High temperature resistant magnet and method for manufacturing the same

By designing the grain boundary structure of low melting point magnets and a specific diffusion source film in the neodymium iron bo magnet to form a specific grain boundary structure, the problems of poor coercive force and high temperature resistance of the neodymium iron bo magnet are solved, and the coercive force and Improved high temperature resistance and suitable for mass production.

CN113871121BActive Publication Date: 2024-12-03YANTAI DONGXING MAGNETIC MATERIALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111120165.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-24
Publication Date
2024-12-03
Estimated Expiration
2041-09-24

AI Technical Summary

Technical Problem

Existing neodymium iron boron magnets have poor high temperature resistance when improving coercive force, making it difficult to maintain high efficiency in mass production.

Method used

By designing a grain boundary structure with low melting point magnets and forming a specific diffusion source film on it, diffusion and aging treatment are performed to form a neodymium iron boron magnet with a specific grain boundary structure, including the main phase, rare earth shell, and transition metal shell. The layer and triangular zone regulate components and structures to improve coercive force and high temperature resistance.

Benefits of technology

The coercive force has been greatly improved, and the high temperature resistance of magnets is improved, and the disadvantages of low melting point magnets and diffusion sources have been overcome. It is suitable for mass production, and the diffusion efficiency of diffusion sources is improved, forming Effective magnetic insulation shell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113871121B_ABST
    Figure CN113871121B_ABST
Patent Text Reader

Abstract

The present invention discloses a high temperature resistant magnet and a manufacturing method, belonging to the field of magnet preparation. By designing the grain boundary as a low melting point magnet, forming a special diffusion source on the magnet, and performing diffusion and aging treatment, a high performance and high temperature resistant neodymium iron boron magnet is obtained. The chemical formula of the low heavy rare earth diffusion source is R 1x R 2y H z M 1‑x‑y‑z , wherein R1 refers to at least one of Nd and Pr, R2 is at least one of Ho and Gd, H refers to at least one of Tb and Dy, and M refers to at least one of Al, Cu, Ga, Ti, Co, Mg, Zn, and Sn, wherein 15<x<50, 0<y≤10, 40≤z≤70, and the ratio is weight percentage, and a triangular area point scanning composition having a grain boundary structure including a main phase, a shell layer, and a specific composition is obtained. A high temperature resistant magnet and a manufacturing method described in the present invention have greatly improved high temperature resistance and coercivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of magnets and magnet preparation, and in particular to a high temperature resistant magnet and a manufacturing method thereof. Background Art

[0002] NdFeB sintered permanent magnets are widely used in high-tech fields such as electronic information, medical equipment, new energy vehicles, household appliances, robots, etc. In the past few decades, NdFeB permanent magnets have developed rapidly, and the residual magnetic properties have basically reached the theoretical limit. However, the coercive force is still far from the theoretical value. Therefore, improving the coercive force of magnets is a major research hotspot.

[0003] Since the traditional manufacturing process consumes a large amount of Tb or Dy heavy rare earth metals, the cost increases. Although the heavy rare earth content can be greatly reduced through grain boundary diffusion technology, the cost is still very high as the current heavy rare earth Tb price soars. Therefore, it is still important to continue to reduce the content of heavy rare earths. The coercive force can be increased by forming a large number of core-shell structures through diffusion hardening of the Nd2Fe14B main phase containing heavy rare earth elements. Therefore, the research on magnets and diffusion sources has become the focus of this program.

[0004] Although the most significant effect of improving coercivity is achieved through the diffusion of heavy rare earths, the abundance of heavy rare earths is low and the price is expensive. Therefore, more and more researchers have achieved the purpose of increasing the coercivity of magnets by diffusion by preparing low-melting-point heavy rare earth alloys as diffusion sources. There are many applications for special grain boundary phase patents, such as the publication number CN112735717A, entitled a neodymium iron boron material and a preparation method thereof. In this patent, a magnet with a special structure is diffused by coating the surface of the magnet with heavy rare earths Tb and Dy to increase the diffusion depth of the magnet and the coercivity, but this is mainly designed in the magnet itself; the publication number CN105513734A, entitled a patent for a mixture of light and heavy rare earths for neodymium iron boron magnets, a neodymium iron boron magnet and a preparation method thereof, is mainly a patent for the increase in Hcj performance after diffusing the mixture of light and heavy rare earths, but this mixture of light and heavy rare earths has poor uniformity, and it is difficult to play a special role in improving the diffusion coefficient of the magnet after forming an alloy. Although the low melting point heavy rare earth diffusion source can greatly increase the coercive force of the magnet, the high temperature resistance of the magnet is poor, that is, the remanence and coercive force high temperature performance of the magnet are low.

[0005] Therefore, it is necessary to find a method that can increase the diffusion depth, that is, the depth of forming a core-shell structure, through the melting point alloy phase and improve the high temperature resistance of the magnet. Summary of the invention

[0006] Purpose of the invention: In order to overcome the deficiencies in the prior art, the present invention provides a high temperature resistant magnet and a method for manufacturing the same.

[0007] Technical solution: To achieve the above object, the grain boundary structure of the magnet of the present invention includes a main phase structure, an R shell, a transition metal shell and a triangular region, wherein the R shell is at least one of Nd, Pr, Ho and Gd, the transition metal shell is at least one of Cu, Al and Ga, and the triangular region point scan composition includes component I, component II, and / or component III, wherein:

[0008] The component I is Nd a Fe b R c M d , the R is at least one of Pr, Ce, and La, M is at least three of Al, Cu, Ga, Ti, Co, Mg, Zn, Sn, and Zr, the weight percentage of Nd is a, 30%≤a≤70%, the weight percentage of Fe is b, 5%≤b≤40%, the weight percentage of R is c, 5%≤c≤35%, and the weight percentage of M is d, 0%≤d≤15%;

[0009] The component II is Nd e Fe f R g H h K i M j , the R is at least one of Pr, Ce, and La, the H is at least one of Dy and Tb, the K is one of Ho and Gd, the M is at least three of Al, Cu, Ga, Ti, Co, Mg, Zn, Sn, and Zr, the weight percentage of Nd is e, 25%≤e≤65%, the weight percentage of Fe is f, 5%≤f≤35%, the weight percentage of R is g, 5%≤g≤30%, the weight percentage of H is h, 5%≤h≤30%, the weight percentage of K is i, 1%≤i≤12%, and the weight percentage of M is j, 0%≤j≤10%;

[0010] The component III is Nd k Fe l R m D n M o , the R is at least one of Pr, Ce, and La, the D is at least one of Al, Cu, and Ga, the M is at least one of Ti, Co, Mg, Zn, Sn, and Zr, the weight percentage of Nd is k, 30%≤k≤70%, the weight percentage of Fe is l, 5%≤l≤35%, the weight percentage of R is m, 5%≤m≤35%, the weight percentage of D is n, 5%≤n≤25%, and the weight percentage of M is o, 0%≤o≤10%.

[0011] Furthermore, the thickness of the magnet is 0.3-6 mm.

[0012] A method for manufacturing the high temperature resistant magnet comprises the following steps:

[0013] (S1) Smelting and rapidly solidifying the prepared NdFeB alloy raw material to obtain NdFeB alloy flakes, and mechanically crushing the obtained alloy flakes into 150-400 μm scaly alloy flakes;

[0014] (S2) mechanically mixing and stirring the flaky alloy flakes, the low melting point powder, and the lubricant, and then placing the mixture in a hydrogen treatment furnace for hydrogen absorption and dehydrogenation treatment, and preparing NdFeB powder by air jet milling, wherein the particle size of the NdFeB powder is 3-5 μm;

[0015] (S3) pressing the NdFeB powder into a shape and sintering to obtain the desired NdFeB magnet;

[0016] (S4) The sintered NdFeB magnet is machined into a desired shape, and then a low-heavy rare earth diffusion source film is formed on the magnet surface perpendicular or parallel to the C-axis direction by coating, wherein the diffusion source is prepared by atomization powder making, amorphous strip spinning or ingot casting.

[0017] (S5) Finally, diffusion and tempering treatments are performed to obtain the NdFeB magnet with the above-mentioned structural characteristics.

[0018] Preferably, in step (S1), the raw material components of the NdFeB alloy and their weight percentages are 28%≤R≤30%, 0.8%≤B≤1.2%, 0%≤M≤3%, and the rest is Fe, the R is at least two of Nd, Pr, Ce, La, Tb, and Dy, and the M is at least one of Co, Mg, Ti, Zr, Nb, and Mo.

[0019] Preferably, in step (S2), the low melting point powder comprises NdCu, NdAl and NdGa, and the weight percentages thereof are 0%≤NdCu≤3%, 0%≤NdAl≤3%, 0%≤NdGa≤3%, and the low melting point powder is 200nm-4μm.

[0020] Preferably, in step (S2), the dehydrogenation temperature is 400-600°C.

[0021] Preferably, in step (S3), after sintering is completed, argon gas needs to be introduced for cooling, and then a primary tempering treatment and a secondary aging treatment are performed, wherein the sintering temperature is 980-1060°C, and the sintering time is 6-15h; the primary aging temperature is 850°C, and the primary aging time is 3h; the secondary aging temperature is 450-660°C, and the aging time is 3h.

[0022] Preferably, in step (S4), the composition of the low-heavy rare earth diffusion source film is R 1x R 2y H z M 1-x-y-z , wherein the R 1 is at least one of Nd and Pr, wherein R 1 The weight percentage is x, 15%<x<50%, the R 2 is at least one of Ho and Gd, and the R 2 The weight percentage of H is y, 0%<y≤10%, the weight percentage of H is z, 40%≤z≤70%, and the weight percentage of M is 1-xyz.

[0023] Preferably, in step (S5), the diffusion temperature of the NdFeB magnet is 850-930°C, the diffusion time is 6-30h, the aging temperature is 420-680°C, and the secondary aging time is 3-10h.

[0024] Preferably, the heating rate of the aging temperature of the NdFeB magnet is 1-5°C / min, and the cooling rate is 5-20°C / min.

[0025] Compared with the prior art, the present invention has at least the following beneficial effects:

[0026] (1) By designing the grain boundary to be a low melting point magnet and forming a diffusion source with a special function on the magnet, diffusion and aging treatment are performed to obtain a neodymium iron boron magnet with a low heavy rare earth content and a specific grain boundary structure; by regulating the magnet composition and the diffusion source structure, a significant improvement in coercivity is achieved;

[0027] (2) The magnet has high temperature resistance, overcoming the disadvantages of low melting point magnets and diffusion sources that greatly increase coercivity but have poor high temperature resistance, and can achieve mass production of products;

[0028] (3) The designed magnet is subjected to an optimization process test to achieve the best performance and then a diffusion test is performed. The coercive force increase after the Dy alloy is diffused can reach 8-10.5 kOe;

[0029] (4) The diffused magnet matrix contains low melting point phases of NdCu, NdAl, and NdGa, which is beneficial to increase the diffusion coefficient of the magnet grain boundary, thereby improving the diffusion efficiency of the diffusion source;

[0030] (5) The diffusion source not only allows the low melting point phase and the heavy rare earth phase to quickly enter the magnet at the same time, greatly improving the high temperature resistance of the magnet, but also can well form a shell layer with magnetic isolation effect, thereby improving the coercive force. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Schematic diagram of SEM test sampling using a ZISS electron microscope. DETAILED DESCRIPTION

[0032] The following combination Figure 1 The principles and features of the present invention are described, and the examples given are only used to explain the present invention, rather than to limit the scope of the present invention.

[0033] It should also be noted that the term “and / or” is inclusive rather than exclusive, so that it includes not only the listed elements but also some elements that are not explicitly listed, and elements necessary for methods, processes, articles and equipment.

[0034] A method for manufacturing a high temperature resistant magnet comprises the following steps:

[0035] (S1) melting the prepared NdFeB alloy raw material and rapidly solidifying the alloy sheet to obtain NdFeB alloy sheet, and mechanically crushing the obtained alloy sheet into 150-400 μm flaky alloy sheet;

[0036] (S2) mechanically mixing and stirring the flaky alloy flakes, the low melting point powder containing NdCu, NdAl and NdGa, and the lubricant, and numbering them as 1 to 22 according to the content of each element, as shown in Table 1 below; then placing them in a hydrogen treatment furnace for hydrogen absorption and dehydrogenation treatment, wherein the dehydrogenation temperature is 600° C., and preparing NdFeB powder by jet milling D50, wherein the particle size of the NdFeB powder is 3-5 μm;

[0037] (S3) Orienting and cold isostatically pressing the alloy powder after jet milling to form a blank, vacuum sintering the pressed blank, rapidly cooling it by passing argon gas, and then performing primary tempering and secondary aging, and testing the magnet performance. The specific process is shown in Table 2 below;

[0038] (S4) machining the blank to cut into samples of corresponding sizes, and coating the diffusion source slurry on two surfaces of the sample perpendicular to the C axis;

[0039] (S5) Finally, diffusion and tempering treatments are performed to obtain the NdFeB magnet with the above-mentioned structural characteristics.

[0040] Taking the diffusion source containing Ho or Gd as an example, and the diffusion source not containing Ho or Gd as a comparative example, the various process conditions of the example are shown in Table 3, and correspondingly, the various process conditions of the comparative example are shown in Table 4.

[0041] Table 1 Elements and their contents after alloy flakes, quick-setting flakes and lubricants are mixed

[0042]

[0043] Table 2 Process conditions of each component

[0044]

[0045] Table 3 Diffusion sources and process conditions of various embodiments

[0046]

[0047] Table 4 Diffusion sources and process conditions performance of each comparative example

[0048]

[0049] Based on the above data, by adding NdCu, NdAl, or NdGa phase powder at the grain boundaries in the spinning strip thin film, NdFeB permanent magnets with low melting point grain boundary channels suitable for magnet diffusion are made, which is conducive to diffusion, especially the diffusion of heavy rare earth dysprosium alloy diffusion sources. After diffusion, △Hcj>7.5kOe, the coercive force increases significantly, and the high temperature resistance coefficient of coercive force is significantly better than that of the control example.

[0050] Specifically, each embodiment and comparative example are analyzed as follows:

[0051] In Example 1, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrHoDyCu diffused in Example 1 decreased by 0.23 kGS, Hcj increased by 10.61 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.50%; in Comparative Example 1, the Br of PrDyCu diffused in Example 1 decreased by 0.2 kGS, Hcj increased by 10.21 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.53%; the advantages of Example 1 are obvious.

[0052] In Example 2, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrHoDyCu diffused in Example 2 decreased by 0.26 kGS, Hcj increased by 9.08 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.495%; in Comparative Example 2, the Br of PrDyCu diffused in Example 2 decreased by 0.24 kGS, Hcj increased by 8.78 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.510%; the advantages of Example 2 are obvious.

[0053] In Example 3, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrHoDyCu diffused in Example 3 decreased by 0.24 kGS, Hcj increased by 8.08 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.45%; in Comparative Example 3, the Br of PrDyCu diffused in Example 3 decreased by 0.22 kGS, Hcj increased by 7.58 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.51%; the advantages of Example 3 are obvious.

[0054] In Example 4, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrHoDyCu diffused in Example 4 decreased by 0.26 kGS, Hcj increased by 8.02 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.497%; in Comparative Example 4, the Br of PrDyCu diffused in Example 4 decreased by 0.24 kGS, Hcj increased by 7.52 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.52%; the advantages of Example 4 are obvious.

[0055] In Example 5, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of NdHoDyCu diffused in Example 5 decreased by 0.27 kGS, Hcj increased by 10.11 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.49%; in Comparative Example 5, the Br of NdDyCu diffused in Example 5 decreased by 0.25 kGS, Hcj increased by 9.51 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.51%; the advantages of Example 5 are obvious.

[0056] In Example 6, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of NdHoDyCu diffused in Example 6 decreased by 0.25 kGS, Hcj increased by 8.71 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.492%; in Comparative Example 6, the Br of NdDyCu diffused in Example 6 decreased by 0.23 kGS, Hcj increased by 8.31 kOe, and the high temperature resistance coefficient of the coercive force of the magnet was -0.52%; the advantages of Example 6 are obvious.

[0057] In Example 7, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of NdHoDyCu diffused in Example 7 decreased by 0.24 kGS, Hcj increased by 9.32 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.482%; in Comparative Example 7, the Br of NdDyCu diffused in Example 7 decreased by 0.22 kGS, Hcj increased by 8.82 kOe, and the high temperature resistance coefficient of the coercive force of the magnet was -0.515%; the advantages of Example 7 are obvious.

[0058] In Example 8, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrGdDyCu diffused in Example 8 decreased by 0.26 kGS, Hcj increased by 9.85 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.49%; in Comparative Example 8, the Br of PrDyCu diffused in Example 8 decreased by 0.21 kGS, Hcj increased by 9.35 kOe, and the high temperature resistance coefficient of the coercive force of the magnet was -0.51%; the advantages of Example 8 are obvious.

[0059] Example 9, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrGdDyCu diffused in Example 9 decreased by 0.24 kGS, Hcj increased by 9.75 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.47%; the Br of PrDyCu diffused in Comparative Example 9 decreased by 0.24 kGS, Hcj increased by 9.35 kOe, and the high temperature resistance coefficient of the coercive force of the magnet was -0.5%; the advantages of Example 9 are obvious.

[0060] In Example 10, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrGdDyCu diffused in Example 10 decreases by 0.27 kGS, Hcj increases by 10.88 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C is -0.48%; in Comparative Example 10, the Br of PrDyCu diffused in Example 10 decreases by 0.22 kGS, Hcj increases by 9.88 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C is -0.515%; the advantages of Example 10 are obvious.

[0061] In Example 11, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrGdDyCu diffused in Example 11 decreased by 0.21 kGS, Hcj increased by 8.24 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.49%; in Comparative Example 11, the Br of PrDyCu diffused in Example 11 decreased by 0.21 kGS, Hcj increased by 7.74 kOe, and the high temperature resistance coefficient of the coercive force of the magnet was -0.525%; the advantages of Example 11 are obvious.

[0062] Example 12, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrGdDyCu diffused in Example 12 decreased by 0.27 kGS, Hcj increased by 8.1 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.457%; the Br of PrDyCu diffused in Comparative Example 12 decreased by 0.22 kGS, Hcj increased by 7.6 kOe, and the high temperature resistance coefficient of the coercive force of the magnet was -0.51%; the advantages of Example 12 are obvious.

[0063] Example 13, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrHoDyCuGa diffused in Example 13 decreased by 0.25 kGS, Hcj increased by 7.9 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.46%; the Br of PrDyCuGa diffused in Comparative Example 13 decreased by 0.25 kGS, Hcj increased by 7.6 kOe, and the high temperature resistance coefficient of the coercive force of the magnet was -0.51%; the advantages of Example 13 are obvious.

[0064] Example 14, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrHoDyCuGa diffused in Example 14 decreases by 0.27 kGS, Hcj increases by 8.85 kOe, and the high temperature resistance coefficient of the coercive force of the magnet is -0.47% at 150°C; the Br of PrDyCuGa diffused in Comparative Example 14 decreases by 0.22 kGS, Hcj increases by 8.25 kOe, and the high temperature resistance coefficient of the coercive force of the magnet is -0.52%; the advantages of Example 14 are obvious.

[0065] Example 15, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrHoDyCuGa diffused in Example 15 decreases by 0.27 kGS, Hcj increases by 9.48 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C is -0.46%; the Br of PrDyCuGa diffused in Comparative Example 15 decreases by 0.25 kGS, Hcj increases by 8.98 kOe, and the high temperature resistance coefficient of the coercive force of the magnet is -0.505%; Example 15 has obvious advantages.

[0066] Example 16, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrHoDyCuAl diffused in Example 16 decreased by 0.26 kGS, Hcj increased by 9.44 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.47%; the Br of PrDyCuAl diffused in Comparative Example 16 decreased by 0.2 kGS, Hcj increased by 10.21 kOe, and the high temperature resistance coefficient of the coercive force of the magnet was -0.51%; Example 16 has obvious advantages.

[0067] Example 17, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrHoDyCuAl diffused in Example 17 decreased by 0.2 kGS, Hcj increased by 8.77 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.48%; the Br of PrDyCuAl diffused in Comparative Example 17 decreased by 0.2 kGS, Hcj increased by 10.21 kOe, and the high temperature resistance coefficient of the coercive force of the magnet was -0.52%; the advantages of Example 17 are obvious.

[0068] Example 18, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrHoDyCuAl diffused in Example 18 decreased by 0.28 kGS, Hcj increased by 9.1 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.49%; the Br of PrDyCuAl diffused in Comparative Example 18 decreased by 0.26 kGS, Hcj increased by 8.6 kOe, and the high temperature resistance coefficient of the coercive force of the magnet was -0.505%; the advantages of Example 18 are obvious.

[0069] Example 19, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrGdDyCu diffused in Example 19 decreased by 0.3 kGS, Hcj increased by 9.1 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.47%; the Br of PrDyCu diffused in Comparative Example 19 decreased by 0.2 kGS, Hcj increased by 10.21 kOe, and the high temperature resistance coefficient of the coercive force of the magnet was -0.53%; the advantages of Example 19 are obvious.

[0070] Example 20, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrGdDyCu diffused in Example 20 decreases by 0.2 kGS, Hcj increases by 7.7 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C is -0.475%; the Br of PrDyCu diffused in Comparative Example 20 decreases by 0.2 kGS, Hcj increases by 7.5 kOe, and the high temperature resistance coefficient of the coercive force of the magnet is -0.5%; the advantages of Example 20 are obvious.

[0071] In Example 21, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrGdDyCu diffused in Example 21 decreases by 0.25 kGS, Hcj increases by 9.8 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C is -0.46%; in Comparative Example 21, the Br of PrDyCu diffused in Example 21 decreases by 0.25 kGS, Hcj increases by 9.5 kOe, and the high temperature resistance coefficient of the coercive force of the magnet is -0.51%; the advantages of Example 21 are obvious.

[0072] Example 22, under the same NdFeB magnet and size, the same diffusion temperature and aging temperature and other conditions, compared with before diffusion, the Br of PrGdDyCu diffused in Example 22 decreased by 0.22 kGS, Hcj increased by 7.9 kOe, and the high temperature resistance coefficient of the coercive force of the magnet at 150°C was -0.455%; the Br of PrDyCu diffused in Comparative Example 22 decreased by 0.2 kGS, Hcj increased by 7.5 kOe, and the high temperature resistance coefficient of the coercive force of the magnet was -0.51%; the advantages of Example 22 are obvious.

[0073] From the above, it can be seen that the high temperature resistance of the heavy rare earth alloy diffusion source after diffusion is significantly better than that of the heavy rare earth alloy in the comparative example. Therefore, we will carry out microstructural measurement of the magnet after diffusion of the heavy rare earth alloy. The ZISS electron microscope is mainly used for SEM testing, and the Oxford EDS is used for the composition of the sample magnet elements. Definition: The rare earth shell, i.e., the R shell, refers to the continuity around the grain exceeding 60%, and the transition metal shell refers to the continuity around the grain exceeding 40%. In addition, points a, b, and c are sampling points at different positions, but in the small triangle area with a size of less than 1 μm, the characteristic is a 6:14 phase-type Cu-rich, i.e., the chemical formula of EDS is: Fe 30-51 (NdPr) 45-60 Cu 2-15 Ga 0-5 Co 0-5 or Fe 30-51 (NdPr) 45-60 Dy 2-15 Cu 2-15 Ga 0-5 Co 0-5, where the number next to the element is the weight percentage of the element. The other three points are the sampling points at SEM3, see Figure 1 By diffusing the diffusion source to form the R shell and transition metal shell, the statistical analysis of the three points a, b, and c is as follows:

[0074] Example 1: After the magnet is diffused with PrHoDyCu, the magnet has a rare earth shell of Pr, Dy, Ho and a transition metal shell of Cu, forming a point scan composition of 1: Nd 50-70 Fe 10-30 Pr 10-20 Cu 0-5 ;Spot scan component 2: Nd 50-55 Fe 10-30 Pr 5-15 Dy 5-15 Ho 2-9 Cu 0-5 ;Spot scan component 3: Nd 50-70 Fe 10-35 Pr 10-20 Cu 10-20 Co 0-5 .

[0075] Example 2: After the magnet is diffused with PrHoDyCu, it has a rare earth shell layer of Pr, Dy, Ho and a transition metal shell layer of Cu, forming a point scan composition of 1: Nd 50-65 Fe 10-30 Pr 10-25 Cu 0-5 Ga 0-5 Al 0-3 ;Spot scan component 2: Nd 50-55 Fe 10-30 Pr 5-15 Dy 5-15 Ho 3- 10 Cu 0-5 ;Spot scan component 3: Nd 50-70 Fe 10-35 Pr 10-20 Cu 10-15 Co 0-5 .

[0076] Example 3: After the magnet with the composition PrHoDyCu is diffused, the magnet has a rare earth shell of Pr, Dy, Ho and a transition metal shell of Cu and Al, forming a point scan composition 1: Nd 45-65 Fe 10-35 Pr 10-25 Cu 0-5 Ga 0-5 Al 3-5 ;Spot scan component 2: Nd 45- 55 Fe 10-30Pr 5-20 Dy 5-10 Ho 3-8 Cu 0-5 ;Spot scan component 3: Nd 50-65 Fe 10-35 Pr 10-20 Cu 10-15 Co 0-5 Al 0-5 .

[0077] Example 4: After the magnet with the composition PrHoDyCu is diffused, the magnet has a rare earth shell of Pr, Dy, Ho and a transition metal shell of Cu and Al, forming a point scan composition 1: Nd 45-60 Fe 10-35 Pr 10-20 Cu 3-8 Ga 0-5 Al 3-5 ;Spot scan component 2: Nd 45- 55 Fe 10-30 Pr 5-20 Dy 5-10 Ho 3-6 Cu 2-5 Al 2-10 ;Spot scan component 3: Nd 45-65 Fe 10-30 Pr 10-20 Cu 10-25 Co 0-5 Al 0-5 .

[0078] Example 5: After the magnet with the composition NdHoDyCu is diffused, the magnet has a rare earth shell layer of Nd, Dy, Ho and a transition metal shell layer of Cu, forming a point scan composition 1: Nd 50-65 Pr 10-15 Fe 10-30 Cu 2-6 Go 0-5 ;Spot scan component 2: Nd 45-60 Fe 5-30 Pr 5- 15 Dy 5-15 Ho 3-10 ;Spot scan component 3: Nd 45-60 Pr 10-20 Fe 5-30 Cu 10-20 Co 0-5 .

[0079] Example 6: After the magnet with the composition NdHoDyCu is diffused, the magnet has a rare earth shell layer of Nd, Dy, Ho and a transition metal shell layer of Cu, forming a point scan composition 1: Nd 45-60 Pr10-20 Fe 10-30 Cu 2-5 Ga 0-5 ;Spot scan component 2: Nd 45-60 Fe 5-25 Pr 5- 12 Dy 5-20 Ho 2-9 ;Spot scan component 3: Nd 50-60 Pr 10-15 Fe 5-25 Cu 5-25 Co 0-5 .

[0080] Example 7: After the magnet with the composition NdHoDyCu is diffused, the magnet has a rare earth shell of Nd, Dy, Ho and a transition metal shell of Cu and Al, forming a point scan composition 1: Nd 50-65 Pr 10-15 Fe 10-40 Cu 5-10 Al 0-5 ;Spot scan component 2: Nd 50-60 Fe 5- 30 Pr 5-15 Dy 5-25 Ho 3-12 Al 2-10 ;Spot scan component 3: Nd 50-60 Pr 10-15 Fe 5-25 Cu 5-15 Co 0-5 Al 0-5 .

[0081] Example 8: After the magnet with the composition PrGdDyCu is diffused, the magnet has a rare earth shell layer of Pr, Dy, Gd and a transition metal shell layer of Cu, forming a point scan composition 1: Nd 40-65 Pr 20-35 Fe 10-25 Cu 5-10 ;Spot scan component 2: Nd 25-40 Fe 10-30 Pr 10- 25 Dy 15-20 G 1-7 Co 0-5 Cu 0-5 ;Spot scan component 3: Nd 35-45 Pr 15-35 Fe 5-25 Cu 10-25 Co 0-5 .

[0082] Example 9: After the magnet with the composition PrGdDyCu is diffused, the magnet has a rare earth shell layer of Pr, Dy, Gd and a transition metal shell layer of Cu, forming a point scan composition 1: Nd 40-60 Pr 20-30 Fe 10-30 Cu 3-8 ;Spot scan component 2: Nd 35-45 Fe 10-30 Pr 10-25 Dy 5- 25 G 2-12 Co 0-5 Cu 0-5 ;Spot scan component 3: Nd 35-50 Pr 15-30 Fe 5-25 Cu 5-20 Co 0-5 .

[0083] Example 10: After the magnet with the composition PrGdDyCu is diffused, the magnet has a rare earth shell layer of Pr, Dy, Gd and a transition metal shell layer of Cu, forming a point scan composition 1: Nd 40-60 Pr 20-35 Fe 10-30 Cu 0-5 ;Spot scan component 2: Nd 25-40 Fe 10-30 Pr 10-25 Dy 5- 15 G 2-7 Co 0-5 Cu 0-5 ;Spot scan component 3: Nd 35-45 Pr 15-35 Fe 5-30 Cu 5-20 Co 0-5 .

[0084] Example 11: After the magnet with the composition PrGdDyCu is diffused, the magnet has a rare earth shell layer of Pr, Dy, Gd and a transition metal shell layer of Cu, forming a point scan composition 1: Nd 50-65 Fe 10-25 Pr 10-20 Cu 0-5 Ga 0-5 Al 0-5 ;Spot scan component 2: Nd 45-55 Fe 10- 30 Pr 5-20 Dy 5-20 G 3-9 Cu 0-5 ;Spot scan component 3: Nd 45-70 Fe 10-30Pr 10-25 Cu 10-25 Co 0-5 Ga 0-5 .

[0085] Example 12: After the magnet with the composition PrGdDyCu is diffused, the magnet has a rare earth shell layer of Pr, Dy, Gd and a transition metal shell layer of Cu, forming a point scan composition 1: Nd 50-65 Fe 10-30 Pr 10-25 Cu 0-5 Ga 2-7 Al 3-7 ;Spot scan component 2: Nd 45-55 Fe 10- 30 Pr 5-20 Dy 5-10 G 2-5 Cu 0-5 Ga 0-5 ;Spot scan component 3: Nd 50-65 Fe 10-35 Pr 5-20 Cu 10-20 Co 0-5 Al 0-5 .

[0086] Example 13: After the magnet with the composition PrHoDyCuGa is diffused, the magnet has a rare earth shell of Pr, Dy, Ho and a transition metal shell of Cu and Ga, forming a point scan composition 1: Nd 45-55 Pr 20-25 Fe 15-30 Ga 2-10 Cu 3-5 ;Spot scan component 2: Nd 30-45 Fe 5- 25 Pr 25-30 Dy 5-20 Ho 1-10 Cu 0-5 ;Spot scan component 3: Nd 35-45 Pr 20-35 Fe 10-35 Cu 5-15 Ga 5-10 Co 2-5 .

[0087] Example 14: After the magnet with the composition PrHoDyCuGa is diffused, the magnet has a rare earth shell of Pr, Dy, Ho and a transition metal shell of Cu and Ga, forming a point scan composition 1: Nd 40-55 Pr 20-30 Fe 15-30 Ga 2-10 Cu 3-5;Spot scan component 2: Nd 30-40 Fe 5- 25 Pr 25-30 Dy 5-15 Ho 2-9 Cu 0-5 ;Spot scan component 3: Nd 30-50 Pr 25-30 Fe 10-30 Cu 5-10 Ga 5-10 Co 2-5 .

[0088] Example 15: After the magnet with the composition is diffused into PrHoDyCuGa, the magnet has a rare earth shell of Pr, Dy, Ho and a transition metal shell of Cu and Ga, forming a point scan composition of 1: Nd 40-55 Pr 20-30 Fe 15-25 Ga 5-10 Cu 3-10 ;Spot scan component 2: Nd 30-40 Fe 5- 25 Pr 15-30 Dy 5-20 Ho 3-12 Cu 0-5 ;Spot scan component 3: Nd 30-45 Pr 25-35 Fe 10-30 Cu 5-10 Ga 5-10 Co 2-5 .

[0089] Example 16: After the magnet with the composition is diffused into PrHoDyCuAl, the magnet has a rare earth shell of Pr, Dy, Ho and a transition metal shell of Cu and Al, forming a point scan composition of 1: Nd 45-65 Fe 10-35 Pr 5-15 Cu 5-15 Al 5-10 ; Point scanning component 2Nd 45-65 Fe 5- 30 Pr 5-20 Dy 5-10 Ho 2-11 Cu 5-10 Al 2-10 ;Spot scan component 3: Nd 50-65 Fe 10-20 Pr 10-15 Cu 10-25 Al 0-5 .

[0090] Example 17: After the magnet with the composition PrHoDyCuAl is diffused, the magnet has a rare earth shell of Pr, Dy, Ho and a transition metal shell of Cu and Al, forming a point scan composition 1: Nd 45-55 Fe 10-30 Pr 5-20 Cu 5-10 Al 2-5 ;Spot scan component 2: Nd 45-60 Fe 5- 25 Pr 5-25 Dy 5-15 Ho 2-10 Cu 5-10 Al 3-5 ;Spot scan component 3: Nd 45-60 Fe 10-20 Pr 10-20 Cu 10-20 Ga 0-5 Al 0-5 .

[0091] Example 18: After the magnet with the composition is diffused into PrHoDyCuAl, the magnet has a rare earth shell of Pr, Dy, Ho and a transition metal shell of Cu and Al, forming a point scan composition of 1: Nd 50-65 Fe 10-30 Pr 5-20 Cu 5-10 Al 2-5 ;Spot scan component 3: Nd 45-65 Fe 5- 30 Pr 5-20 Dy 5-15 Ho 1-6 Cu 5-10 Al 5-10 ;Spot scan component 2: Nd 45-60 Fe 10-25 Pr 10-20 Cu 10-20 Ga 0-5 Al 0-5 .

[0092] Example 19: After the magnet with the composition PrGdDyCu is diffused, the magnet has a rare earth shell layer of Pr, Dy, Gd and a transition metal shell layer of Cu, forming a point scan composition 1: Nd 45-55 Fe 5-30 Pr 20-35 Cu 0-5 ;Spot scan component 2: Nd 45-55 Fe 5-10 Pr 10-30 Dy 5- 20 G 2-8 Cu0-5 ;Spot scan component 3: Nd 35-55 Fe 5-30 Pr 10-35 Cu 5-10 Ga 0-5 Co 0-5 .

[0093] Example 20: After the magnet with the composition PrGdDyCu is diffused, the magnet has a rare earth shell layer of Pr, Dy, Gd and a transition metal shell layer of Cu, forming a point scan composition 1: Nd 35-50 Fe 15-40 Pr 15-30 Cu 0-10 Ga 0-3 Al 0-3 ;Spot scan component 2: Nd 40-60 Fe 3- 30 Pr 10-20 G 1-7 Dy 5-25 ;Spot scan component 3: Nd 40-55 Fe 5-35 Pr 15-30 Cu 5-25 Ga 0-5 Co 0-5 .

[0094] Example 21: After the magnet is diffused into PrGdDyCu, the magnet has a rare earth shell of Pr, Dy, Gd and a transition metal shell of Cu, forming a point scan composition of 1: Nd 30-45 Fe 10-30 Pr 20-25 Cu 5-10 Ga 0-5 Co 0-5 Ti 0-5 ;Spot scan component 2: Nd 30- 40 Fe 5-25 Pr 10-15 Dy 10-30 G 2-6 Ho 3-9 ;Spot scan component 3: Nd 35-45 Fe 5-30 Pr 15-30 Cu 5-25 Ga 0-3 Co 0-5 .

[0095] Example 22: After the magnet is diffused into PrGdDyCu, the magnet has a rare earth shell layer of Pr, Dy, Gd and a transition metal shell layer of Cu, forming a point scan composition 1: Nd 25-35 Fe 20-30 Pr20-30 Cu 0-10 Ga 0-5 ;Spot scan component 2: Nd 45-55 Fe 10-20 Pr 20- 30 Dy 5-20 G 4-10 ;Spot scan component 3: Nd 40-55 Fe 10-25 Pr 15-40 Cu 5-20 Ga 0-10 Co 0-5 .

[0096] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A high temperature resistant magnet, characterized in that: The grain boundary structure of the magnet includes a main phase structure, an R shell, a transition metal shell and a triangular region, wherein the R shell is at least one of Nd, Pr, Ho and Gd, the transition metal shell is at least one of Cu, Al and Ga, and the triangular region point scan composition includes component I, component II, and / or component III, wherein: The component I is Nd a Fe b R c M d , R is at least one of Pr, Ce, and La, M is at least three of Al, Cu, Ga, Ti, Co, Mg, Zn, Sn, and Zr, the weight percentage of Nd is a, 30%≤a≤70%, the weight percentage of Fe is b, 5%≤b≤40%, the weight percentage of R is c, 5%≤c≤35%, and the weight percentage of M is d, 0%≤d≤15%; The component II is Nd e Fe f R g H h K i M j , the R is at least one of Pr, Ce, and La, the H is at least one of Dy and Tb, the K is one of Ho and Gd, the M is at least three of Al, Cu, Ga, Ti, Co, Mg, Zn, Sn, and Zr, the weight percentage of Nd is e, 25%≤e≤65%, the weight percentage of Fe is f, 5%≤f≤35%, the weight percentage of R is g, 5%≤g≤30%, the weight percentage of H is h, 5%≤h≤30%, the weight percentage of K is i, 1%≤i≤12%, and the weight percentage of M is j, 0%≤j≤10%; The component III is Nd k Fe l R m D n M o , the R is at least one of Pr, Ce, and La, the D is at least one of Al, Cu, and Ga, the M is at least one of Ti, Co, Mg, Zn, Sn, and Zr, the weight percentage of Nd is k, 30%≤k≤70%, the weight percentage of Fe is l, 5%≤l≤35%, the weight percentage of R is m, 5%≤m≤35%, the weight percentage of D is n, 5%≤n≤25%, and the weight percentage of M is o, 0%≤o≤10%; The method for manufacturing the high temperature resistant magnet comprises the following steps: (S1) Smelting and rapidly solidifying the prepared NdFeB alloy raw material to obtain NdFeB alloy flakes, and mechanically crushing the obtained alloy flakes into 150-400 μm scaly alloy flakes; (S2) mechanically mixing and stirring the flaky alloy flakes, the low melting point powder, and the lubricant, and then placing them in a hydrogen treatment furnace for hydrogen absorption and dehydrogenation treatment, and preparing NdFeB powder by air flow milling, wherein the particle size of the NdFeB powder is 3-5 μm; (S3) pressing the NdFeB powder into a shape and sintering to obtain the desired NdFeB magnet; (S4) machining the sintered NdFeB magnet into a desired shape, and then coating the magnet to form a low-heavy rare earth diffusion source film on a surface perpendicular or parallel to the C-axis, wherein the diffusion source is prepared by atomization powder making, amorphous belt spinning or ingot casting; (S5) finally performing diffusion and tempering treatment to obtain the NdFeB magnet with the above structural characteristics; Wherein, in step (S4), the composition of the low-heavy rare earth diffusion source film is R 1x R 2y H z M 1-x-y-z , wherein R1 is at least one of Nd and Pr, the weight percentage of R1 is x, 15%<x<50%, R2 is at least one of Ho and Gd, the weight percentage of R2 is y, 0%<y≤10%, H is at least one of Tb and Dy, the weight percentage of H is z, 40%≤z≤70%, and M is at least one of Al, Cu, Ga, Ti, Co, Mg, Zn, and Sn, and the weight percentage of M is 1-xyz.

2. The high temperature resistant magnet according to claim 1, characterized in that: The thickness of the magnet is 0.3-6 mm.

3. The high temperature resistant magnet according to claim 1, characterized in that: In step (S1), the raw material components of the NdFeB alloy and their weight percentages are respectively 28%≤R≤30%, 0.8%≤B≤1.2%, 0%≤M≤3%, and the rest is Fe, the R is at least two of Nd, Pr, Ce, La, Tb, Dy, Ho, and Gd, and the M is at least one of Co, Mg, Ti, Zr, Nb, and Mo.

4. The high temperature resistant magnet according to claim 1, characterized in that: In step (S2), the low melting point powder includes at least one of NdCu, NdAl and NdGa, and the weight percentages thereof are 0%≤NdCu≤3%, 0%≤NdAl≤3%, 0%≤NdGa≤3%, and the low melting point powder is 200nm-4μm.

5. The high temperature resistant magnet according to claim 1, characterized in that: In step (S2), the dehydrogenation temperature is 400-600°C.

6. The high temperature resistant magnet according to claim 1, characterized in that: In step (S3), after sintering is completed, argon gas needs to be introduced for cooling, and then primary tempering treatment and secondary aging treatment are performed, wherein the sintering temperature is 980-1060°C, and the sintering time is 6-15h; the primary aging temperature is 850°C, and the primary aging time is 3h; the secondary aging temperature is 450-660°C, and the secondary aging time is 3h.

7. The high temperature resistant magnet according to claim 1, characterized in that: In step (S5), the diffusion temperature of the NdFeB magnet is 850-930°C, the diffusion time is 6-30h, the aging temperature is 420-680°C, and the aging time is 3-10h.

8. The high temperature resistant magnet according to claim 1, characterized in that: The heating rate of the aging temperature of the NdFeB magnet is 1-5°C / min, and the cooling rate is 5-20°C / min.