdCl4 stock solution was added to a 50mL single-necked flask, and then 4.12mL methanol was added to the flask to make it 10mL. After magnetic stirring at 1200 rpm for 3 minutes, 0.1269g of white crystals of tetraoctylammonium bromide were added under continuous stirring, and the solution immediately changed from brown-red to dark red. Stirring was continued for 20 minutes, and then 5mL of methanol solution containing 0.0435g of captopril was added, and the color immediately changed to light red. After continuous stirring for another 30 minutes, 5mL of ice-water solution containing 0.0759g of NaBH4 was added, and the solution immediately turned black. After 8 to 10 hours of reaction, the reaction mixture is centrifuged at a speed of 5000 rpm for 10 minutes to remove a small amount of insoluble Pd(II):Capt polymer, the supernatant is rotary evaporated at 30 to 50° C. for 15 to 25 minutes, 1 mL of methanol is added to the concentrated solution to dissolve the product adhering to the wall of the flask, and then 25 to 50 mL of anhydrous ethanol is added and allowed to stand overnight to obtain a cluster precipitate; the obtained precipitate is vacuum dried at 30 to 60° C. for 10 to 16 hours to obtain a crude product; then, the crude product is extracted and purified with 1 to 3 mL of methanol for 3 to 6 times to remove the substances insoluble in methanol, and then 25 to 50 mL of anhydrous ethanol is added to obtain a nanocluster precipitate, which is centrifuged and the obtained precipitate is vacuum dried at 30 to 60° C. for 10 to 16 hours to obtain a purified Pd nanocluster black powder, named Pd-Capt, which is dissolved in deionized water to prepare a 100 mL solution (0.1316 mg / mL).

[0010] (2) Preparation of nanosheet array-like M1M2-LDH / rGO hybrid carrier

[0011] The multi-level nanosheet array type M1M2-LDH / rGO hybrid carrier was prepared by aqueous coprecipitation method (LGDou, H.Zhang, J.Mater.Chem.A, 2016, 4, 18990-19002.). The specific steps are as follows: 7.7mL of 6.5mg / mL graphite oxide (GO) sol was dispersed in 100mL deionized water, and ultrasonicated for 15-20 minutes to obtain a peeled GO suspension. Then 25mg of citric acid was added and ultrasonicated for 5-10 minutes to obtain a citric acid-modified GO suspension. NaOH and Na2CO3 were dissolved in 100mL deionized water to prepare a mixed alkaline solution, in which OH - and CO3 2-The molar concentration ratio of M1 and M2 is 3.2. The nitrates of M1 and M2 are added to 100 mL of deionized water to prepare a mixed salt solution, where M1 is Ni 2+ 、Co 2+ and Mg 2+ Any one or two of the divalent metal cations, M2 is Al 3+ and Ce 3+ Any one or two of the trivalent metal cations, the total amount of M1 and M2 is 20mmol, the molar ratio of M1 to M2 is 3:1, and CO3 2- The molar concentration ratio of M2 to M2 is 2. The above mixed alkali solution is added dropwise to the citric acid-modified GO suspension under vigorous stirring until the pH is 10.0±0.1 and stabilized for 5 to 10 minutes to deprotonate the citric acid on the GO surface to form -COO - Anions. Then, a mixed salt and a mixed alkali solution are added dropwise at the same time, and the pH is maintained at 10.0±0.1. After the salt solution is added dropwise, the resulting reaction solution is crystallized in a water bath at 65-80°C for 4-6 hours. Finally, the mixture is centrifuged and washed with deionized water until the supernatant is neutral. The resulting precipitate is vacuum freeze-dried for 6 hours to obtain a multi-level structure nanosheet array type hybrid carrier M1M2-LDH / rGO.

[0012] (3) Preparation of nanosheet array-like supported palladium nanocluster catalyst x-PdNCs / M1M2(O) / rGO-T

[0013] The x-PdNCs / M1M2(O) / rGO-T catalyst was prepared by the pH-adjusted electrostatic adsorption method. The specific operation steps are as follows: 1.0 g of the M1M2-LDH / rGO carrier obtained in step (2) was added to 40 mL of deionized water, ultrasonicated for 2 to 5 minutes, and adjusted to pH = 6.5 to 9.5 with Na2CO3 under vigorous stirring at 1000 rpm at room temperature to obtain a carrier suspension. Then, the Pd-Capt nanocluster aqueous solution obtained in step (1) was added dropwise to the above carrier suspension, with a theoretical loading of 0.1 to 0.5 wt%, and stirring was continued for 40 minutes. The obtained mixed solution is then centrifuged, the precipitate is collected, and the precipitate is vacuum freeze-dried for 6 hours to obtain the catalyst precursor x-Pd-Capt / M1M2-LDH / rGO; the obtained precursor is placed in 50-200 mL / min flowing N2, maintained at 250-320°C for 2-4 hours at a heating rate of 1-5°C / min, and then naturally cooled to room temperature to obtain a nanosheet array-like supported palladium nanocluster catalyst x-PdNCs / M1M2(O) / rGO-T.

[0014] The advantages of the present invention are:

[0015] (1) Provided is a graphene-based nanosheet array composite metal oxide supported water-soluble ultrafine Pd nanocluster catalyst and a preparation method thereof. First, a clean, green, and environmentally friendly water-soluble captopril (Capt) protected ultrafine palladium nanoclusters (Pd-Capt) are prepared by a simple chemical reduction method, and then loaded on a nanosheet array-like M1M2-LDH / rGO hybrid carrier by a pH-adjusted electrostatic adsorption method to obtain a catalyst precursor x-Pd-Capt / M1M2-LDH / rGO, and then calcined in a nitrogen atmosphere to remove the protective Capt ligands on the surface of the nanocluster to obtain a highly dispersed ultrafine Pd nanocluster catalyst x-PdNCs / M1M2(O) / rGO-T, wherein Pd NCs (1.3-1.8nm) are highly dispersed at the edge of the M1M2(O) nanosheets.

[0016] (2) The multi-level nanosheet array hybrid carrier has a high specific surface area and rich mesoporous structure, which provides abundant anchoring sites for Pd NCs. The Pd NCs in the obtained catalyst are highly uniformly dispersed at the edge of the vertically staggered M1M2(O) nanosheets, which is conducive to the subsequent contact with the reaction substrate.

[0017] (3) The obtained catalyst not only exhibits excellent catalytic reduction activity for aromatic nitro compounds, but also exhibits excellent degradation ability for anionic azo dyes. The present invention not only provides a simple synthetic strategy for synthesizing clean, efficient and environmentally friendly supported metal nanocluster catalysts, but also provides a new idea for the efficient catalytic degradation of wastewater containing nitrophenol compounds and anionic azo dyes. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a high-resolution transmission electron microscopy image of the Pd-Capt nanoclusters dispersed in an alkaline buffer solution at pH = 8.0 ± 0.5 in Example 1.

[0019] Figure 2 This is the X-ray diffraction pattern of the Pd-Capt nanoclusters in Example 1.

[0020] Figure 3 This is a scanning electron microscope image of the catalyst 0.2-PdNCs / CoAl(O) / rGO-300 in Example 1.

[0021] Figure 4 This is a phase-corrected high-angle annular dark-field scanning transmission electron microscopy image of the catalyst 0.2-PdNCs / CoAl(O) / rGO-300 in Example 1.

[0022] Figure 5 This is the particle size distribution diagram of Pd nanoclusters of the catalyst 0.2-PdNCs / CoAl(O) / rGO-300 in Example 1.

[0023] Figure 6 This is the UV-visible spectrum of the catalyst 0.2-PdNCs / CoAl(O) / rGO-300 in Example 1 catalytic reduction of p-nitrophenol. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below in conjunction with specific embodiments, but the embodiments of the present invention are not limited thereto.

[0025] Example 1

[0026] (1) Preparation of water-soluble ultrafine palladium nanoclusters (Pd-Capt)

[0027] Sodium tetrachloropalladate (Na2PdCl4) was used as the initial raw material. 1g Na2PdCl4 was dissolved in 50mL methanol to a constant volume of 100mL to obtain a 10mg / mL stock solution. At 25±1°C, 5.88mL Na2PdCl4 stock solution was added to a 50mL single-necked flask, and then 4.12mL methanol was added. After magnetic stirring for 3 minutes (1200 rpm), 0.1269g tetraoctylammonium bromide white crystals were added under continuous stirring, and the solution immediately changed from brown-red to dark red; continued stirring for 20 minutes, and then 5mL of methanol solution containing 0.0435g Capt was added, and the color immediately changed to light red; after continuous stirring for 30 minutes, 5mL of ice-water solution containing 0.0759g NaBH4 was added, and the solution immediately turned black; after 9 hours of reaction, the reaction mixture was centrifuged (5000 rpm, 10 minutes) to remove the remaining The insoluble Pd(II):Capt polymer was removed by rotary evaporation at 40°C for 20 minutes, and 1 mL of methanol was added to the concentrated solution to dissolve the product adhering to the wall of the flask, and then 30 mL of anhydrous ethanol was added and allowed to stand overnight to obtain a cluster precipitate; the obtained precipitate was vacuum dried at 40°C for 12 hours to obtain a crude product; then, the crude product was extracted and purified with 2 mL of methanol for 4 times to remove the substances insoluble in methanol, and 30 mL of anhydrous ethanol was added to obtain a nanocluster precipitate, which was centrifuged and vacuum dried at 40°C for 12 hours to obtain a purified Pd nanocluster black powder, named Pd-Capt, which was dissolved in deionized water to prepare a 100 mL solution;

[0028] High-resolution transmission electron microscopy images of Pd-Capt nanoclusters dispersed in an alkaline buffer solution at pH = 8.0 ± 0.5 are shown in Figure 2. Figure 1 The particle size distribution is 1.3±0.5nm. The X-ray diffraction pattern of Pd-Capt nanoclusters is shown in Figure 2 As shown, there is a significant diffraction peak at about 40.10° 2θ, which is attributed to the Pd (111) crystal plane (standard card number 46-1043).

[0029] (2) Preparation of nanosheet array-like Co3Al-LDH / rGO hybrid carrier

[0030] 7.7 mL of GO sol (6.5 mg / mL) was dispersed in 100 mL of deionized water and ultrasonicated for 15 minutes to obtain a stripped GO suspension; then 25 mg of citric acid was added and ultrasonicated for 5 minutes to obtain a citric acid-modified GO suspension. 32 mmol NaOH (1.28 g) and 10 mmol Na2CO3 (1.06 g) were weighed and added to 100 mL of deionized water to prepare a mixed alkali solution; 15 mmol Co(NO3)2·6H2O (4.365 g) and 5 mmol Al(NO3)3·9H2O (1.875 g) were weighed and added to 100 mL of deionized water to prepare a mixed salt solution. The above mixed alkali solution was added dropwise to the citric acid-modified GO suspension under vigorous stirring until pH = 10.0 ± 0.1 and stabilized for 5 minutes. Then the mixed salt and mixed alkali solutions were added dropwise at the same time, and the pH was maintained at 10.0 ± 0.1. After the salt solution was added, the resulting reaction solution was crystallized in a water bath at 65°C for 4 hours. Finally, the reaction solution was separated by centrifugation and washed with deionized water until the supernatant was neutral. The resulting precipitate was vacuum freeze-dried for 6 hours to obtain a multi-level structure nanosheet array type hybrid carrier Co3Al-LDH / rGO.

[0031] (3) Preparation of 0.2-PdNCs / CoAl(O) / rGO-300 catalyst

[0032] 1.0 g of the Co3Al-LDH / rGO hybrid carrier obtained in step (2) was added to 40 mL of deionized water, ultrasonicated for 2 minutes, and adjusted to pH = 8 ± 0.1 with Na2CO3 under vigorous stirring at room temperature (1000 rpm) to obtain a carrier suspension. Then 12.2 mL of Pd-Capt nanocluster aqueous solution (0.1316 mg / mL, pH = 6.65) was measured and added dropwise to the above carrier suspension, and stirring was continued for 40 minutes. The resulting mixed solution was then centrifuged and the precipitate was vacuum freeze-dried for 6 hours to obtain the catalyst precursor 0.2-Pd-Capt / Co3Al-LDH / rGO. The resulting precursor was placed in 50 mL / min of flowing N2, kept at 300°C for 2 hours at a heating rate of 5°C / min, and then naturally cooled to room temperature to obtain a nanosheet array catalyst 0.2-PdNCs / CoAl(O) / rGO-300.

[0033] The scanning electron microscopy images and phase-corrected high-angle annular dark-field scanning transmission electron microscopy images of the catalyst 0.2-PdNCs / CoAl(O) / rGO-300 are shown in Figure 3 and 4The catalyst presents a nanosheet array morphology. CoAl(O) nanosheets with a size of ~65nm and a thickness of ~8nm grow vertically on both sides of the rGO matrix. Ultrafine PdNCs with a size of ~1.5nm are highly dispersed on the edge of the CoAl(O) nanosheets. The particle size distribution is shown in Figure 5 shown.

[0034] The catalytic reduction performance of the 0.2-PdNCs / CoAl(O) / rGO-300 catalyst obtained above was tested:

[0035] The catalytic hydrogenation of 4-NP was used as a model reaction to evaluate the catalytic activity of 0.2-PdNCs / CoAl(O) / rGO-300. The specific operation was as follows: 200 μL of 1 mM 4-NP aqueous solution and 2.5 mL of 10 mM freshly prepared NaBH4 solution were added to a standard quartz cuvette in sequence. After thorough mixing, 20 μL of 2.5 mg / mL 0.2-PdNCs / CoAl(O) / rGO-300 catalyst was added to the mixture. The absorbance change of 4-nitrophenol anion in the mixed solution was detected by UV spectrophotometer in the scanning range of 250-500 nm. The results are shown in Figure 2. Figure 6 As shown, 0.2-PdNCs / CoAl(O) / rGO-300 can rapidly catalyze the reduction of 4-NP within 30 seconds, indicating that 0.2-PdNCs / CoAl(O) / rGO-300 prepared in Example 1 has excellent catalytic reduction activity for 4-NP. The same test steps were used to evaluate the activity of the catalyst in catalytic reduction of other aromatic nitro compounds and degradation of organic dyes. Among them, other aromatic nitro compounds include o-nitrophenol, m-nitrophenol, 2,4-dinitrotoluene, 4-nitrobenzaldehyde and 4-nitroaniline; organic dyes include methyl orange, acid orange 7, rhodamine B, methylene blue, Congo red and acid black. All the above experimental operations were carried out at room temperature 25°C.

[0036] Example 2

[0037] (1) Preparation of water-soluble ultrafine palladium nanoclusters (Pd-Capt)

[0038] Sodium tetrachloropalladate (Na2PdCl4) was used as the initial raw material. 1g Na2PdCl4 was dissolved in 50mL methanol to a volume of 100mL to prepare a 10mg / mL stock solution. At 25±1℃, 5.88mL Na2PdCl4 stock solution was added to a 50mL single-necked flask, and then 4.12mL methanol was added. After magnetic stirring for 3 minutes (1200 rpm), 0.1269g white crystals of tetraoctylammonium bromide were added under continuous stirring, and the solution immediately changed from brown-red to dark red; continued stirring for 20 minutes, and then 5mL of methanol solution containing 0.0435g Capt was added, and the color immediately changed to light red; after continuous stirring for 30 minutes, 5mL of ice-water solution containing 0.0759g NaBH4 was added, and the solution immediately turned black; after 8 hours of reaction, the reaction mixture was centrifuged (5000 rpm, 10 minutes) to remove a small amount of insoluble Pd ( II): Capt polymer, the supernatant was rotary evaporated at 30°C for 25 minutes, and 1 mL of methanol was added to the obtained concentrated solution to dissolve the product adhering to the wall of the flask, and then 25 mL of anhydrous ethanol was added and allowed to stand overnight to obtain a cluster precipitate; the obtained precipitate was vacuum dried at 30°C for 16 hours to obtain a crude product; then, the crude product was extracted and purified with 1 mL of methanol for 3 times to remove the substances insoluble in methanol, and 25 mL of anhydrous ethanol was added to obtain a nanocluster precipitate, which was centrifuged and vacuum dried at 60°C for 10 hours to obtain a purified Pd nanocluster black powder, named Pd-Capt, which was dissolved in deionized water to prepare a 100 mL solution;

[0039] (2) Preparation of nanosheet array-like Ni3Al-LDH / rGO hybrid carrier

[0040] 7.7 mL of GO sol (6.5 mg / mL) was dispersed in 100 mL of deionized water and ultrasonicated for 20 minutes to obtain a stripped GO suspension; then 25 mg of citric acid was added and ultrasonicated for 10 minutes to obtain a citric acid-modified GO suspension. 32 mmol NaOH (1.28 g) and 10 mmol Na2CO3 (1.06 g) were weighed and added to 100 mL of deionized water to prepare a mixed alkali solution; 15 mmol Ni(NO3)2·6H2O (4.365 g) and 5 mmol Al(NO3)3·9H2O (1.875 g) were weighed and added to 100 mL of deionized water to prepare a mixed salt solution. The above mixed alkali solution was added dropwise under vigorous stirring until pH = 10.0 ± 0.1 and stabilized for 10 minutes. Then the mixed salt and mixed alkali solution were added dropwise at the same time, and the pH was maintained at 10.0 ± 0.1; after the salt solution was added dropwise, the resulting reaction solution was crystallized in a 65°C water bath for 4 hours. Finally, the mixture was separated by centrifugation and washed with deionized water until the supernatant was neutral. The obtained precipitate was freeze-dried in vacuum for 6 hours to obtain a multi-level structured nanosheet array type hybrid carrier Ni3Al-LDH / rGO.

[0041] (3) Preparation of 0.1-PdNCs / NiAl(O) / rGO-280 catalyst

[0042] 1.0 g of the Ni3Al-LDH / rGO hybrid carrier obtained in step (2) was added to 40 mL of deionized water, and after ultrasonic treatment for 2 minutes, the pH was adjusted to 6.5±0.1 with Na2CO3 under vigorous stirring (1000 rpm) at room temperature to obtain a carrier suspension. 6.1 mL of Pd-Capt nanocluster aqueous solution (0.1316 mg / mL, pH=6.65) was then added dropwise to the above carrier suspension and stirred for 40 minutes. The resulting mixed solution was then centrifuged and the precipitate was vacuum freeze-dried for 6 hours to obtain a catalyst precursor 0.1-Pd-Capt / Ni3Al-LDH / rGO. The resulting precursor was placed in 80 mL / min of flowing N2, kept at 280°C for 3 hours at a heating rate of 2°C / min, and then naturally cooled to room temperature to obtain a nanosheet array catalyst 0.1-PdNCs / NiAl(O) / rGO-280.

[0043] Example 3

[0044] (1) Preparation of water-soluble ultrafine palladium nanoclusters (Pd-Capt)

[0045] Sodium tetrachloropalladate (Na2PdCl4) was used as the initial raw material. 1g Na2PdCl4 was dissolved in 50mL methanol to a volume of 100mL to prepare a 10mg / mL stock solution. At 25±1℃, 5.88mL Na2PdCl4 stock solution was added to a 50mL single-necked flask, and then 4.12mL methanol was added. After magnetic stirring for 3 minutes (1200 rpm), 0.1269g white crystals of tetraoctylammonium bromide were added under continuous stirring, and the solution immediately changed from brown-red to dark red; continued stirring for 20 minutes, and then 5mL of methanol solution containing 0.0435g Capt was added, and the color immediately changed to light red; after continuous stirring for 30 minutes, 5mL of ice-water solution containing 0.0759g NaBH4 was added, and the solution immediately turned black; after 10 hours of reaction, the reaction mixture was centrifuged (5000 rpm, 10 minutes) to remove a small amount of insoluble Pd ( II): Capt polymer, the supernatant was rotary evaporated at 50°C for 15 minutes, and 1 mL of methanol was added to the obtained concentrated solution to dissolve the product adhering to the wall of the flask, and then 50 mL of anhydrous ethanol was added and allowed to stand overnight to obtain a cluster precipitate; the obtained precipitate was vacuum dried at 60°C for 10 hours to obtain a crude product; then, the crude product was extracted and purified with 3 mL of methanol for 6 times to remove the substances insoluble in methanol, and 50 mL of anhydrous ethanol was added to obtain a nanocluster precipitate, which was centrifuged and vacuum dried at 30°C for 16 hours to obtain a purified Pd nanocluster black powder, named Pd-Capt, which was dissolved in deionized water to prepare a 100 mL solution;

[0046] (2) Preparation of nanosheet array-like Mg3Al-LDH / rGO hybrid carrier

[0047] 7.7 mL of GO sol (6.5 mg / mL) was dispersed in 100 mL of deionized water and ultrasonicated for 18 minutes to obtain a stripped GO suspension; then 25 mg of citric acid was added and ultrasonicated for 8 minutes to obtain a citric acid-modified GO suspension. 32 mmol NaOH (1.28 g) and 10 mmol Na2CO3 (1.06 g) were weighed and added to 100 mL of deionized water to prepare a mixed alkali solution; 15 mmol Mg(NO3)2·6H2O (3.846 g) and 5 mmol Al(NO3)3·9H2O (1.875 g) were weighed and added to 100 mL of deionized water to prepare a mixed salt solution. The above mixed alkali solution was added dropwise under vigorous stirring until pH = 10.0 ± 0.1 and stabilized for 8 minutes. Then the mixed salt and mixed alkali solution were added dropwise at the same time, and the pH was maintained at 10.0 ± 0.1; after the salt solution was added dropwise, the resulting reaction solution was crystallized in a 65°C water bath for 4 hours. Finally, the mixture was separated by centrifugation and washed with deionized water until the supernatant was neutral. The obtained precipitate was freeze-dried in vacuum for 6 hours to obtain a multi-level structure nanosheet array type hybrid carrier Mg3Al-LDH / rGO.

[0048] (3) Preparation of 0.5-PdNCs / MgAl(O) / rGO-320 catalyst

[0049] 1.0 g of the Mg3Al-LDH / rGO hybrid carrier obtained in step (2) was added to 40 mL of deionized water, and after ultrasonication for 5 minutes, the pH was adjusted to 9.5±0.1 with Na2CO3 under vigorous stirring at room temperature (1000 rpm) to obtain a carrier suspension. 30.4 mL of Pd-Capt nanocluster aqueous solution (0.1316 mg / mL, pH=6.65) was then measured and added dropwise to the above carrier suspension, and stirring was continued for 40 minutes. The resulting mixed solution was then centrifuged and the precipitate was vacuum freeze-dried for 6 hours to obtain the catalyst precursor 0.5-Pd-Capt / Mg3Al-LDH / rGO. The resulting precursor was placed in 100 mL / min of flowing N2, kept at 320°C for 2 hours at a heating rate of 1°C / min, and then naturally cooled to room temperature to obtain a nanosheet array catalyst 0.5-PdNCs / MgAl(O) / rGO-320.

[0050] Example 4

[0051] (1) Preparation of water-soluble ultrafine palladium nanoclusters (Pd-Capt)

[0052] Referring to Example 1;

[0053] (2) Preparation of nanosheet array-like Co3Al-LDH / rGO hybrid carrier

[0054] Referring to Example 1;

[0055] (3) Preparation of 0.2-PdNCs / CoAl(O) / rGO-250 catalyst

[0056] The catalyst precursor 0.2-Pd-Capt / Co3Al-LDH / rGO refers to Example 1. The obtained precursor was placed in 200 mL / min of flowing N2, kept at 250°C for 2 hours at a heating rate of 5°C / min, and then naturally cooled to room temperature to obtain a nanosheet array-type catalyst 0.2-PdNCs / CoAl(O) / rGO-250.

[0057] Example 5

[0058] (1) Preparation of water-soluble ultrafine palladium nanoclusters (Pd-Capt)

[0059] Referring to Example 1;

[0060] (2) Preparation of nanosheet array-like Co2NiAl-LDH / rGO hybrid carrier

[0061] 7.7 mL of GO sol (6.5 mg / mL) was dispersed in 100 mL of deionized water and ultrasonicated for 20 minutes to obtain a stripped GO suspension; then 25 mg of citric acid was added and ultrasonicated for 5 minutes to obtain a citric acid-modified GO suspension. 32 mmol NaOH (1.28 g) and 10 mmol Na2CO3 (1.06 g) were weighed and added to 100 mL of deionized water to prepare a mixed alkali solution; 10 mmol Co(NO3)2·6H2O (2.910 g), 5 mmol Ni(NO3)2·6H2O (1.454 g) and 5 mmol Al(NO3)3·9H2O (1.875 g) were weighed and added to 100 mL of deionized water to prepare a mixed salt solution. The above mixed alkali solution was added dropwise under vigorous stirring until pH = 10.0 ± 0.1 and stabilized for 10 minutes. Then, a mixed salt solution and a mixed alkali solution were added dropwise at the same time, and the pH was maintained at 10.0±0.1; after the salt solution was added dropwise, the resulting reaction solution was crystallized in a water bath at 65°C for 4 hours. Finally, the mixture was centrifuged and washed with deionized water until the supernatant was neutral, and the resulting precipitate was vacuum freeze-dried for 6 hours to obtain a multi-level structure nanosheet array type hybrid carrier Co2NiAl-LDH / rGO.

[0062] (3) Preparation of 0.2-PdNCs / CoNiAl(O) / rGO-300 catalyst

[0063] 1.0 g of the Co2NiAl-LDH / rGO hybrid carrier obtained in step (2) was added to 40 mL of deionized water, and after ultrasonication for 3 minutes, the pH was adjusted to 8±0.1 with Na2CO3 under vigorous stirring at room temperature (1000 rpm) to obtain a carrier suspension. Then 12.2 mL of Pd-Capt nanocluster aqueous solution (0.1316 mg / mL, pH=6.65) was measured and added dropwise to the above carrier suspension, and stirring was continued for 40 minutes. The resulting mixed solution was then centrifuged and the precipitate was vacuum freeze-dried for 6 hours to obtain the catalyst precursor 0.2-Pd-Capt / Co2NiAl-LDH / rGO. The resulting precursor was placed in 50 mL / min of flowing N2, kept at 300°C for 4 hours at a heating rate of 5°C / min, and then naturally cooled to room temperature to obtain a nanosheet array catalyst 0.2-PdNCs / CoNiAl(O) / rGO-300.

[0064] Example 6

[0065] (1) Preparation of water-soluble ultrafine palladium nanoclusters (Pd-Capt)

[0066] Referring to Example 1;

[0067] (2) Preparation of nanosheet array-like Co2MgAl-LDH / rGO hybrid carrier

[0068] 7.7 mL of GO sol (6.5 mg / mL) was dispersed in 100 mL of deionized water and ultrasonicated for 20 minutes to obtain a stripped GO suspension; then 25 mg of citric acid was added and ultrasonicated for 5 minutes to obtain a citric acid-modified GO suspension. 32 mmol NaOH (1.28 g) and 10 mmol Na2CO3 (1.06 g) were weighed and added to 100 mL of deionized water to prepare a mixed alkali solution; 10 mmol Co(NO3)2·6H2O (2.910 g), 5 mmol Mg(NO3)2·6H2O (1.282 g) and 5 mmol Al(NO3)3·9H2O (1.875 g) were weighed and added to 100 mL of deionized water to prepare a mixed salt solution. The above mixed alkali solution was added dropwise under vigorous stirring until pH = 10.0 ± 0.1 and stabilized for 10 minutes. Then, a mixed salt solution and a mixed alkali solution were added dropwise at the same time, and the pH was maintained at 10.0±0.1; after the salt solution was added dropwise, the resulting reaction solution was crystallized in a water bath at 65°C for 4 hours. Finally, the mixture was centrifuged and washed with deionized water until the supernatant was neutral, and the resulting precipitate was vacuum freeze-dried for 6 hours to obtain a multi-level structure nanosheet array type hybrid carrier Co2MgAl-LDH / rGO.

[0069] (3) Preparation of 0.2-PdNCs / CoMgAl(O) / rGO-300 catalyst

[0070] 1.0 g of the Co2MgAl-LDH / rGO hybrid carrier obtained in step (2) was added to 40 mL of deionized water, and after ultrasonication for 2 minutes, the pH was adjusted to 8±0.1 with Na2CO3 under vigorous stirring at room temperature (1000 rpm) to obtain a carrier suspension. Then 12.2 mL of Pd-Capt nanocluster aqueous solution (0.1316 mg / mL, pH=6.65) was measured and added dropwise to the above carrier suspension, and stirring was continued for 40 minutes. The resulting mixed solution was then centrifuged and the precipitate was vacuum freeze-dried for 6 hours to obtain the catalyst precursor 0.2-Pd-Capt / Co2MgAl-LDH / rGO. The resulting precursor was placed in 50 mL / min of flowing N2, kept at 300°C for 2 hours at a heating rate of 5°C / min, and then naturally cooled to room temperature to obtain a nanosheet array catalyst 0.2-PdNCs / CoMgAl(O) / rGO-300.

[0071] Example 7

[0072] (1) Preparation of water-soluble ultrafine palladium nanoclusters (Pd-Capt)

[0073] Referring to Example 1;

[0074] (2) Preparation of nanosheet array-like Ni2MgAl-LDH / rGO hybrid carrier

[0075] 7.7 mL of GO sol (6.5 mg / mL) was dispersed in 100 mL of deionized water and ultrasonicated for 20 minutes to obtain a stripped GO suspension; then 25 mg of citric acid was added and ultrasonicated for 5 minutes to obtain a citric acid-modified GO suspension. 32 mmol NaOH (1.28 g) and 10 mmol Na2CO3 (1.06 g) were weighed and added to 100 mL of deionized water to prepare a mixed alkaline solution; 10 mmol Ni(NO3)2·6H2O (2.908 g), 5 mmol Mg(NO3)2·6H2O (1.282 g) and 5 mmol Al(NO3)3·9H2O (1.875 g) were weighed and added to 100 mL of deionized water to prepare a mixed salt solution. The above mixed alkaline solution was added dropwise under vigorous stirring until pH = 10.0 ± 0.1 and stabilized for 10 minutes. Then, a mixed salt solution and a mixed alkali solution were added dropwise at the same time, and the pH was maintained at 10.0±0.1; after the salt solution was added dropwise, the resulting reaction solution was crystallized in a water bath at 65°C for 4 hours. Finally, the mixture was centrifuged and washed with deionized water until the supernatant was neutral, and the resulting precipitate was vacuum freeze-dried for 6 hours to obtain a multi-level structure nanosheet array type hybrid carrier Ni2MgAl-LDH / rGO.

[0076] (3) Preparation of 0.2-PdNCs / NiMgAl(O) / rGO-300 catalyst

[0077] 1.0 g of the Ni2MgAl-LDH / rGO hybrid carrier obtained in step (2) was added to 40 mL of deionized water, and after ultrasonication for 2 minutes, the pH was adjusted to 8±0.1 with Na2CO3 under vigorous stirring at room temperature (1000 rpm) to obtain a carrier suspension. Then 12.2 mL of Pd-Capt nanocluster aqueous solution (0.1316 mg / mL, pH=6.65) was measured and added dropwise to the above carrier suspension, and stirring was continued for 40 minutes. The resulting mixed solution was then centrifuged and the precipitate was vacuum freeze-dried for 6 hours to obtain the catalyst precursor 0.2-Pd-Capt / Ni2MgAl-LDH / rGO. The resulting precursor was placed in 50 mL / min of flowing N2, kept at 300°C for 2 hours at a heating rate of 5°C / min, and then naturally cooled to room temperature to obtain a nanosheet array catalyst 0.2-PdNCs / NiMgAl(O) / rGO-300.

[0078] Example 8

[0079] (1) Preparation of water-soluble ultrafine palladium nanoclusters (Pd-Capt)

[0080] Referring to Example 1;

[0081] (2) Nanosheet array-like Co3Ce 0.1Al 0.9 Preparation of -LDH / rGO hybrid carrier

[0082] 7.7 mL of GO sol (6.5 mg / mL) was dispersed in 100 mL of deionized water and ultrasonicated for 20 minutes to obtain a stripped GO suspension; then 25 mg of citric acid was added and ultrasonicated for 5 minutes to obtain a citric acid-modified GO suspension. 32 mmol NaOH (1.28 g) and 10 mmol Na2CO3 (1.06 g) were weighed and added to 100 mL of deionized water to prepare a mixed alkali solution; 15 mmol Co(NO3)2·6H2O (4.369 g) and 0.5 mmol Ce(NO3)3·6H2O (0.217 g) and 4.5 mmol Al(NO3)3·9H2O (1.688 g) were weighed and added to 100 mL of deionized water to prepare a mixed salt solution. The above mixed alkali solution was added dropwise under vigorous stirring until pH = 10.0 ± 0.1 and stabilized for 10 minutes. Then, the mixed salt and mixed alkali solution were added dropwise at the same time, and the pH was maintained at 10.0±0.1; after the salt solution was added dropwise, the resulting reaction solution was crystallized in a 65°C water bath for 5 hours. Finally, the mixture was centrifuged and washed with deionized water until the supernatant was neutral, and the resulting precipitate was vacuum freeze-dried for 6 hours to obtain a multi-level structure nanosheet array type hybrid carrier Co3Ce 0.1 Al 0.9 -LDH / rGO.

[0083] (3) Preparation of 0.2-PdNCs / CoCeAl(O) / rGO-300 catalyst

[0084] 1.0 g of Co3Ce obtained in step (2) 0.1 Al 0.9 -LDH / rGO hybrid carrier was added to 40mL deionized water, and after ultrasonic treatment for 2 minutes, the pH was adjusted to 8±0.1 with Na2CO3 under vigorous stirring (1000 rpm) at room temperature to obtain a carrier suspension. Then 12.2mL Pd-Capt nanocluster aqueous solution (0.1316mg / mL, pH=6.65) was measured and added dropwise to the above carrier suspension, and stirring was continued for 40 minutes. The resulting mixed solution was then centrifuged and the precipitate was vacuum freeze-dried for 6 hours to obtain the catalyst precursor 0.2-Pd-Capt / Co3Ce 0.1 Al 0.9 The obtained precursor was placed in a flowing N2 of 50 mL / min, kept at 300°C for 2 hours at a heating rate of 5°C / min, and then naturally cooled to room temperature to obtain a nanosheet array-type catalyst 0.2-PdNCs / CoCeAl(O) / rGO-300.

[0085] Example 9

[0086] (1) Preparation of water-soluble ultrafine palladium nanoclusters (Pd-Capt)

[0087] Referring to Example 1;

[0088] (2) Nanosheet array-type Ni3Ce 0.1 Al 0.9 Preparation of -LDH / rGO hybrid carrier

[0089] 7.7 mL of GO sol (6.5 mg / mL) was dispersed in 100 mL of deionized water and ultrasonicated for 20 minutes to obtain a stripped GO suspension; then 25 mg of citric acid was added and ultrasonicated for 5 minutes to obtain a citric acid-modified GO suspension. 32 mmol NaOH (1.28 g) and 10 mmol Na2CO3 (1.06 g) were weighed and added to 100 mL of deionized water to prepare a mixed alkali solution; 15 mmol Ni(NO3)2·6H2O (4.362 g) and 0.5 mmol Ce(NO3)3·6H2O (0.217 g) and 4.5 mmol Al(NO3)3·9H2O (1.688 g) were weighed and added to 100 mL of deionized water to prepare a mixed salt solution. The above mixed alkali solution was added dropwise under vigorous stirring until pH = 10.0 ± 0.1 and stabilized for 10 minutes. Then, the mixed salt and mixed alkali solution were added dropwise at the same time and the pH was maintained at 10.0±0.1. After the salt solution was added dropwise, the obtained reaction solution was crystallized in a 70°C water bath for 6 hours. Finally, the mixture was centrifuged and washed with deionized water until the supernatant was neutral. The obtained precipitate was vacuum freeze-dried for 6 hours to obtain a multi-level structure nanosheet array type hybrid carrier Ni3Ce 0.1 Al 0.9 -LDH / rGO.

[0090] (3) Preparation of 0.2-PdNCs / NiCeAl(O) / rGO-300 catalyst

[0091] 1.0 g of Ni3Ce obtained in step (2) 0.1 Al 0.9 -LDH / rGO hybrid carrier was added to 40mL deionized water, and after ultrasonic treatment for 2 minutes, the pH was adjusted to 6.5±0.1 with Na2CO3 under vigorous stirring at room temperature (1000 rpm) to obtain a carrier suspension. Then 12.2mL Pd-Capt nanocluster aqueous solution (0.1316mg / mL, pH=6.65) was measured and added dropwise to the above carrier suspension, and stirring was continued for 40 minutes. The resulting mixed solution was then centrifuged and the precipitate was vacuum freeze-dried for 6 hours to obtain the catalyst precursor 0.2-Pd-Capt / Ni3Ce 0.1 Al0.9 The obtained precursor was placed in a flowing N2 of 50 mL / min, kept at 300°C for 2 hours at a heating rate of 5°C / min, and then naturally cooled to room temperature to obtain a nanosheet array-type catalyst 0.2-PdNCs / NiCeAl(O) / rGO-300.

[0092] Example 10

[0093] (1) Preparation of water-soluble ultrafine palladium nanoclusters (Pd-Capt)

[0094] Referring to Example 1;

[0095] (2) Nanosheet array-type Mg3Ce 0.1 Al 0.9 Preparation of -LDH / rGO hybrid carrier

[0096] 7.7 mL of GO sol (6.5 mg / mL) was dispersed in 100 mL of deionized water and ultrasonicated for 20 minutes to obtain a stripped GO suspension; then 25 mg of citric acid was added and ultrasonicated for 5 minutes to obtain a citric acid-modified GO suspension. 32 mmol NaOH (1.28 g) and 10 mmol Na2CO3 (1.06 g) were weighed and added to 100 mL of deionized water to prepare a mixed alkali solution; 15 mmol Mg(NO3)2·6H2O (3.846 g) and 0.5 mmol Ce(NO3)3·6H2O (0.217 g) and 4.5 mmol Al(NO3)3·9H2O (1.688 g) were weighed and added to 100 mL of deionized water to prepare a mixed salt solution. The above mixed alkali solution was added dropwise under vigorous stirring until pH = 10.0 ± 0.1 and stabilized for 10 minutes. Then, the mixed salt and mixed alkali solution were added dropwise at the same time, and the pH was maintained at 10.0±0.1; after the salt solution was added dropwise, the resulting reaction solution was crystallized in a water bath at 80°C for 5 hours. Finally, the mixture was centrifuged and washed with deionized water until the supernatant was neutral, and the resulting precipitate was vacuum freeze-dried for 6 hours to obtain a multi-level structure nanosheet array type hybrid carrier Mg3Ce 0.1 Al 0.9 -LDH / rGO.

[0097] (3) Preparation of 0.2-PdNCs / MgCeAl(O) / rGO-300 catalyst

[0098] 1.0 g of Mg3Ce obtained in step (2) 0.1 Al 0.9-LDH / rGO hybrid carrier was added to 40mL deionized water, and after ultrasonic treatment for 2 minutes, the pH was adjusted to 9.5±0.1 with Na2CO3 under vigorous stirring at room temperature (1000 rpm) to obtain a carrier suspension. Then 12.2mL Pd-Capt nanocluster aqueous solution (0.1316mg / mL, pH=6.65) was measured and added dropwise to the above carrier suspension, and stirring was continued for 40 minutes. The resulting mixed solution was then centrifuged and the precipitate was vacuum freeze-dried for 6 hours to obtain the catalyst precursor 0.2-Pd-Capt / Mg3Ce 0.1 Al 0.9 The obtained precursor was placed in a flowing N2 of 50 mL / min, kept at 300°C for 2 hours at a heating rate of 5°C / min, and then naturally cooled to room temperature to obtain a nanosheet array-type catalyst 0.2-PdNCs / MgCeAl(O) / rGO-300.

[0099] Embodiment 11

[0100] (1) Preparation of water-soluble ultrafine palladium nanoclusters (Pd-Capt)

[0101] Referring to Example 1;

[0102] (2) Nanosheet array-type Ni 1.5 Mg 1.5 Al 0.9 Ce 0.1 Preparation of -LDH / rGO hybrid carrier

[0103] 7.7 mL of GO sol (6.5 mg / mL) was dispersed in 100 mL of deionized water and ultrasonicated for 20 minutes to obtain a stripped GO suspension; then 25 mg of citric acid was added and ultrasonicated for 10 minutes to obtain a citric acid-modified GO suspension. 32 mmol NaOH (1.28 g) and 10 mmol Na2CO3 (1.06 g) were weighed and added to 100 mL of deionized water to prepare a mixed alkali solution; 7.5 mmol Ni(NO3)2·6H2O (2.181 g), 7.5 mmol Mg(NO3)2·6H2O (1.923 g), 4.5 mmol Al(NO3)3·9H2O (1.688 g) and 0.5 mmol Ce(NO3)3·6H2O (0.217 g) were weighed and added to 100 mL of deionized water to prepare a mixed salt solution. The above mixed alkali solution was added dropwise under vigorous stirring until pH = 10.0 ± 0.1 and stabilized for 10 minutes. Then, the mixed salt and mixed alkali solution were added dropwise at the same time, and the pH was maintained at 10.0±0.1; after the salt solution was added dropwise, the resulting reaction solution was crystallized in a 65°C water bath for 6 hours. Finally, the mixture was centrifuged and washed with deionized water until the supernatant was neutral, and the resulting precipitate was vacuum freeze-dried for 6 hours to obtain a multi-level structure nanosheet array type hybrid carrier Ni 1.5 Mg 1.5 Al 0.9 Ce 0.1 -LDH / rGO.

[0104] (3) Preparation of 0.2-PdNCs / NiMgAlCe(O) / rGO-300 catalyst

[0105] 1.0 g of Ni obtained in step (2) 1.5 Mg 1.5 Al 0.9 Ce 0.1 -LDH / rGO hybrid carrier was added to 40mL deionized water, and after ultrasonic treatment for 2 minutes, the pH was adjusted to 8±0.1 with Na2CO3 under vigorous stirring at room temperature (1000 rpm) to obtain a carrier suspension. Then 12.2mL Pd-Capt nanocluster aqueous solution (0.1316mg / mL, pH=6.65) was measured and added dropwise to the above carrier suspension, and stirring was continued for 40 minutes. The resulting mixed solution was then centrifuged and the precipitate was vacuum freeze-dried for 6 hours to obtain the catalyst precursor 0.2-Pd-Capt / Ni 1.5 Mg 1.5 Al 0.9 Ce 0.1The obtained precursor was placed in 50 mL / min flowing N2, kept at 300°C for 2 hours at a heating rate of 5°C / min, and then naturally cooled to room temperature to obtain a nanosheet array-type catalyst 0.2-PdNCs / NiMgAlCe(O) / rGO-300.

Claims

1. A graphene-based nanosheet array composite supported palladium cluster catalyst, characterized in that: The expression is x-PdNCs / M1M2(O) / rGO-T, where x represents the mass loading of Pd, which is 0.1-0.5wt%; M1M2(O) represents the composite metal oxide obtained by topological transformation of layered double hydroxide precursors, and M1 is Ni 2+ 、Co 2+ and Mg 2+ Any one or two of the divalent metal cations, M2 is Al 3+ and Ce 3+ Any one or two of the trivalent metal cations, and the molar ratio of M1 to M2 is 3:1; rGO is reduced graphene oxide; T is the calcination temperature, which is 250-320°C; the calcination atmosphere is nitrogen; the obtained catalyst has a multi-level nanosheet array morphology, wherein the M1M2(O) nanosheets are vertically oriented and grown on both sides of the rGO sheet, and PdNCs with a size of 1.3-1.8 nm are highly dispersed at the edge of the M1M2(O) nanosheets; The preparation method of the catalyst comprises the following preparation steps: (1) Preparation of water-soluble ultrafine Pd-Capt nanoclusters Captopril-protected water-soluble ultrafine palladium nanoclusters were prepared by a simple chemical reduction method. The specific preparation steps are as follows: at 25±1°C, 5.88 mL of a 10 mg / mL Na2PdCl4 methanol solution was added to a 50 mL single-necked flask, and then 4.12 mL of methanol was added to the flask to make the volume 10 mL. After magnetic stirring at a speed of 1200 rpm for 3 minutes, 0.1269 g of white tetraoctylammonium bromide crystals were added under continuous stirring, and the solution immediately changed from brown-red to dark red; stirring was continued for 20 minutes, and then 5 mL of a methanol solution containing 0.0435 g of captopril (Capt) was added, and the color immediately changed to light red; after continuous stirring for 30 minutes, 5 mL of an ice-water solution containing 0.0759 g of NaBH4 was added, and the solution immediately turned black; after reacting for 8 to 10 hours, the reaction mixture was The mixture was centrifuged at 5000 rpm for 10 minutes to remove a small amount of insoluble Pd(II):Capt polymer, the supernatant was rotary evaporated at 30-50°C for 15-25 minutes, 1 mL of methanol was added to the concentrated solution to dissolve the product adhering to the wall of the flask, and then 25-50 mL of anhydrous ethanol was added and allowed to stand overnight to obtain a cluster precipitate; the obtained precipitate was vacuum dried at 30-60°C for 10-16 hours to obtain a crude product; then, the crude product was extracted and purified 3-6 times with 1-3 mL of methanol to remove the substances insoluble in methanol, and 25-50 mL of anhydrous ethanol was added to obtain a nanocluster precipitate, which was centrifuged and the obtained precipitate was vacuum dried at 30-60°C for 10-16 hours to obtain a purified Pd nanocluster black powder, named Pd-Capt, which was dissolved in deionized water to prepare a 100 mL solution; (2) Preparation of nanosheet array-like M1M2-LDH / rGO hybrid carrier The nanosheet array-type M1M2-LDH / rGO hybrid carrier was prepared by aqueous coprecipitation method. The specific preparation steps were as follows: 7.7 mL of 6.5 mg / mL graphite oxide, i.e., GO sol, was dispersed in 100 mL of deionized water and ultrasonicated for 15 to 20 minutes to obtain an exfoliated GO suspension; then 25 mg of citric acid was added and ultrasonicated for 5 to 10 minutes to obtain a citric acid-modified GO suspension; NaOH and Na2CO3 were dissolved in 100 mL of deionized water to prepare a mixed alkaline solution, wherein OH - and CO3 2- The molar concentration ratio is 3.2; the nitrates of M1 and M2 are added to 100 mL of deionized water to prepare a mixed salt solution, where M1 is Ni 2+ 、Co 2+ and Mg 2 + Any one or two of the divalent metal cations, M2 is Al 3+ and Ce 3+ Any one or two of the trivalent metal cations, the total amount of M1 and M2 is 20mmol, the molar ratio of M1 to M2 is 3:1, and CO3 2- The molar concentration ratio of M2 to M2 is 2; the mixed alkali solution is added dropwise to the above citric acid-modified GO suspension under vigorous stirring until the pH is 10.0±0.1, and stabilized for 5 to 10 minutes to deprotonate the citric acid on the GO surface to form -COO - anion; then add mixed salt and mixed alkali solution at the same time, and keep pH = 10.0 ± 0.1; after the salt solution is added, the obtained reaction solution is crystallized in a water bath at 65-80°C for 4-6 hours; finally, centrifugation is performed, and the supernatant is washed with deionized water until it is neutral, and the obtained precipitate is vacuum freeze-dried for 6 hours to obtain a multi-level structure nanosheet array type hybrid carrier M1M2-LDH / rGO; (3) Preparation of nanosheet array-like supported palladium nanocluster catalyst x-PdNCs / M1M2(O) / rGO-T 1.0 g of the M1M2-LDH / rGO hybrid carrier obtained in step (2) was added to 40 mL of deionized water, ultrasonicated for 2 to 5 minutes, and adjusted to pH = 6.5 to 9.5 with Na2CO3 under vigorous stirring at a speed of 1000 rpm at room temperature to obtain a carrier suspension; then the Pd-Capt nanocluster aqueous solution obtained in step (1) was added dropwise to the above carrier suspension, with a theoretical loading amount of 0.1 to 0.5 wt%, and stirring was continued for 40 minutes; then the obtained mixed solution was centrifuged, and the precipitate was vacuum freeze-dried for 6 hours to obtain a catalyst precursor x-Pd-Capt / M1M2-LDH / rGO; the obtained precursor was placed in 50 to 200 mL / min of flowing N2, maintained at 250 to 320°C for 2 to 4 hours at a heating rate of 1 to 5°C / min, and then naturally cooled to room temperature to obtain a nanosheet array-like supported palladium nanocluster catalyst x-PdNCs / M1M2(O) / rGO-T.

2. A method for preparing the graphene-based nanosheet array composite metal oxide supported water-soluble ultrafine palladium nanoclusters (PdNCs) catalyst according to claim 1, characterized in that: The method comprises the following preparation steps: (1) Preparation of water-soluble ultrafine Pd-Capt nanoclusters Captopril-protected water-soluble ultrafine palladium nanoclusters were prepared by a simple chemical reduction method. The specific preparation steps are as follows: at 25±1°C, 5.88 mL of a 10 mg / mL Na2PdCl4 methanol solution was added to a 50 mL single-necked flask, and then 4.12 mL of methanol was added to the flask to make the volume 10 mL. After magnetic stirring at a speed of 1200 rpm for 3 minutes, 0.1269 g of white tetraoctylammonium bromide crystals were added under continuous stirring, and the solution immediately changed from brown-red to dark red; stirring was continued for 20 minutes, and then 5 mL of a methanol solution containing 0.0435 g of captopril (Capt) was added, and the color immediately changed to light red; after continuous stirring for 30 minutes, 5 mL of an ice-water solution containing 0.0759 g of NaBH4 was added, and the solution immediately turned black; after reacting for 8 to 10 hours, the reaction mixture was The mixture was centrifuged at 5000 rpm for 10 minutes to remove a small amount of insoluble Pd(II):Capt polymer, the supernatant was rotary evaporated at 30-50°C for 15-25 minutes, 1 mL of methanol was added to the concentrated solution to dissolve the product adhering to the wall of the flask, and then 25-50 mL of anhydrous ethanol was added and allowed to stand overnight to obtain a cluster precipitate; the obtained precipitate was vacuum dried at 30-60°C for 10-16 hours to obtain a crude product; then, the crude product was extracted and purified 3-6 times with 1-3 mL of methanol to remove the substances insoluble in methanol, and 25-50 mL of anhydrous ethanol was added to obtain a nanocluster precipitate, which was centrifuged and the obtained precipitate was vacuum dried at 30-60°C for 10-16 hours to obtain a purified Pd nanocluster black powder, named Pd-Capt, which was dissolved in deionized water to prepare a 100 mL solution; (2) Preparation of nanosheet array-like M1M2-LDH / rGO hybrid carrier The nanosheet array-type M1M2-LDH / rGO hybrid carrier was prepared by aqueous coprecipitation method. The specific preparation steps were as follows: 7.7 mL of 6.5 mg / mL graphite oxide, i.e., GO sol, was dispersed in 100 mL of deionized water and ultrasonicated for 15 to 20 minutes to obtain an exfoliated GO suspension; then 25 mg of citric acid was added and ultrasonicated for 5 to 10 minutes to obtain a citric acid-modified GO suspension; NaOH and Na2CO3 were dissolved in 100 mL of deionized water to prepare a mixed alkaline solution, wherein OH - and CO3 2- The molar concentration ratio is 3.2; the nitrates of M1 and M2 are added to 100 mL of deionized water to prepare a mixed salt solution, where M1 is Ni 2+ 、Co 2+ and Mg 2 + Any one or two of the divalent metal cations, M2 is Al 3+ and Ce 3+ Any one or two of the trivalent metal cations, the total amount of M1 and M2 is 20mmol, the molar ratio of M1 to M2 is 3:1, and CO3 2- The molar concentration ratio of M2 to M2 is 2; the mixed alkali solution is added dropwise to the above citric acid-modified GO suspension under vigorous stirring until the pH is 10.0±0.1, and stabilized for 5 to 10 minutes to deprotonate the citric acid on the GO surface to form -COO - anion; then add mixed salt and mixed alkali solution at the same time, and keep pH = 10.0 ± 0.1; after the salt solution is added, the obtained reaction solution is crystallized in a water bath at 65-80°C for 4-6 hours; finally, centrifugation is performed, and the supernatant is washed with deionized water until it is neutral, and the obtained precipitate is vacuum freeze-dried for 6 hours to obtain a multi-level structure nanosheet array type hybrid carrier M1M2-LDH / rGO; (3) Preparation of nanosheet array-like supported palladium nanocluster catalyst x-PdNCs / M1M2(O) / rGO-T 1.0 g of the M1M2-LDH / rGO hybrid carrier obtained in step (2) was added to 40 mL of deionized water, ultrasonicated for 2 to 5 minutes, and adjusted to pH = 6.5 to 9.5 with Na2CO3 under vigorous stirring at a speed of 1000 rpm at room temperature to obtain a carrier suspension; then the Pd-Capt nanocluster aqueous solution obtained in step (1) was added dropwise to the above carrier suspension, with a theoretical loading amount of 0.1 to 0.5 wt%, and stirring was continued for 40 minutes; then the obtained mixed solution was centrifuged, and the precipitate was vacuum freeze-dried for 6 hours to obtain a catalyst precursor x-Pd-Capt / M1M2-LDH / rGO; the obtained precursor was placed in 50 to 200 mL / min of flowing N2, maintained at 250 to 320°C for 2 to 4 hours at a heating rate of 1 to 5°C / min, and then naturally cooled to room temperature to obtain a nanosheet array-like supported palladium nanocluster catalyst x-PdNCs / M1M2(O) / rGO-T.