Method of making a spring core for a mattress or seating product

Through cold coil technology and the use of high-carbon steel alloy wires, local permanent deformation and slack problems of spring core of mattress or seating device are solved, and low or no slack is achieved, which improves mechanical properties and Fatigue resistance and reduce product weight and production costs.

CN113874135BActive Publication Date: 2024-11-12NV BEKAERT SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080037249.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-05-20
Filing Date
2020-03-26
Publication Date
2024-11-12
Estimated Expiration
2040-03-26

AI Technical Summary

Technical Problem

In the prior art, when manufacturing wire spring cores for mattresses or seating devices, there are problems of local permanent deformation and slack, and the heat treatment is unstable, affecting the mechanical properties of the spring.

Method used

Using cold coil technology to manufacture spiral-winded wire springs, use steel alloy wires with high carbon content, and avoid heat treatment by winding at room temperature, ensuring high yield strength and tensile strength ratio of the wire spring, reducing local permanent deformation , and reduce slack through specific fabric structures and connections.

Benefits of technology

The manufacture of wire spring cores with low slack or no slack is achieved, which improves the mechanical properties and fatigue resistance of the spring, reduces product weight, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113874135B_ABST
    Figure CN113874135B_ABST
Patent Text Reader

Abstract

A method for manufacturing a wire spring core for a mattress or seating device, the method comprising the steps of: providing a carrier including a steel wire; repeatedly cold-rolling a steel wire spring using the steel wire taken from the carrier; and connecting a series of wound steel wire springs to each other. The steel wire has a diameter d between 0.8 and 4.5 mm; and has a drawn pearlite microstructure. The steel wire comprises a steel alloy having a carbon content between 0.35 wt% and 0.85 wt%. The steel wire on the carrier has a yield strength R p0.2 (in MPa) and tensile strength R m (in MPa) is higher than 85% (expressed as a percentage).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a steel wire spring core for a mattress or a seating device. The steel wire spring core may be, for example, a pocket spring core, a Bonnell spring core, a LFK spring core or a continuous steel wire spring core. Background Art

[0002] Different types of wire spring cores are known for use in mattresses or seating arrangements such as sofas. Examples of wire spring cores are pocket spring cores, Bonnell spring cores, LFK spring cores, and continuous wire spring cores.

[0003] WO98 / 53933 describes a method and apparatus for forming a length of connected pocketed coil springs for use in mattresses and the like. On this apparatus, steel wire from a supply source is heated to between 232°C and 260°C by an induction heater, hot coiled, cut and cooled to a temperature below where further processing of the springs may cause permanent deformation. Thereafter, the spring is compressed in preparation for its insertion into a space provided by a stretchable fabric from a supply reel. The fabric is folded upon itself to provide the space. The temperature of the spring must also be low enough to contact the fabric without causing burning or other damage. After the compressed spring is inserted into the space, the fabric is ultrasonically welded to produce a separate but connected pocket for each spring. Thereafter, the springs are oriented to allow each spring to expand, thereby producing a length of connected, pocketed coil springs.

[0004] GB2347638A discloses a mattress spring unit, which is manufactured by forming a plurality of spring elements from a coil of steel wire. The rows of spring elements are fixed together by a certain length of spiral wire until a spring unit of the desired size is formed. The formed spring unit is transferred to an oven, where it is tempered. After cooling in air, the spring unit is formed into a coil, or a band is attached to an external spring element. During the tempering process, the overall height of the spring element is reduced.

[0005] WO96 / 05109A1 discloses a method for producing a pocket coil spring for an inner spring structure. The method comprises the following steps: forming a coil spring from a spring wire at a first temperature (wherein the spring wire has an inherent residual stress); tempering the coil spring at a second temperature sufficient to significantly reduce the inherent residual stress in the spring wire of the coil spring; adjusting the temperature of the tempered coil spring to a third temperature sufficient to enable the tempered coil spring to be inserted into a fabric pocket; and inserting the coil spring into the fabric pocket. Summary of the invention

[0006] The present invention is a method for manufacturing a wire spring core for a mattress or a seating device. The method comprises the following steps: providing a carrier comprising a steel wire; repeatedly cold-rolling a steel wire spring using the steel wire taken from the carrier; and connecting a series of wound steel wire springs to each other. Preferably, the steel wire spring is a helically wound steel wire spring. The diameter d of the steel wire is between 0.5 and 4.5 mm. The steel wire comprises a steel alloy having a carbon content between 0.35 wt% (weight percentage) and 0.85 wt%. The steel wire has a drawn pearlite microstructure. The steel wire on the carrier has a yield strength R p0.2 (in MPa) and tensile strength R m A ratio (expressed as a percentage) of the mechanical properties (in MPa) higher than 85%, preferably higher than 87%, even more preferably higher than 90%, even more preferably higher than 92%, even more preferably higher than 93%. m and R p0.2 Defined and tested according to ISO6892-1:2016. Tensile strength R m is the maximum stress in the tensile test (in MPa). Yield strength R p0.2 (in MPa) is the stress at which the tensile curve intersects the line through 0.2% strain and is parallel to the elastic modulus line. Ratio R p0.2 / R m YesR p0.2 The value of (in MPa) divided by R m The value is in MPa and expressed as a percentage.

[0007] Cold coiling refers to coiling at room temperature, which means that the wire is not heated for winding into a wire spring.

[0008] The use of specific wire properties of the wire on the carrier for winding into a wire spring ensures that the wire spring is manufactured at high speed in a reliable and consistent manner with low or no slack when used in a wire spring core in a mattress or seating product. As a result, the local permanent deformation of the spring core is low when used in a mattress or seating product.

[0009] The use of a carrier comprising a steel wire in the present invention makes it unnecessary to carry out special heat treatments of the spring winding machine or of the steel wire spring core before or after the spring winding in order to reduce local permanent deformations of the steel wire spring core for use in mattresses or seating products. (Special) heat treatments of the steel wire on the spring winding machine or of the wound steel springs on the spring winding machine cannot be carried out in a reliable and constant manner, also because of the increased speed of spring winding.

[0010] The use of cold coiling to make springs allows for high speed winding of the springs since the wire does not need to be heated on the spring winding machine.

[0011] The heat resistance of the textile fabric of the pocket spring core (usually a polymer fiber nonwoven fabric) is not sufficient to withstand thermal post-treatment of the pocket spring core to reduce or eliminate relaxation of the wire springs of the pocket spring core.

[0012] The steel wire used in the method of the invention can be produced by drawing a steel wire starting from a steel wire rod. A drawn steel wire having a microstructure of drawn lamellar pearlite generally has a tensile strength R m About 70-75% of R p0.2 By heat treating the steel wire at a temperature between 200 and 300 °C, R p0.2 Value relative to tensile strength R m to the levels specified in the present invention.The heat treatment can be carried out as an in-line process at the end of the wire drawing or off-line in a batch process in a furnace.

[0013] Preferably, the steel alloy contains more than 0.55 wt % C, even more preferably more than 0.6 wt % C. Even more preferably, the steel alloy contains more than 0.7 wt % C. Such embodiments are particularly preferred. Higher carbon contents of the steel alloy provide higher strength (higher R m The steel wire used in the present invention has a high relative R p0.2 The value means that in such an embodiment R p0.2 The absolute value of is even higher. This is advantageous for the invention, since a mattress spring core with even lower spring relaxation is provided.

[0014] Preferably, the elongation at break in the tensile test of the steel wire is higher than 3%.

[0015] Preferably, the steel alloy comprises between 0.1 and 1.4 wt% Si; and preferably less than 0.8 wt% Si; more preferably less than 0.3 wt% Si.

[0016] Optionally, the steel alloy may contain microalloying elements in individual amounts less than 0.5 wt%, even more preferably in individual amounts less than 0.3 wt%.Examples of such microalloying elements are Cr, W, V, Mo, Ti, Nb.

[0017] The steel alloy also contains unavoidable impurities: preferably phosphorus is limited to 0.035 wt%, preferably sulphur is limited to less than 0.035 wt%, preferably aluminium is limited to less than 0.1 wt%; and preferably copper is limited to less than 0.2 wt%.

[0018] In a preferred embodiment, the steel alloy does not contain any of the following microalloying elements Cr, W, V, Mo, Ti, Nb beyond the impurity level. The steel wire also contains unavoidable impurities: preferably, phosphorus is limited to 0.035 wt%, sulfur is limited to less than 0.035 wt%, aluminum is limited to less than 0.1 wt%; copper is limited to less than 0.2 wt%. In a more preferred embodiment, the steel alloy contains Mn and Si; the balance of the composition of the steel alloy is iron.

[0019] Preferably, the steel wire has a diameter ranging between 1.6 mm and 2.5 mm.

[0020] Preferably, the diameter of the steel wire is greater than 1.7 mm.

[0021] Preferably, the diameter of the steel wire is less than 2.3 mm.

[0022] Preferably, the diameter of the steel wire is between 1.7 mm and 2.3 mm.

[0023] In a preferred method, the steel alloy contains between 0.2 and 0.9 wt % Mn and more preferably greater than 0.4 wt % Mn.

[0024] Preferably, the steel alloy contains between 1.3 and 1.6 wt% Si and between 0.6 and 0.9 wt% Cr. More preferably, the steel alloy consists of between 0.35 and 0.85 wt% C, between 1.3 and 1.6 wt% Si, between 0.6 and 0.9 wt% Cr, unavoidable impurities, the balance being iron.

[0025] In a preferred method, the carrier is a bobbin on which the wire is wound. This method is preferred because the use of other carriers can negatively affect the mechanical properties of the wire on the carrier. For example, the use of a star is not preferred because the wire needs to be deformed to place the wire on the star, and this deformation can negatively affect the mechanical properties of the wire associated with the compression spring.

[0026] In a preferred method, the steel alloy of the steel wire contains between 0.02 and 0.06 wt% aluminium.This method is preferred because the presence of aluminium in the steel alloy improves the ductility of the steel wire and thus improves spring winding.

[0027] In a preferred method, more than 120 wire springs are produced per minute.

[0028] Preferably, the tensile strength R of the steel wire m(in MPa) is higher than the value obtained by the formula 2200-390.71*ln(d); d is the diameter of the steel wire in mm, ln(d) is the natural logarithm of the diameter d in mm. More preferably, the diameter of the steel wire in these embodiments is less than 1.7 mm; even more preferably less than 1.6 mm. For the sake of clarity, a calculation example is given: for a steel wire with a diameter of 1.5 mm, the formula 2200-390.72*ln(1.5) gives 2041.6 MPa.

[0029] Preferably, the tensile strength R of the steel wire m (in MPa) is less than the value obtained by the formula 2450-390.71*ln(d); where d is the wire diameter in mm.

[0030] In a preferred method, the steel wire does not include a metal coating. In the absence of a metal coating, the steel wire is provided with oil or wax to prevent corrosion.

[0031] In an alternative preferred method, the steel wire is provided with a metal coating. Preferably, the metal coating comprises or consists of zinc; or comprises at least 84 wt% zinc and optionally aluminium. More preferably, the microstructure of the metal coating comprises a spheroidised aluminium-rich phase. Such a spheroidised aluminium-rich phase is produced in particular when the steel wire is subjected to a heat treatment, whether the heat treatment is carried out in-line (meaning a continuous operation) or in a batch process. It is believed that the spheroidised aluminium-rich phase improves the corrosion resistance of the metal coating; this allows the use of thinner metal coatings while still providing corrosion protection.

[0032] Preferably, when the steel wire comprises a metal coating, the amount of the metal coating is less than 120 g / m 2 , more preferably less than 80g / m 2 , even more preferably less than 60 g / m 2 .

[0033] Viewed from alternative and general aspects, the present invention is directed to reducing the weight of a wire spring core for a mattress or seating arrangement that still exhibits low relaxation characteristics.

[0034] The following formula determines the spring rate R of a steel spring:

[0035] R=Gxd 4 / (8N a xD m 3 )

[0036] in

[0037] d is the wire diameter

[0038] D m is the spring diameter

[0039] N a is the number of turns

[0040] G is the shear modulus.

[0041] Therefore, the stiffness of the spring is proportional to the fourth power of the wire diameter and inversely proportional to the number of turns.

[0042] To reduce weight, the wire diameter can be reduced. In order to keep the spring rate R at the same level for a spring with the same diameter and height, the number of turns N must be reduced. a . The number of turns N a The reduction results in a reduction in the length of the wire in the spring. Thus, the weight saving effect is twofold: finer diameter wire and shorter wire length. However, for the same spring compression, the number of turns N a The steel wire is subjected to a higher degree of torsion. Due to this higher degree of torsion, the steel wire runs the risk of flowing faster in the plastic zone. The steel wire must therefore exhibit a higher yield strength to avoid plastic deformation and guarantee multiple rebounds of the steel spring.

[0043] Steel wire yield strength R expressed in MPa p0.2 Preferably higher than the value obtained by the formula 1870 - 332.10 x ln(d), most preferably higher than the value obtained by the formula 1980 - 351.63 x ln(d), wherein d is the wire diameter in millimeters.

[0044] Pocket spring core made from a linear string of pocket springs

[0045] In a preferred method, connecting a series of coiled wire springs to each other is carried out by inserting the coiled wire springs in a compressed state into a bag made of cloth. A linear string of pocket springs is obtained. In such an embodiment, a pocket spring core is manufactured. More preferably, the pockets of the linear string of pocket springs are formed by a single piece of cloth. Even more preferably, the pockets are closed and a linear string of pocket springs is obtained. The spring core unit for a mattress can be made by connecting (preferably by gluing) a linear string of pocket springs in parallel to each other. The benefit of this preferred method (in which a series of coiled wire springs are connected to each other by inserting the coiled wire springs in a compressed state into a bag made of cloth) is that a lighter wire spring core can be manufactured. In the prior art, the springs are compressed and placed in the bag. The free height of the springs of the pocket spring core of the prior art (this is the height when no compressive load is applied to the spring) is greater than the height of the bag. The corresponding pre-compression of the springs in the bag helps to prevent permanent compression deformation of the mattress made of the spring core. In the present invention, the spring is less susceptible to permanent compression set, less pre-compression of the spring in the pocket is required, and the free height of the spring can be lower, thereby making the pocket spring core lighter.

[0046] Pocket spring cores made directly from a two-dimensional matrix of pocket springs - more specifically so-called "micro-coil" spring cores or "nano-coil" spring cores

[0047] In a preferred method, a two-dimensional matrix of wound wire springs is provided. The wound wire springs are enclosed in a bag. The plane of the two-dimensional matrix is ​​perpendicular to the longitudinal axis of the wound wire springs. The bag is formed by a first fabric layer on top of the wound wire springs, a second fabric layer below the wound wire springs, and a seam between the first fabric layer and the second fabric layer. The seam surrounds the wound wire springs. Preferably, the first fabric layer and the second fabric layer are fabrics made of thermoplastic fibers; more preferably, nonwoven fabrics made of thermoplastic fibers; such as spunbond nonwoven fabrics. Preferably, the weld is a welded seam, thermally bonding the thermoplastic first fabric layer to the thermoplastic second fabric layer.

[0048] Preferably, the height of such a wire spring core is less than 6 cm, more preferably less than 5 cm, even more preferably less than 4 cm.

[0049] In the preferred method, the wire diameter is preferably less than 1 mm, such as 0.8 mm.

[0050] This method is particularly interesting when manufacturing a wire spring core of low height (e.g., height less than 5 cm). In this preferred method, a spring core with low height but no slack or low slack can be manufactured.

[0051] In a more preferred embodiment of the method, more than 200 springs are produced per minute.

[0052] The advantage of these preferred method embodiments is that a spring core of small height can be manufactured, which can be used as a comfort layer of a mattress, on top of another spring core (e.g., a pocket spring core). Such a comfort layer manufactured according to the invention is breathable and elastic in multiple directions, with limited or even no relaxation. This means that when the spring core is used, the spring will experience limited or no permanent deformation. The high-speed manufacturing of the wire springs and the specific fabric selection (most of the time polymer fiber nonwovens) make it almost impossible to heat the spring manufacturing machine and / or the wire or wound wire spring on the spring core manufacturing machine.

[0053] In an embodiment, the first fabric layer and the second fabric layer may be two different fabrics.

[0054] In another embodiment, the first fabric layer and the second fabric layer may be one folded fabric.

[0055] BONNELL or LFK type spring core

[0056] The preferred method comprises the step of connecting the wound springs to each other by tightening a wire through the wound springs. More preferably, the springs are wound individually and provided to the operation as discrete components, wherein the wire is tightened through the wound springs to connect them to each other. In this way, a "Bonell" type or "LFK" type spring core can be produced.

[0057] In a preferred embodiment, the wound spring has knots provided by a wire at both ends thereof, from which the spring is wound, in which the wire is knotted itself. More preferably, the wire is passed through the wound springs and tightened to connect the wound springs to each other. In this way, a Bonell type spring core can be manufactured.

[0058] In a preferred embodiment, the wound spring does not have a knot provided by the wire at either end, from which the spring is wound. More preferably, the wire is tightened through the wound springs to connect the wound springs to each other. In this way, a LFK type spring core can be manufactured.

[0059] Continuous wire spring core

[0060] In a preferred embodiment, a plurality of wire springs are wound without cutting the wires so that the wires extend continuously through the plurality of wire springs in the spring core. In this way, a continuous coil type spring core for a mattress or seating device is manufactured. Optionally, additional lacing wires may be used to improve the interconnection between the wire springs. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 The tensile stress-strain curve of the steel wire is shown.

[0062] Figure 2 A pocket spring mattress core that can be made using the method of the present invention is shown.

[0063] Figure 3 An example of a Bonnell spring is shown.

[0064] Figure 4 A Bonnell spring core for a mattress that can be made using the method of the present invention is shown.

[0065] Figure 5 An example of a LFK spring is shown.

[0066] Figure 6 An LFK spring core for a mattress that can be manufactured using the method of the present invention is shown.

[0067] Figure 7 A continuous spring that can be manufactured using the method of the present invention is shown.

[0068] Figure 8Another type of wire spring core is shown in which the wire spring is enclosed in a fabric bag. DETAILED DESCRIPTION

[0069] Figure 1 Information is provided on the way in which the mechanical properties of steel wire are described in this document. The mechanical properties are described and tested in accordance with ISO 6892-1:2016, which is titled “Metallic materials – Tensile tests – Part 1: Test methods at room temperature”. Figure 1 The stress-strain curve of a steel wire in a uniaxial tensile test is schematically shown. On the X-axis, the strain is provided. The vertical (Y) axis provides the tensile stress (in MPa). The elongation at break is given by A t Indicates tensile strength R m is the maximum stress. Yield strength R p0.2 It is the stress when the tensile curve intersects the line through 0.2% strain and is parallel to the elastic modulus line.

[0070] Figure 2 A pocket spring mattress core that can be made using the method of the present invention is shown. Figure 3 An example of a Bonnell spring is shown. Figure 4 A Bonnell spring core for a mattress that can be made using the method of the present invention is shown. Figure 5 An LFK spring is shown. Figure 6 An LFK spring core for a mattress that can be manufactured using the method of the present invention is shown. Figure 7 It is shown that a continuous spring for a mattress core can be manufactured using the method of the present invention.

[0071] Figure 8 Another type of wire spring core is shown, in which the wire spring is encapsulated in a fabric; and can be manufactured with the method according to the invention. The wire springs are located in a two-dimensional matrix. A nonwoven fabric (or nonwoven fabric, nonwoven fabric) is provided on top and below the two-dimensional array of wire springs. The bag is formed by a first nonwoven fabric on top of the wound wire springs, a second nonwoven fabric below the wound wire springs, and a seam between the first nonwoven fabric and the second nonwoven fabric. The seam surrounds the wound wire spring. The seam can be produced by a heat weld (e.g. produced by an ultrasonic welding device) that bonds two nonwoven fabrics to each other.

[0072] The first series of experiments was related to pocket spring cores for mattresses. A steel wire with a diameter of 2 mm was used, the wire being made of a steel alloy consisting of: between 0.71 and 0.75 wt% carbon, between 0.6 and 0.9 wt% manganese, up to 0.03 wt% aluminum; unavoidable impurities, the remainder being iron. The wire with a diameter of 2 mm was drawn starting from a wire rod with a diameter of 5.5 mm. The tensile properties of the wire have been tested according to ISO 6892-1:2016: Tensile strength R m =2018MPa, R p0.2 =1507MPa (meaning R p0.2 is the tensile strength R m = 75% of the total heat treatment), and elongation at break = 3%. The steel wire bobbin has been treated in a furnace at 300°C during 2 hours. After this heat treatment, the tensile properties were tested again: tensile strength R m =2052MPa, R p0.2 =1823MPa (meaning R p0.2 is the tensile strength R m 89%), and the elongation at break was 7%.

[0073] The helically wound springs were made according to the pocket spring design from steel wire treated in an oven as described in the previous paragraph. The spring height was 210 mm, the spring diameter was 80 mm and the spring had 7 turns. The springs were tested according to the Brazilian standard ABNT 15413-1:2013, entitled "Spring mattresses and foundations - Part 1: Requirements and test methods". This part of ABNT NBR 15413 establishes the requirements and test methods for spring mattresses and foundations. The test method described in this standard consists in compressing a single spring by hand to full compression during 10 seconds. After removing the load and letting the spring recover, a new compression cycle is performed during 10 seconds to full compression by hand. After removing the load and letting the spring recover, a new compression cycle is performed during 60 seconds to full compression by hand. After removing the load, the height loss of the spring compared to its initial height is measured and expressed as a percentage of the initial height of the spring. According to this Brazilian standard, a maximum height loss of 8% is acceptable. This test performed on the helically wound springs with heat-treated steel wire showed no height loss.

[0074] The fatigue resistance of the spring core produced according to the method of the invention has been tested: the results show that the helical spring produced from the heat-treated steel wire has a high fatigue resistance.

[0075] The second series of tests is related to the steel wire used to make the Bonnell spring core. The steel wire with a diameter of 2.2 mm is made from a steel alloy consisting of: between 0.55 and 0.59 wt% carbon and between 0.6 and 0.9 wt% manganese, a maximum of 0.03 wt% aluminium; and unavoidable impurities, the balance being iron. The steel wire is drawn to a diameter of 2.2 mm starting from a wire rod with a diameter of 5.5 mm. The tensile properties of the steel wire are tested according to ISO 6892-1:2016: Tensile strength R m =1415MPa, R p0.2 =1050MPa (meaning R p0.2 is the tensile strength R m =74.2% of the total weight of the steel wire), and elongation at break = 3.25%. The steel wire bobbins were treated in a furnace at different temperatures during one hour. After this heat treatment, the tensile properties were tested again and the results are given in Table I. The first column of Table I indicates the temperature at which the heat treatment was carried out in the furnace.

[0076]

[0077] Table I - Tensile test results of steel wire from heat treated bobbins

[0078] The following table illustrates how the present invention may be applied to achieve weight reduction in a wire spring core for a mattress or seating arrangement.

[0079]

[0080]

[0081] Table 2

[0082] According to the results in Table II, a weight reduction of 39% was achieved.

Claims

1. A method for manufacturing a wire spring core for a mattress or seating device, comprising the following steps - providing a carrier comprising a steel wire; - repeatedly cold-rolling a wire spring from a wire taken from a load-bearing member, and -Connecting a series of coiled wire springs to each other; in, The diameter d of the steel wire is between 0.5 and 4.5 mm; wherein the steel wire comprises a steel alloy, wherein the carbon content of the steel alloy is between 0.35wt% and 0.85wt%; Among them, the steel wire has a drawn pearlite microstructure; The steel wire on the load-bearing part has a yield strength R in MPa. p0.2 and the tensile strength R in MPa m A ratio expressed as a percentage above 85%.

2. The method according to claim 1, in, The carbon content of the steel alloy is above 0.6 wt%.

3. The method according to claim 1, in, The carrier is a bobbin on which the wire is wound.

4. The method according to claim 1, in, The steel alloy comprises between 1.3 and 1.6 wt % Si; and between 0.6 and 0.9 wt % Cr.

5. The method according to claim 4, in, The steel alloy consists of between 0.35 and 0.85 wt% C, between 1.3 and 1.6 wt% Si, between 0.6 and 0.9 wt% Cr, unavoidable impurities, the balance being iron.

6. The method according to claim 1, in, The steel alloy contains between 0.02 and 0.06 wt % aluminium.

7. The method according to claim 1, in, More than 120 wire springs are manufactured per minute.

8. The method according to claim 1, in, Tensile strength R of steel wire in MPa m Higher than the value obtained by the formula 2200-390.71*ln(d); where d is the wire diameter in mm.

9. The method according to claim 1, in, The wire does not include the metal coating.

10. The method according to claim 1, in, The steel wire is provided with a metal coating, wherein the microstructure of the metal coating comprises a spheroidized aluminum-rich phase.

11. The method according to any one of the preceding claims 1 to 10, in, Connecting a series of coiled wire springs to each other is performed by inserting the coiled wire springs in a compressed state into a bag made of cloth, Therein, a linear string of pocket springs is obtained.

12. The method according to claim 11, in, The bags are formed from a single piece of cloth, and wherein the bags are closed and linearly joined to each other by welding bonding.

13. The method according to any one of the preceding claims 1 to 10, in, providing a two-dimensional matrix of coiled wire springs, wherein a plane of the two-dimensional matrix is ​​perpendicular to a longitudinal axis of the coiled wire springs; wherein the coiled wire springs are enclosed in a bag; Therein, the pocket is formed by a first fabric layer on top of a coiled wire spring, a second fabric layer below the coiled wire spring, and a seam between the first and second fabric layers, wherein the seam surrounds the coiled wire spring.

14. A method according to any one of the preceding claims 1 to 10, comprising the step of connecting the wound springs to each other by tightening a wire through the wound springs.

15. The method according to any one of the preceding claims 1 to 10, in, The plurality of wire springs are coiled without cutting the wire so that the wire extends continuously through the plurality of wire springs in the spring core.