A method for preparing a PVDF ultrafiltration membrane with polyester lining

By using polyester braided tube lining and PVDF materials in the hollow fiber membrane, combined with PMMA and other additives, and using a non-solvent phase inversion method, the problem of insufficient mechanical strength of the hollow fiber membrane is solved, and high strength and good stability are prepared. Ultrafiltration membrane, suitable for industrial applications.

CN113813799BActive Publication Date: 2024-10-15白琳
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202111068231.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-13
Publication Date
2024-10-15
Estimated Expiration
2041-09-13

AI Technical Summary

Technical Problem

Existing hollow fiber membranes are easily damaged by high-pressure water or airflow during use, and their mechanical strength is low, making it difficult to balance compressive strength and tensile strength. The preparation process is complex, resulting in adhesion between the support and the membrane separation layer. Insufficient, affecting the service life of the membrane.

Method used

Using polyester braided tube as the inner lining, PVDF as the membrane material, PMMA as the binder, BD-3071, PVP-k30 and glycerin as additives, a high-strength modified ultrafiltration membrane is prepared in one step through a non-solvent phase inversion method to enhance Mechanical strength and adhesion of the film.

Benefits of technology

The prepared ultrafiltration membrane has high pressure resistance, stable operation capability, easy operation, mild preparation conditions, low cost, is suitable for industrial applications, and significantly improves the service life and performance of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113813799B_ABST
    Figure CN113813799B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a PVDF ultrafiltration membrane with a polyester liner. A polyester braided tube is used as the liner, PVDF as the membrane material, DMAc as the solvent, BD-3071 as the dispersant, and PMMA, PVP-K30, and glycerol as additives. The mixture is stirred at 65-75°C for 16-20 hours, followed by a 12-16 hour settling period for degassing. A metering pump delivers the casting solution to the spinneret at a rate of 300-350 ml / min, with the polyester liner passing through the center of the spinneret. The casting solution is uniformly coated on the outer surface of the polyester braided tube, and the core solution (pure water) flows at a rate of 120-180 ml / min. The braided tube coated with the casting solution is then placed in a gel bath containing an aqueous DMAc solution and undergoes phase inversion at 32-38°C to form a membrane. The solidified membrane fibers are collected by a take-up wheel at a rate of 18-23 m / min and then soaked in water-glycerol mixed solutions with different proportions in stages to obtain a polyester-lined reinforced PVDF ultrafiltration membrane. The ultrafiltration membrane of the present invention has high pressure resistance, strong adhesion between the membrane separation layer and the inner liner, and can operate stably for a long time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer membrane materials, in particular to a method for preparing a PVDF ultrafiltration membrane with a polyester lining. Background Art

[0002] Human survival and social development cannot be separated from the support of water resources. With the acceleration of industrialization and population growth, the shortage of freshwater resources has become a global problem. Seawater desalination and wastewater reuse is a sustainable means to solve the water crisis. Membrane separation technology has the advantages of room temperature operation, no phase change, small footprint, high efficiency, modular design and easy combination with other processes. As a new, efficient and green separation technology, membrane separation has been widely used in petrochemical, biomedicine, food processing, environmental protection, metallurgy, seawater desalination, medical and other fields, especially suitable for the urgent needs of modern industry for energy conservation and emission reduction, efficient use of resources and so on.

[0003] An ideal separation membrane should have high permeability, good mechanical strength and chemical stability. The selection of membrane-forming materials and the membrane preparation process will directly affect the above-mentioned properties of the membrane. For membranes used in commercial applications, their mechanical strength and permeation selectivity are important indicators for measuring membrane performance. Hollow fiber membrane is a self-supporting membrane with advantages such as high packing density, large specific surface area and easy assembly. It has been widely used in deep treatment of sewage. However, hollow fiber membranes generally have low strength, making them easily damaged by high-pressure water or air flow during use. There have been a lot of studies on improving the mechanical strength of hollow fiber membranes, and introducing reinforcement into the membrane has been proven to be an effective method.

[0004] The enhanced central control fiber membrane is generally composed of three parts, namely the internal reinforcement, the membrane separation layer and the interface bonding layer between the two. The interface bonding layer determines the bonding force between the reinforcement and the separation layer, and has a crucial impact on the membrane performance. At present, the enhanced hollow fiber membranes at home and abroad are mainly divided into long fiber reinforced and fiber tube reinforced hollow fiber membranes, but the long fiber reinforced central control fiber membrane cannot take into account both compressive strength and tensile strength. The fiber tube reinforced hollow fiber membrane is made by coating the casting liquid on the outer surface of the fiber tube, which can maximize the strength of the fiber membrane while ensuring the membrane separation performance, but its preparation process is complicated and difficult to operate. There are still many problems to be solved. Among them, how to improve the adhesion between the support body and the membrane separation layer is directly related to the service life of the membrane. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present invention is to provide a method for preparing a PVDF ultrafiltration membrane with a polyester lining, which uses a polyester braided tube as the lining, PVDF as the membrane material, PMMA as a binder to enhance the bonding force between the lining and the membrane material, BD-3071, PVP-k30 and glycerol as additives to regulate the membrane microstructure and hydrophilicity, and prepares a high-strength modified ultrafiltration membrane in one step through a non-solvent-induced phase transformation method.

[0006] The technical scheme of the present invention is a method for preparing a PVDF ultrafiltration membrane with a polyester lining, a. using a polyester braided tube as an inner lining, PVDF as a membrane material, DMAc as a solvent, polyether-modified polydimethylsiloxane (BD-3071) as a dispersant, polymethyl methacrylate (PMMA), PVP-k30 and glycerol as additives, wherein the addition amount of PMMA is 0.05wt% to 2.5wt%, the addition amount of BD-3071 is 0.05wt% to 2.5wt%, the addition amount of PVP-k30 is 1wt% to 12wt%, and the addition amount of glycerol is 1wt% to 12wt%, and the mixture is stirred at 65-75°C for 16-20h and then allowed to stand for degassing for 12-16h;

[0007] b. The casting liquid is delivered to the spinneret at a speed of 300-350 ml / min by a metering pump, the polyester liner passes through the center of the spinneret, the casting liquid is evenly coated on the outer surface of the polyester braided tube, and the flow rate of the core liquid pure water is 120-180 ml / min; the braided tube coated with the casting liquid enters a gel bath containing a DMAc aqueous solution and phase-converts into a membrane at 32-38°C;

[0008] c. The solidified membrane filaments are collected by a collection wheel at 18-23 m / min and then immersed in water-glycerol mixed solutions with different proportions in stages to finally obtain a polyester lined reinforced PVDF ultrafiltration membrane.

[0009] Polyester has good elasticity and is not easy to deform. It has the best thermal stability among synthetic fibers. This property is conducive to the uniform coverage of the casting liquid on its surface. The above addition ratio is the content of each component in 100g of casting liquid.

[0010] The PVDF membrane is located on the outer interface of the braided tube and is in a coaxial cylindrical relationship with the braided tube.

[0011] After the conversion into a membrane, the membrane of the present invention can only be obtained by a sufficient solvent and non-solvent exchange process, that is, water is used to replace the small amount of solvent in the membrane after the initial solidification. The purpose of collecting the wire is to roll up the membrane for subsequent processing. On the one hand, soaking allows the solvent and non-solvent to be fully exchanged, and on the other hand, it allows glycerol to enter the membrane pores so that the membrane will not collapse due to excessive evaporation of water during the drying process. Membranes containing reinforced linings can be called reinforced membranes, such as the polyester braided tube in the present invention.

[0012] Preferably, the water-glycerol mixed solution of different proportions described in step c refers to soaking in water-glycerol ratios of 9.5-10.5:1, 6.5-7.5:3, 4.5-5.5:5, and 2-3:6-7. First soak in a water-glycerol solution of 9.5-10.5:1 for 10-12 hours, and then soak in a water-glycerol solution of 6.5-7.5:3, 4.5-5.5:5, and 2-3:6-7 for 3 to 5 hours. Finally, take out the membrane and hang it to dry. The ratio is a weight ratio. Soaking in water-glycerol solutions of different proportions can effectively prevent the shrinkage of the membrane pores.

[0013] According to the method for preparing a polyester lined PVDF ultrafiltration membrane of the present invention, preferably, the stirring speed is 70-90 rpm.

[0014] According to the method for preparing a polyester-lined PVDF ultrafiltration membrane of the present invention, preferably, the concentration of the DMAc aqueous solution is 0.5-2 wt %.

[0015] According to the method for preparing a polyester lined PVDF ultrafiltration membrane of the present invention, preferably, the polyester braided tube has an inner diameter of 0.6-1.0 mm, an outer diameter of 1.6-2.0 mm, and a pore size of 0.3-0.5 mm.

[0016] According to the method for preparing a polyester-lined PVDF ultrafiltration membrane of the present invention, preferably, the amount of PMMA added is 0.1% to 2%.

[0017] According to the method for preparing a polyester lined PVDF ultrafiltration membrane of the present invention, preferably, the addition amount of BD-3071 is 0.1% to 2%.

[0018] According to the method for preparing a polyester-lined PVDF ultrafiltration membrane of the present invention, preferably, the addition amount of the PVP-k30 is 2% to 10%.

[0019] According to the method for preparing a polyester-lined PVDF ultrafiltration membrane of the present invention, preferably, the added amount of glycerol is 2% to 10%.

[0020] According to the method for preparing a polyester-lined PVDF ultrafiltration membrane of the present invention, preferably, the pure water flux of the prepared ultrafiltration membrane is 140-160 L / (m 2 ·h); bubble point pressure is 0.04-0.06MPa.

[0021] The treatment capacity for wastewater with a turbidity of 0.484 NTU is 110-130 L / (m 2 h), the turbidity of the treated wastewater is <0.1NTU.

[0022] Compared with the prior art, the present invention has the following positive effects:

[0023] The positive significance of the present invention is that the prepared ultrafiltration membrane has high compressive strength, the adhesion between the membrane separation layer and the inner lining is strong, and it can operate stably for a long time. The ultrafiltration membrane prepared with polyester braided tube as the inner lining is easy to operate, has mild preparation conditions, low cost, and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is a scanning electron microscope cross-sectional view of the ultrafiltration membrane of Example 1;

[0025] Figure 2 This is a scanning electron microscope surface image of the ultrafiltration membrane of Example 1;

[0026] Figure 3 is a scanning electron microscope cross-sectional view of the ultrafiltration membrane of Example 1;

[0027] Figure 4 is a scanning electron microscope cross-sectional view of the ultrafiltration membrane of Example 1;

[0028] Figure 5 This is a schematic diagram of the performance test of the ultrafiltration membrane of Example 3. DETAILED DESCRIPTION

[0029] The following provides a specific embodiment of the method for preparing a polyester lined PVDF ultrafiltration membrane of the present invention.

[0030] A method for preparing a polyester lined PVDF ultrafiltration membrane, which specifically comprises:

[0031] The prepared ultrafiltration membrane was pre-pressed with pure water at 0.02 MPa for half an hour, and the water flux of the membrane was tested with pure water. The calculation formula is shown in (1).

[0032]

[0033] Where J is the flux of the membrane (L / (m 2 ·h)), V is the volume of the collected permeate (L), A is the effective area of ​​the membrane (m 2 ), T is the time (h) required to collect V volume of permeate.

[0034] The retention performance of the membrane was tested using 20 ppm BAS solution as the feed solution. The sample was tested after 30 minutes. The calculation method is shown in (2).

[0035]

[0036] Where R is the retention rate of the membrane, C pis the concentration on the permeate side (ppm), C f is the concentration on the feed side (ppm).

[0037] The concentration of the organic solution was measured by a total organic carbon (TOC) analyzer to determine its retention rate.

[0038] The membrane after filtering BSA was washed with pure water and then its pure water flux was tested. The calculation method of the washing recovery rate was shown in (3).

[0039]

[0040] Among them J w1 is the initial pure water flux (L / (m 2 h)), J w2 is the pure water flux of the membrane after cleaning (L / (m 2 h)).

[0041] The tensile strength of the film was tested using a tensile strength tester.

[0042] The bubble pressure meter measures the bubble point pressure of the membrane.

[0043] The preliminary preparation of the present invention comprises the following steps:

[0044] (1) Control of the experimental environment: Adjust the temperature of the experimental environment to between 15°C and 35°C, and control the relative humidity of the laboratory to 45-65%.

[0045] (2) Fabrication of membrane components: The membrane fibers were dried in the above experimental environment until there were no droplets on the surface, and then the dried membrane fibers were cast into components using polyurethane hard glue and soft glue with hardness of 70-80D and 30-40A respectively.

[0046] Example 1

[0047] The polyester braided tube is used as the inner lining and PVDF is used as the membrane material. The inner diameter of the polyester braided tube is 0.6mm, the outer diameter is 1.6mm, and the pore size is 0.3mm. The addition amount of PMMA is 0.05wt%, the addition amount of BD-3071 is 1%, the addition amount of PVP-k30 is 5wt%, and the addition amount of glycerol is 4wt%. After stirring at 68°C for 16h, it is placed for degassing for 12h. The casting liquid is transported to the spinneret at a speed of 310ml / min by a metering pump. The polyester lining passes through the center of the spinneret, and the casting liquid is evenly coated on the outer surface of the polyester braided tube. The flow rate of the core liquid pure water is 120ml / min; the braided tube coated with the casting liquid enters the gel bath containing DMAc aqueous solution at 35°C to form a membrane; the solidified membrane filaments are collected by the collection wheel at 20m / min and then immersed in a water-glycerol mixed solution with different proportions in stages, and finally a polyester lining reinforced PVDF ultrafiltration membrane is obtained.

[0048] The membranes were immersed in water-glycerol solutions with a ratio of 9:1, 6.5:3, 5:5, and 3:6, respectively. The membranes were first immersed in a 9:1 water-glycerol solution for 10 h, and then immersed in the water-glycerol solutions with the latter three ratios for 3.5 h. Finally, the membranes were taken out and hung to dry.

[0049] The ultrafiltration membrane fibers were encapsulated in the assembly with sealant, and the completed membrane assembly was installed in the test device. The water flux and organic matter retention performance were tested. The test results are as follows.

[0050]

[0051] Actual wastewater was used as influent to investigate the separation performance of the membrane. The test results are as follows.

[0052]

[0053] Example 2

[0054] The polyester braided tube is used as the inner lining, and PVDF is used as the membrane material. The inner diameter of the polyester braided tube is 0.8 mm, the outer diameter is 1.8 mm, and the pore size is 0.4 mm. The addition amount of PMMA is 0.5 wt%, the addition amount of BD-3071 is 1.8%, the addition amount of PVP-k30 is 1 wt%, and the addition amount of glycerol is 1 wt%. After stirring at 70°C for 18 hours, the mixture is allowed to stand for degassing for 14 hours. The casting liquid is transported to the spinneret at a speed of 320 ml / min by a metering pump. The polyester lining passes through the center of the spinneret, and the casting liquid is evenly coated on the outer surface of the polyester braided tube. The flow rate of the core liquid pure water is 150 ml / min. The braided tube coated with the casting liquid enters a gel bath containing a DMAc aqueous solution and phase-transforms into a membrane at 32°C. The solidified membrane filaments are collected by a collection wheel at 18 m / min and then immersed in a water-glycerol mixed solution with different proportions in stages, and finally a polyester lining reinforced PVDF ultrafiltration membrane is obtained. The membranes were immersed in water-glycerol solutions with a ratio of 9.5:1, 7:3, 5.5:5, and 3:7. The membranes were first immersed in a water-glycerol solution with a ratio of 9.5:1 for 11 hours, and then immersed in water-glycerol solutions with the latter three ratios for 4 hours. Finally, the membranes were taken out and hung to dry.

[0055] The ultrafiltration membrane fibers were encapsulated in the assembly with sealant, and the completed membrane assembly was installed in the test device. The water flux and organic matter retention performance were tested. The test results are as follows.

[0056]

[0057] Actual wastewater was used as influent to investigate the separation performance of the membrane. The test results are as follows.

[0058]

[0059] Example 3

[0060] The polyester braided tube is used as the inner lining, and PVDF is used as the membrane material. The inner diameter of the polyester braided tube is 1.0 mm, the outer diameter is 2.0 mm, and the pore size is 0.5 mm. The addition amount of PMMA is 2.3 wt%, the addition amount of BD-3071 is 0.1%, the addition amount of PVP-k30 is 10 wt%, and the addition amount of the glycerol is 9 wt%. After stirring at 72 ° C for 19 hours, the film is placed for degassing for 16 hours. The casting liquid is transported to the spinneret at a speed of 350 ml / min by a metering pump. The polyester lining passes through the center of the spinneret, and the casting liquid is evenly coated on the outer surface of the polyester braided tube. The flow rate of the core liquid pure water is 180 ml / min; the braided tube coated with the casting liquid enters the gel bath containing DMAc aqueous solution at 38 ° C to phase transform into a membrane; the solidified membrane filaments are collected by a collection wheel at 23 m / min and then immersed in a water-glycerol mixed solution with different proportions in stages, and finally a polyester lining reinforced PVDF ultrafiltration membrane is obtained. The membranes were immersed in water-glycerol solutions with a ratio of 10:1, 7.5:3, 5:5, and 2.5:6. The membranes were first immersed in the 10:1 water-glycerol solution for 12 hours, and then immersed in the three water-glycerol solutions with the latter ratios for 5 hours. Finally, the membranes were taken out and hung to dry.

[0061] The ultrafiltration membrane fibers were encapsulated in the assembly with sealant, and the completed membrane assembly was installed in the test device. The water flux and organic matter retention performance were tested. The test results are as follows.

[0062]

[0063] Actual wastewater was used as influent to investigate the separation performance of the membrane. The test results are as follows.

[0064]

[0065] The stability of the membrane was investigated, and the test results were as follows Figure 5 .

[0066] The invention uses a polyester braided tube as an inner lining and adopts a non-solvent-induced phase conversion method to prepare a high-strength, high-flux, and stable-performance enhanced PVDF ultrafiltration membrane. The invention has a simple process and significant industrial practical value.

Claims

1. A method for preparing a polyester lined PVDF ultrafiltration membrane, characterized in that: The steps include: a. A polyester braided tube is used as the inner lining, PVDF is used as the membrane material, DMAc is used as the solvent, polyether modified polydimethylsiloxane BD-3071 is used as the dispersant, polymethyl methacrylate PMMA, PVP-k30 and glycerol are used as additives, the addition amount of PMMA is 0.05wt% to 2.5wt%, the addition amount of BD-3071 is 0.05wt% to 2.5wt%, the addition amount of PVP-k30 is 1wt% to 12wt%, the addition amount of glycerol is 1wt% to 12wt%, and the mixture is stirred at 65-75°C for 16-20h and then allowed to stand for degassing for 12-16h; the above addition amount ratio is the content of each component in 100g of the casting solution; b. The casting liquid is delivered to the spinneret at a speed of 300-350 ml / min by a metering pump, the polyester liner passes through the center of the spinneret, the casting liquid is evenly coated on the outer surface of the polyester braided tube, and the flow rate of the core liquid pure water is 120-180 ml / min; the braided tube coated with the casting liquid enters a gel bath containing a DMAc aqueous solution and phase-converts into a membrane at 32-38°C; c. The solidified membrane filaments are collected by a collecting wheel at 18-23 m / min and then immersed in water-glycerol mixed solutions with different proportions in stages to finally obtain a polyester lined reinforced PVDF ultrafiltration membrane; the immersion in water-glycerol mixed solutions with different proportions in stages refers to immersion in water-glycerol weight ratios of 9.5-10.5:1, 6.5-7.5:3, 4.5-5.5:5, and 2-3:6-7, respectively; first, immersion in a water-glycerol solution of 9.5-10.5:1 for 10-12 hours, and then immersion in water-glycerol solutions of 6.5-7.5:3, 4.5-5.5:5, and 2-3:6-7 for 3 to 5 hours, respectively.

2. The method for preparing a polyester lined PVDF ultrafiltration membrane according to claim 1, characterized in that: The stirring speed is 70-90 rpm.

3. The method for preparing a polyester lined PVDF ultrafiltration membrane according to claim 1, characterized in that: The concentration of the DMAc aqueous solution is 0.5-2 wt %.

4. The method for preparing a polyester lined PVDF ultrafiltration membrane according to claim 1, characterized in that: The inner diameter of the polyester braided tube is 0.6-1.0mm, the outer diameter is 1.6-2.0mm, and the pore size is 0.3-0.5mm.

5. The method for preparing a polyester lined PVDF ultrafiltration membrane according to claim 1, characterized in that: The addition amount of PMMA is 0.1 wt% to 2 wt%.

6. The method for preparing a polyester lined PVDF ultrafiltration membrane according to claim 1, characterized in that: The addition amount of BD-3071 is 0.1 wt% to 2 wt%.

7. The method for preparing a polyester lined PVDF ultrafiltration membrane according to claim 1, characterized in that: The added amount of the PVP-k30 is 2wt% to 10wt%.

8. The method for preparing a polyester lined PVDF ultrafiltration membrane according to claim 1, characterized in that: The added amount of the glycerol is 2wt% to 10wt%.

9. The method for preparing a polyester lined PVDF ultrafiltration membrane according to claim 1, characterized in that: The pure water flux of the prepared ultrafiltration membrane is 140-160L / (m 2 ·h); bubble point pressure is 0.04-0.06Mpa; The prepared ultrafiltration membrane was pre-pressed with pure water at 0.02 MPa for half an hour, and the water flux of the membrane was tested with pure water. The calculation formula is shown in (1): Where J is the flux of the membrane (L / (m 2 ·h)), V is the volume of the collected permeate (L), A is the effective area of ​​the membrane (m 2 ), T is the time required to collect V volume of permeate (h); The retention performance of the membrane was tested using a 20 ppm BAS solution as the feed solution. The sample was tested after 30 minutes. The calculation method is shown in (2): Where R is the retention rate of the membrane, C p is the concentration on the permeate side (ppm), C f is the concentration on the feed side (ppm); The concentration of the organic solution is measured by a total organic carbon (TOC) analyzer to determine its retention rate; After filtering BSA, the membrane was washed with pure water and then its pure water flux was tested. The calculation method of the washing recovery rate is shown in (3): Among them J w1 is the initial pure water flux (L / (m 2 h)), J w2 is the pure water flux of the membrane after cleaning (L / (m 2 h)); The tensile strength of the film was tested using a tensile strength tester; The bubble pressure meter measures the bubble point pressure of the membrane.

Citation Information

Patent Citations

  • Polyvinyl chloride membrane with supporting materials and preparation method thereof

    CN102343220A

  • Hollow fiber membrane having a reinforced monofilament

    CN103501881A

  • Reinforced composite supported hollow fiber membrane and preparation method thereof

    CN104117289A

  • High-pollution-resistance type polyvinylidene fluoride (PVDF) hollow fiber ultrafiltration membrane, preparation method and device

    CN106731897A

  • Preparation method of reinforced PVDF hollow fiber film applied to compound braided tubes

    CN106861462A