12.9 grade non-quenched and tempered hot-rolled high carbon cold heading steel wire rod and its manufacturing method

Through the design of high C-Si-Mn-low Cr-low Mo composition and online molten salt isothermal phase change control, the microstructure is mainly tempered pearlite, which solves the problem of non-temperature cooling of high-carbon steel strips at level 12.9 The difficulty of taking into account both strength and plasticity in the upset steel reduces the cost of materials and cracking risks, and achieves efficient manufacturing of 12.9-level non-temperature fasteners.

CN118497633BActive Publication Date: 2024-11-15JIANGSU YONGGANG GROUP CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410969478.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-15
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

It is difficult for existing high-carbon steel strips to achieve high strength and high plasticity in 12.9-level non-tempered cold heading steel, and the material cost is high, and there is a risk of drawing and breaking wires and cold heading cracking.

Method used

Using high C-Si-Mn-low Cr-low Mo composition design, combined with online molten salt isothermal phase change control and roller slow cooling technology, the microstructure is mainly tempered pearlite, containing a small amount of ferrite and fused pearlite to avoid the formation of mesh carbides, reduce material costs and improve strong plastic properties.

Benefits of technology

It has achieved efficient green manufacturing of 12.9-level non-temperature fasteners, reducing the risks of drawing and breaking wires and cold heading cracking, reducing material costs, matching strength with plasticity, and good market application prospects and industrial adaptability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118497633B_ABST
    Figure CN118497633B_ABST
Patent Text Reader

Abstract

The invention relates to a 12.9-grade non-quenched and tempered hot-rolled high-carbon cold-heading steel wire rod and a manufacturing method thereof. The wire rod is produced by controlled rolling and controlled cooling with high C-Si-Mn-Cr-Mo composition. After the wire rod is spun into a wire rod at a spinning temperature of ≥940°C, the wire rod is subjected to online molten salt isothermal phase transformation control, so that the wire rod is cooled to a pearlite phase region at a cooling rate of ≥38°C / s for isothermal phase transformation, and simultaneously promotes high-temperature softening of pearlite formed by phase transformation, promotes melting and transformation of pearlite lamellae into fused pearlite, and finally is slowly cooled by a roller to form a cold-heading steel wire rod with a microstructure including tempered pearlite with a volume percentage of ≥93%, and the rest being ferrite and fused pearlite, so that the wire rod structure is regulated, and a tensile strength of 1165-1215MPa, a cross-sectional shrinkage of 53%-58%, a same-circle mechanical fluctuation of ≤28MPa, and a network carbide of level 0 is achieved. The wire rod is used for non-quenched and tempered, efficient and green manufacturing of 12.9-grade fasteners.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot-rolled cold-heading steel wire rods, and in particular relates to a 12.9-grade non-quenched and tempered hot-rolled high-carbon cold-heading steel wire rod and a manufacturing method thereof. Background Art

[0002] Non-quenched and tempered cold heading steel has attracted much attention because it does not require spheroidizing annealing and tempering processes, which can greatly improve production efficiency and reduce energy consumption in the production of fasteners such as bolts. At the same time, since it saves the spheroidizing annealing process used to improve the cold processing deformation ability of hot-rolled wire rods and reduce the tendency to crack, as well as the tempering process used to improve the comprehensive mechanical properties of hot-rolled wire rods after drawing to obtain the final performance grade, higher requirements are put forward for the strength and plasticity of hot-rolled wire rods as raw materials. At present, non-quenched and tempered cold heading steel is concentrated in 8.8~10.9 grade fasteners. It is often obtained by adding appropriate amounts of micro-alloying elements such as Ti, Nb, and V to carbon alloys, and combining controlled rolling and controlled cooling technology to obtain hot-rolled wire rods. The development of non-quenched and tempered cold heading steel wire rods with higher strength grades of 12.9 is difficult, and there are few reports or they are limited to the research and development of low and medium carbon steels. For example, patent CN116162853A discloses a 12.9-grade non-quenched and tempered long-rod bolt steel and its preparation method, which adopts a low C-Mn-Cr-V-Nb-Al composition design, combined with low-temperature spinning and low-speed cooling processes, to obtain a lower bainite structure after air cooling, and achieves a hot-rolled tensile strength of 886~1020MPa, and a cross-sectional shrinkage of 46.6~53.5%. However, on the one hand, high Mn, V, Nb, etc. make the material cost high, and on the other hand, the strength and plasticity are insufficient, which will lead to the fastener processing requiring large drawing deformation and cold deformation strengthening strength increase of more than 180MPa to achieve With the increase of strength grade, the risk of cold heading cracking is extremely high; although the 12.9 grade quenching-free high hardenability hot-rolled complex phase cold heading steel wire rod and its manufacturing method disclosed in patent CN118186310A adopts a medium C-Si-Mn-Cr-Mo composition design, combined with online molten salt strong quenching and strong tempering after spinning, to obtain the structure of tempered martensite, tempered bainite and quasi-spheroidized carbide, to achieve a tensile strength of 1066~1120MPa, a cross-sectional shrinkage rate of 56%~62%, which can reduce material costs and improve the strength performance of wire rods, but the material cost is not low enough, and two salt bath processes are required, and the process is not simplified enough.

[0003] C element is the most basic and cheap strengthening element in steel, which is beneficial to reducing the cost of steel grades and improving the strength and hardness of steel. However, the high carbon steel wire rods in the prior art are mainly used in the fields of high-strength bridge cables, cords, stranded wires, etc., and it is difficult for them to meet the technical difficulties and causes of 12.9 grade non-quenched and tempered cold heading applications:

[0004] (1) The increase in carbon content increases the risk of carbide precipitation along the grain boundaries during cooling. The existing high-carbon steel wire rod mainly reduces the network carbon problem during wire drawing or cooling by appropriately increasing the wire drawing temperature and the air volume of the Stelmor air cooling line after wire drawing. However, the maximum cooling rate of air cooling is limited, and the wire rod still spends a long time in the precipitation temperature range of secondary cementite, which makes it difficult to effectively eliminate the network carbides. The network carbides will increase the unevenness of the chemical composition and the structural stress in the steel, especially causing the impact toughness of the steel to drop sharply. The method of eliminating network carbon by heat treatment after unwinding the wire rod is contrary to the original intention of annealing-free quenching and tempering, resulting in wire breakage during drawing or cracking during cold heading. Continuing to increase the wire drawing temperature will not only aggravate the network carbon problem during air cooling, but also increase the cooling rate of air cooling, which will increase the temperature difference of the wire rod due to the increase in the difference in air volume between the windward side and the leeward side of the wire rod, thereby increasing the phase change unevenness and the fluctuation of the mechanical properties of the final wire rod, which is not conducive to drawing and cold heading.

[0005] (2) The existing high carbon steel wire rod also suppresses the precipitation of the proeutectoid phase by appropriately lowering the spinning temperature and then using forced air cooling to form a sorbite structure in a lower phase transformation temperature zone to increase the sorbite rate of the wire rod, thereby increasing the tensile strength of the material. Even if the heat preservation treatment process after air cooling is adopted, the time that the wire rod passes through the sorbite phase transformation temperature zone is short. After the phase transformation incubation, the wire rod is in a low temperature state that cannot be softened during the continuous cooling process, and a certain amount of material plasticity is lost. The cross-sectional shrinkage rate of the obtained wire rod is about 20%~35%, while Lowering the proportion of troostite in the organization and increasing the proportion of ferrite will seriously damage the strength of the wire rod. Although adding strong hardenability components can improve the strength of the wire rod to a certain extent, it also increases the material cost, and will also bring about the problem of alloy non-homogenization at low wire drawing temperature, and increase the risk of producing martensite or bainite brittle organization that is not conducive to drawing, which will make it difficult to balance the final strength and plasticity, cracking during drawing or cold heading, or unable to achieve the ultra-high strength performance level of 12.9 through simple aging treatment without annealing and tempering. Summary of the invention

[0006] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a 12.9-grade non-quenched and tempered hot-rolled high-carbon cold-heading steel wire rod and a manufacturing method thereof. The high-carbon chemical composition design can be used to effectively reduce material costs and simplify manufacturing methods, effectively reduce the level of network carbides, and achieve regulation of wire rod structure and strength and plasticity properties. It is used for non-quenched and tempered, efficient and green manufacturing of 12.9-grade fasteners, and can reduce the risks of wire breakage during drawing and cracking during cold heading.

[0007] The technical solution adopted by the present invention to solve its technical problem is:

[0008] A 12.9-grade non-quenched and tempered hot-rolled high-carbon cold-heading steel wire rod, the chemical composition and mass percentage of the cold-heading steel wire rod include C: 0.72%-0.76%, Si: 0.20%-0.35%, Mn: 0.60%-0.90%, Cr: 0.34%-0.42%, Mo: 0.10%-0.30%, P≤0.015%, S≤0.015%, and the rest is Fe and unavoidable impurities; its microstructure includes tempered pearlite with a volume percentage of ≥93%, and the rest is ferrite and fused pearlite.

[0009] The design basis of the chemical composition and mass percentage of the above-mentioned cold heading steel wire rod includes:

[0010] (1) Carbon: The carbon element is the main strengthening element of the present invention and is more economical in steel than other elements. It exists in the form of interstitial solid solution or carbide. A high carbon content is conducive to solid solution strengthening and precipitation strengthening, providing matrix strength and hardness of the material, but at the same time increases the risk of decarburization and the risk of cementite being distributed in a network along the pearlite grain boundary. Therefore, in order to enable the cold heading steel wire rod to achieve the final performance level of 12.9 grade fasteners through a short-time aging treatment under the annealing and tempering-free process, while taking into account the cold deformation performance of the cold heading steel wire rod, the mass percentage of C is controlled to be 0.72%~0.76%.

[0011] (2) Silicon: Si is a good deoxidizing element during steel smelting. It can dissolve in ferrite and austenite to increase the hardness and strength of steel. However, excessive silicon will easily produce bainite structure due to the improvement of steel hardenability, reduce the plasticity and impact toughness of steel, and make cold heading more difficult. Therefore, the mass percentage of Si is controlled to be 0.20%~0.35%.

[0012] (3) Manganese: Mn is a good deoxidizer and desulfurizer in the steelmaking process and has a solid solution strengthening effect. However, while improving the strength of steel, too high Mn content will aggravate the segregation during the solidification process of the steel billet, resulting in poor uniformity of the steel. Because it causes the C curve to shift to the right, it improves the hardenability of the steel and is prone to produce bainite structure, which is not conducive to structure control. In addition, too high Mn content will also increase material costs. Therefore, the mass percentage of Mn is controlled to be 0.60%~0.90%.

[0013] (4) Chromium: Cr is a medium-strong carbide-forming element that can significantly strengthen the matrix. However, too high a Cr content will increase the brittle phase transition temperature of the steel, making the steel have a higher hardenability and increasing the risk of producing low-temperature structures, which is not conducive to structural control and reduces the plasticity and toughness of the material. There is also a risk of coarse grains under long-term high temperatures, which is not conducive to the strengthening effect of Cr. Therefore, the mass percentage of Cr is controlled to be 0.34%~0.42%.

[0014] (5) Molybdenum: The Mo element helps to inhibit the deterioration of plasticity due to the coarsening of precipitated phases such as Cr, which is beneficial to the strengthening effect of Cr and improves the strength of the material. However, the cost of Mo element alloys is high. Too high Mo content will increase the material cost and the hardenability of steel, and there is a risk of decarburization and the appearance of brittle phases, resulting in reduced cold deformability. Therefore, the mass percentage of Mo is controlled to be 0.10%~0.30%.

[0015] (6) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.

[0016] The cold heading steel wire rod adopts a high C-Si-Mn-low Cr-low Mo composition design, does not add expensive microalloying elements such as Ti, Nb, and V, and replaces the addition of high Mn, Cr, Mo and other alloy components with C, a more economical strengthening element, so that the material cost is further reduced. At the same time, compared with the existing high carbon steel wire rod with a high troostite content, the cold heading steel wire rod microstructure has a higher proportion of tempered pearlite. Since the interlamellar spacing of pearlite is larger than that of troostite and the plasticity is better, after being transformed into tempered pearlite and fused pearlite, the tissue stress and dislocation density can be effectively reduced, and the wire rod structure is further softened, so that The cold heading steel wire rod has significantly improved plasticity and can delay the formation and expansion of cracks, making up for the adverse effects of high carbon on the hardness and cold heading performance of the wire rod. Compared with the wire rod that optimizes plasticity by increasing the proportion of ferrite after adding microalloying components, the cold heading steel wire rod can retain the characteristic that the strength of pearlite is higher than that of ferrite with a higher proportion of tempered pearlite without adding microalloying elements or reducing the content of alloy components, and maintain a certain matrix strength with high carbon components, thereby achieving the strength-plasticity match of the cold heading steel wire rod, breaking the limitation of low-cost high-carbon components on the manufacture of cold heading steel wire rod, and can be used for the efficient and green production of 12.9 grade non-quenched and tempered fasteners.

[0017] Preferably, the lamellar spacing of the tempered pearlite is 150-185 nm. A relatively fine lamellar spacing can improve the matrix strength, is beneficial to the melting of the pearlite, and avoids the disadvantage of too fine lamellar spacing on the plasticity of the cold heading steel wire rod.

[0018] Preferably, the volume percentage of the ferrite is 1% to 5%. The lower the proportion of ferrite, the finer the spacing between tempered pearlite lamellae, the higher the strength of the cold heading steel wire rod and the lower the plasticity. The proportion of ferrite and fused pearlite can be further controlled to optimize the strength and plasticity of the wire rod.

[0019] Preferably, the network carbide of the cold heading steel wire rod is level 0, which effectively reduces the level of the network carbide and is beneficial to reducing the risk of wire breakage during drawing and cracking during cold heading.

[0020] Preferably, the diameter of the cold heading steel wire rod is 10.0~22.0mm, the tensile strength is 1165~1215MPa, the cross-sectional shrinkage rate is 53%~58%, and the mechanical fluctuation in the same circle is ≤28MPa. It has high strength and plasticity matching, small mechanical fluctuation in the same circle, and can manufacture 12.9 grade fasteners under non-quenching and tempering process, effectively reducing the risk of wire breakage during drawing and cracking during cold heading.

[0021] The manufacturing method of the above-mentioned 12.9 grade non-quenched and tempered hot-rolled high carbon cold heading steel wire rod comprises: producing a wire rod by controlled rolling and controlled cooling according to the chemical composition of the 12.9 grade non-quenched and tempered hot-rolled high carbon cold heading steel wire rod, after the wire rod is spun into a wire rod at a spinning temperature of ≥940°C, it is subjected to online molten salt isothermal phase transformation control, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥38°C / s for isothermal phase transformation, and at the same time, the pearlite formed by the phase transformation is promoted to undergo high-temperature softening, and the pearlite lamellae are promoted to be melted and transformed into fused pearlite, and finally, it is slowly cooled by a roller to produce a cold heading steel wire rod whose microstructure includes tempered pearlite with a volume percentage of ≥93%, and the rest is ferrite and fused pearlite.

[0022] The above manufacturing method adopts high C chemical composition design and combines online molten salt isothermal phase transformation control after high-temperature spinning to avoid the precipitation of network carbides from high-carbon wire rods during the spinning stage. At the same time, the high heat exchange characteristics of molten salt are utilized to control the wire rod to quickly enter the pearlite phase region for isothermal phase transformation as much as possible, and the temperature range in which carbides precipitate from austenite along grain boundaries and austenite transforms into ferrite can be quickly skipped. On the one hand, there is no time to form a coarse network that is harmful to the performance of the wire rod, thereby effectively eliminating the network carbides of the steel and avoiding the adverse effects of the network carbides on the uniformity of composition and the plasticity and toughness. During the process, the wire rod is cooled evenly and the temperature difference is small, which can reduce the fluctuation of mechanical properties and is beneficial to the uniform transformation of the organization. On the other hand, it can reduce the pro-eutectoid in the organization. The precipitation of ferrite allows the high-temperature austenite structure in the wire rod to be transformed into pearlite structure as much as possible, providing matrix strength and avoiding excessive undercooling that makes the pearlite sheet spacing small, which is not conducive to melting and plasticity improvement. Compared with the low-temperature state after continuous cooling and incubation of troostite structure after air cooling, the online molten salt can maintain the wire rod in the pearlite phase region for a longer period of high-temperature isothermal state, so that the newly formed pearlite of diffusion-type phase transformation can obtain a reduction in organizational stress and dislocation density at high temperature, and at the same time promote the melting of pearlite lamellae to form melting pearlite. Combined with the inhibitory effect of Mo on the coarsening of precipitated phases such as Cr, the high-temperature softening and tempering state are regulated to avoid insufficient organizational transformation to form abnormal bainite organization, so as to ensure the strength and plasticity matching of the wire rod.

[0023] The above manufacturing method only requires one molten salt control, and the process and control are further simplified. Finally, it is slowly cooled by rollers and cooled relatively quickly. The high temperature state of the wire rod after leaving the molten salt can be further utilized through slow cooling, and the softening and melting effects of the later stage of the online molten salt isothermal phase transformation can be continued, thereby further improving the plasticity of the wire rod, and obtaining a mixed structure composed mainly of tempered pearlite structure and a small amount of ferrite and fused pearlite, thereby realizing the final structure control and strength-plasticity matching of cold heading steel.

[0024] Preferably, when heating the steel billet before controlled rolling and controlled cooling, the steel billet soaking temperature is controlled to be ≤1140°C and the soaking time is controlled to be ≤2h, which can promote component homogenization and avoid decarburization caused by excessive soaking temperature and soaking time.

[0025] Preferably, during the controlled rolling and controlled cooling, the initial rolling temperature is controlled to be 1075~1125℃, and the initial rolling reduction is 40%~50%. Selecting a high initial rolling temperature can promote the homogenization of the alloy of the high carbon component system, and at the same time, a larger initial rolling reduction is used to prepare for subsequent rolling to obtain uniformly refined grains.

[0026] Preferably, during the controlled rolling and controlled cooling, the final rolling temperature is controlled to be ≥960°C, and the final rolling reduction is 38%~46%. A higher final rolling temperature can reduce the wear and loss of the rolling mill, promote the alloy homogenization of the high carbon component system and the uniformity of the original structure, and can completely recrystallize. A larger final rolling reduction can be used to refine the grains, increase the grain boundary area and produce deformation bands in the grains, which is beneficial to reducing the level of network carbides. The preferred final rolling temperature is 960~1030°C and the wire drawing temperature is 940~1000°C, which can reduce the tendency of grain growth and further increase the pearlite phase deformation nucleation rate and driving energy, and then use the online molten salt isothermal phase transformation after wire drawing to control rapid cooling, so that the grains do not have time to grow and continue the refinement effect.

[0027] Preferably, during the online molten salt isothermal phase transformation control, the molten salt isothermal temperature is controlled to be 510~560℃, and the processing time is 400~700s. The higher the molten salt isothermal temperature, the larger the lamellar spacing of the tempered pearlite and the higher the ferrite content in the organization, which is beneficial to the melting of the pearlite lamellae, and the strength of the cold heading steel wire rod decreases and the plasticity increases. However, too high a molten salt isothermal temperature will lead to too high a ferrite content in the organization, which is detrimental to the strength of the matrix. Conversely, the lower the molten salt isothermal temperature, the smaller the lamellar spacing of the tempered pearlite and the lower the ferrite content in the organization, the strength of the cold heading steel wire rod increases and the plasticity decreases. However, too low a molten salt isothermal temperature will lead to the generation of bainite or even martensite abnormal organizations in the organization, which seriously affects the plasticity of the wire rod.

[0028] The longer the treatment time, the better the tempering and softening effect of pearlite, the more and more uniform the melted pearlite structure, the lower the strength and the higher the plasticity of the cold heading steel wire rod. However, too long a treatment time will accelerate the precipitation and coarsening of Cr, significantly reducing the plasticity of the wire rod. On the contrary, the shorter the treatment time, the weaker the high-temperature softening effect of the pearlite structure, which is not conducive to the melting of the pearlite lamellae, causing the strength of the cold heading steel wire rod to increase and the plasticity to decrease. Further shortening the treatment time is not conducive to the full transformation of the structure to inhibit the subsequent occurrence of bainite abnormal structure. Therefore, the molten salt isothermal temperature and treatment time can be further controlled to adjust the proportion and spacing of tempered pearlite lamellae, the softening effect of the structure and the uniformity of the structure, so that the strength and plasticity of the cold heading steel wire rod match.

[0029] Preferably, since the temperature difference of the wire rod from the spinning temperature to the isothermal temperature of the pearlite phase region is large, when controlling the online molten salt isothermal phase transformation, the molten salt circulation volume at the front end of the salt bath is controlled to be 600-800 t / h, and the molten salt temperature rise is ≤12°C, so as to control the wire rod to quickly enter the pearlite phase region for isothermal phase transformation as much as possible.

[0030] Preferably, since the temperature rise of the wire rod is small after long-term isothermal treatment, during the online molten salt isothermal phase change control, the molten salt circulation volume at the rear end of the salt bath is controlled to be 350~550t / h, and the molten salt temperature rise is ≤5°C. The phase change temperature is controlled as much as possible to improve the organizational uniformity of the wire rod, so as to promote sufficient phase change of the wire rod, reduce mechanical fluctuations in the same circle, and prevent precipitation coarsening caused by excessive molten salt temperature rise.

[0031] Preferably, the roller slow cooling adopts the roller insulation cover to be closed, and the wire rod is cooled to 350~400℃ at a cooling rate of 0.25~1.0℃ / s, and then the roller speed is increased to 0.6~0.8m / s for transportation to the coil. Preferably, the initial roller speed is 0.2~0.45m / s, so that the wire rod can maintain a slower cooling rate after passing through the molten salt to further soften the wire rod structure. After that, the temperature is reduced and the softening effect is weakened. The production efficiency is improved by increasing the roller speed to quickly enter the coil.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) In view of the fact that the existing 12.9 grade non-quenched and tempered steel is rarely developed and the small amount of development adds Ti, Nb, V microalloying elements, combined with the large drawing deformation in the bolt factory, resulting in a very high risk of cold heading cracking, the present invention adopts a high C-Si-Mn-low Cr-low Mo composition design, does not add expensive microalloying elements such as Ti, Nb, V, etc., and replaces the addition of high Mn, Cr, Mo and other alloying components with C, which is a more economical strengthening element, so that the material cost is further reduced. At the same time, the microstructure is mainly tempered pearlite, contains a small amount of ferrite and fused pearlite, and the network carbide can reach level 0, so that the high strength and high plasticity of the wire rod are matched, and the product tensile strength Rm can reach 1165~1215MPa, and the cross-sectional shrinkage Z is 53%~58%. It is used in the manufacture of 12.9 grade non-quenched and tempered fasteners, bolts and other application fields, has good market application prospects, and can reduce the risk of wire breakage during drawing and cold heading cracking.

[0034] (2) The manufacturing method of the present invention adopts a high C chemical composition design, combined with online molten salt isothermal phase transformation control and roller slow cooling technology process design, which can quickly skip the temperature range of carbide precipitation from austenite along the grain boundary and the transformation of austenite to ferrite, and control the wire rod to quickly enter the pearlite phase region for isothermal phase transformation as much as possible. After a long period of molten salt isothermal treatment, the pearlite structure is tempered and softened as much as possible, and the pearlite lamellar melting is promoted to be transformed into a fused pearlite structure. Combined with the inhibitory effect of Mo on the coarsening of precipitated phases such as Cr, high-temperature softening and tempering state control are carried out, and roller slow cooling is used for further softening to ensure the strength and plasticity matching of the wire rod. 12.9 grade non-quenched and tempered hot-rolled high carbon cold heading steel wire rod is successfully prepared, which can simplify the process and has good industrial adaptability.

[0035] (3) The manufacturing method of the present invention combines controlled rolling and controlled cooling technology, uses higher rolling temperature and larger reduction, further promotes the alloy homogenization and grain refinement of the high carbon component system, and cooperates with the regulation of the molten salt temperature rise at the front and rear ends of the salt bath during online molten salt isothermal phase transformation control to further improve the uniformity of the wire rod structure, economical production, and good industrial adaptability. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0037] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;

[0038] Figure 2 is the metallographic structure diagram of Example 2 of the present invention;

[0039] Figure 3 is the metallographic structure diagram of Comparative Example 5 of the present invention;

[0040] Figure 4 It is the metallographic structure diagram of Example 3 of the present invention. DETAILED DESCRIPTION

[0041] The embodiments described below with reference to the accompanying drawings are exemplary and are only for illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention. They should not be construed as limiting the scope of the present invention, which is limited only by the appended claims. Embodiment 1:

[0042] A preferred embodiment of the manufacturing method of the 12.9 grade non-quenched and tempered hot-rolled high-carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include C: 0.75%, Si: 0.28%, Mn: 0.88%, Cr: 0.36%, Mo: 0.1%, P: 0.015%, S: 0.012%, and the rest are Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling and controlled cooling → wire laying → online molten salt isothermal phase change control → roller slow cooling → coiling, specifically:

[0043] The controlled rolling and controlled cooling is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the components of the steel billet and avoid decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 20mm through a rolling line. A high rolling temperature and a large reduction are selected to promote the alloy homogenization and grain refinement of the high-carbon component system. Specifically: the steel billet soaking temperature is controlled to be 1130°C, the soaking time is 1.8h, the initial rolling temperature is 1115°C, the initial rolling reduction is 45%, the final rolling temperature is 1005°C, and the final rolling reduction is 39%.

[0044] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller. The appropriate spinning temperature is used to avoid the precipitation of network carbides in the high-carbon wire rod during the spinning stage, and to avoid excessively high temperature to increase the tendency of grain growth, thereby creating conditions for the deformation nucleus of the pearlite phase. Specifically, the spinning temperature is controlled to be 971°C.

[0045] The online molten salt isothermal phase transformation control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature. Even if the wire rod is cooled to the pearlite phase region at a cooling rate of 41°C / s for isothermal phase transformation, the temperature range in which carbides precipitate from austenite along grain boundaries in a network and austenite transforms into ferrite is quickly skipped. At the same time, the pearlite formed by the phase transformation is promoted to undergo high-temperature softening, and the pearlite lamellar melting is promoted to transform into melting pearlite. In combination with the inhibitory effect of Mo on the coarsening of precipitated phases such as Cr, high-temperature softening and tempering state control are performed to improve the organizational uniformity of the wire rod as much as possible. Specifically, the molten salt isothermal temperature is controlled to be 510°C, the processing time is 522s, the molten salt circulation volume at the front end of the salt bath tank is controlled to be 800t / h, the molten salt temperature rise is ≤12°C, and the molten salt circulation volume at the rear end of the salt bath tank is controlled to be 440t / h, and the molten salt temperature rise is ≤5°C.

[0046] The roller slow cooling process adopts the roller insulation cover to be closed, and the wire rod coming out of the salt bath tank is conveyed by rollers into the insulation cover for slow cooling treatment to promote further softening of the wire rod structure. Specifically: the initial roller speed is 0.2m / s, and the wire rod is cooled to 400℃ at a cooling rate of 0.25℃ / s, and then the roller speed is increased to 0.8m / s for conveying until coiling; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 310℃. After packaging and storage, the finished cold heading steel wire rod is obtained, and its metallographic structure diagram is as follows Figure 1 shown.

[0047] Comparative Example 1:

[0048] A method for manufacturing hot-rolled high-carbon wire rod, which differs from Example 1 in that: the method is manufactured according to the process flow of controlled rolling and controlled cooling → wire laying → Stelmor rapid cooling → roller slow cooling → coiling. Specifically: the Stelmor rapid cooling is to open 1~7# fans at 98%, so that the wire rod is cooled to 575°C at a cooling rate of 10°C / s; the roller slow cooling is to close all fans and insulation covers, so that the wire rod completes phase change at a cooling rate of 1.3°C / s in the cover, and the finished wire rod is obtained after coiling off the line.

[0049] Comparative Example 2:

[0050] A method for manufacturing a hot-rolled high-carbon wire rod, which differs from Example 1 in that: the manufacturing method is manufactured according to the process flow of controlled rolling and controlled cooling → low-temperature wire drawing → online molten salt isothermal phase change control → roller slow cooling → coiling, specifically: the steel billet soaking temperature is controlled to be 1085°C, the soaking time is 2h, the initial rolling temperature is 1065°C, the initial rolling reduction is 39%, the final rolling temperature is 950°C, the final rolling reduction is 37%, and the wire drawing temperature is 930°C. Embodiment 2:

[0051] A preferred embodiment of the manufacturing method of the 12.9 grade non-quenched and tempered hot-rolled high-carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include C: 0.75%, Si: 0.35%, Mn: 0.68%, Cr: 0.34%, Mo: 0.19%, P: 0.013%, S: 0.014%, and the rest are Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling and controlled cooling → wire laying → online molten salt isothermal phase change control → roller slow cooling → coiling, specifically:

[0052] The controlled rolling and controlled cooling is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the components of the steel billet and avoid decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 15mm through a rolling line. A high rolling temperature and a large reduction are selected to promote the alloy homogenization and grain refinement of the high-carbon component system. Specifically: the steel billet soaking temperature is controlled to be 1110°C, the soaking time is 1.8h, the initial rolling temperature is 1095°C, the initial rolling reduction is 47%, the final rolling temperature is 995°C, and the final rolling reduction is 42%.

[0053] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller. The appropriate spinning temperature is used to avoid the precipitation of network carbides in the high-carbon wire rod during the spinning stage, and to avoid excessively high temperature to increase the tendency of grain growth, thereby creating conditions for the deformation nucleus of the pearlite phase. Specifically, the spinning temperature is controlled to be 965°C.

[0054] The online molten salt isothermal phase transformation control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature. Even if the wire rod is cooled to the pearlite phase region at a cooling rate of 39°C / s for isothermal phase transformation, the temperature range in which carbides precipitate from austenite along grain boundaries in a network and austenite transforms into ferrite is quickly skipped. At the same time, the pearlite formed by the phase transformation is promoted to undergo high-temperature softening, and the pearlite lamellar melting is promoted to transform into melting pearlite. In combination with the inhibitory effect of Mo on the coarsening of precipitated phases such as Cr, high-temperature softening and tempering state regulation are performed to improve the organizational uniformity of the wire rod as much as possible. Specifically, the molten salt isothermal temperature is controlled to be 528°C, the processing time is 700s, the molten salt circulation volume at the front end of the salt bath tank is controlled to be 670t / h, the molten salt temperature rise is ≤12°C, and the molten salt circulation volume at the rear end of the salt bath tank is controlled to be 350t / h, and the molten salt temperature rise is ≤5°C.

[0055] The roller slow cooling process adopts the roller insulation cover to be closed, and the wire rod coming out of the salt bath tank is conveyed by rollers into the insulation cover for slow cooling treatment to promote further softening of the wire rod structure. Specifically: the initial roller speed is 0.3m / s, and the wire rod is cooled to 380°C at a cooling rate of 0.55°C / s, and then the roller speed is increased to 0.75m / s for conveying until it is coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 320°C. After packaging and storage, the cold heading steel wire rod product is obtained, and its metallographic structure diagram is as follows Figure 2 shown.

[0056] Comparative Example 3:

[0057] A method for manufacturing a hot-rolled high-carbon wire rod, the manufacturing method of which differs from that of Example 2 in that the isothermal temperature of the molten salt is controlled to be 581° C., and the finished wire rod is obtained after the coil is rolled off the production line.

[0058] Comparative Example 4:

[0059] A method for manufacturing a hot-rolled high-carbon wire rod, the manufacturing method of which differs from that of Example 2 in that the isothermal temperature of the molten salt is controlled to be 500° C., and the finished wire rod is obtained after the coil is rolled off the production line.

[0060] Comparative Example 5:

[0061] A method for manufacturing a hot-rolled high-carbon wire rod, the difference between the manufacturing method and Example 2 is that: the molten salt isothermal temperature is controlled to be 50°C, the processing time is 30s, and the finished wire rod is obtained without coiling. The metallographic structure diagram is as follows Figure 3 shown. Embodiment 3:

[0062] A preferred embodiment of the manufacturing method of the 12.9 grade non-quenched and tempered hot-rolled high-carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include C: 0.76%, Si: 0.2%, Mn: 0.9%, Cr: 0.39%, Mo: 0.25%, P: 0.014%, S: 0.015%, and the rest are Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling and controlled cooling → wire laying → online molten salt isothermal phase change control → roller slow cooling → coiling, specifically:

[0063] The controlled rolling and controlled cooling is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the components of the steel billet and avoid decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter specification of 22mm through a rolling line. A high rolling temperature and a large reduction are selected to promote the alloy homogenization and grain refinement of the high-carbon component system. Specifically: the steel billet soaking temperature is controlled to be 1140°C, the soaking time is 2h, the initial rolling temperature is 1125°C, the initial rolling reduction is 40%, the final rolling temperature is 1030°C, and the final rolling reduction is 38%.

[0064] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller. Through an appropriate spinning temperature, the high carbon wire rod is prevented from precipitating network carbides during the spinning stage, and the excessive temperature is prevented from increasing the tendency of grain growth, thereby creating conditions for the pearlite phase deformation nucleus. Specifically, the spinning temperature is controlled to be 1000°C.

[0065] The online molten salt isothermal phase transformation control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature. Even if the wire rod is cooled to the pearlite phase region at a cooling rate of 40°C / s for isothermal phase transformation, the temperature range in which carbides precipitate from austenite along grain boundaries in a network and austenite transforms into ferrite is quickly skipped. At the same time, the pearlite formed by the phase transformation is promoted to undergo high-temperature softening, and the pearlite lamellar melting is promoted to transform into melting pearlite. In combination with the inhibitory effect of Mo on the coarsening of precipitated phases such as Cr, high-temperature softening and tempering state control are performed to improve the uniformity of the wire rod structure as much as possible. Specifically, the molten salt isothermal temperature is controlled to be 560°C, the processing time is 615s, the molten salt circulation volume at the front end of the salt bath tank is controlled to be 720t / h, the molten salt temperature rise is ≤12°C, and the molten salt circulation volume at the rear end of the salt bath tank is controlled to be 380t / h, and the molten salt temperature rise is ≤5°C.

[0066] The roller slow cooling process adopts the roller insulation cover to be closed, and the wire rod coming out of the salt bath tank is conveyed by rollers into the insulation cover for slow cooling treatment to promote further softening of the wire rod structure. Specifically: the initial roller speed is 0.45m / s, and the wire rod is cooled to 350℃ at a cooling rate of 1℃ / s, and then the roller speed is increased to 0.6m / s for conveying until it is coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 300℃. After packaging and storage, the finished cold heading steel wire rod is obtained, and its metallographic structure diagram is as follows Figure 4 shown.

[0067] Comparative Example 6:

[0068] A method for manufacturing a hot-rolled high-carbon wire rod, the manufacturing method of which is different from that of Example 3 in that the processing time of the online molten salt isothermal phase change control is 750s, and the finished wire rod is obtained after the coil is rolled off the line.

[0069] Comparative Example 7:

[0070] A method for manufacturing a hot-rolled high-carbon wire rod, the manufacturing method of which is different from that of Example 3 in that the processing time of the online molten salt isothermal phase change control is 830s, and the finished wire rod is obtained after the coil is rolled off the line.

[0071] Comparative Example 8:

[0072] A method for manufacturing a hot-rolled high-carbon wire rod, the manufacturing method of which is different from that of Example 3 in that the processing time of the online molten salt isothermal phase change control is 300s, and the finished wire rod is obtained after the coil is rolled off the line. Embodiment 4:

[0073] A preferred embodiment of the manufacturing method of the 12.9 grade non-quenched and tempered hot-rolled high-carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include C: 0.72%, Si: 0.27%, Mn: 0.6%, Cr: 0.42%, Mo: 0.3%, P: 0.014%, S: 0.015%, and the rest are Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling and controlled cooling → wire laying → online molten salt isothermal phase change control → roller slow cooling → coiling, specifically:

[0074] The controlled rolling and controlled cooling is used to heat a steel billet with a specification of 180mm×180mm through a heating furnace to promote the homogenization of the components of the steel billet and avoid decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 10mm through a rolling line. A high rolling temperature and a large reduction are selected to promote the alloy homogenization and grain refinement of the high-carbon component system. Specifically: the steel billet soaking temperature is controlled to be 1090°C, the soaking time is 1.5h, the initial rolling temperature is 1075°C, the initial rolling reduction is 50%, the final rolling temperature is 960°C, and the final rolling reduction is 46%.

[0075] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller. The appropriate spinning temperature is used to avoid the precipitation of network carbides in the high-carbon wire rod during the spinning stage, and to avoid excessively high temperature to increase the tendency of grain growth, thereby creating conditions for the deformation nucleus of the pearlite phase. Specifically, the spinning temperature is controlled to be 940°C.

[0076] The online molten salt isothermal phase transformation control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature. Even if the wire rod is cooled to the pearlite phase region at a cooling rate of 38°C / s for isothermal phase transformation, the temperature range in which carbides precipitate from austenite along grain boundaries in a network and austenite transforms into ferrite is quickly skipped. At the same time, the pearlite formed by the phase transformation is promoted to undergo high-temperature softening, and the pearlite lamellar melting is promoted to transform into melting pearlite. In combination with the inhibitory effect of Mo on the coarsening of precipitated phases such as Cr, high-temperature softening and tempering state control are performed to improve the uniformity of the wire rod structure as much as possible. Specifically, the molten salt isothermal temperature is controlled to be 541°C, the processing time is 400s, the molten salt circulation volume at the front end of the salt bath tank is controlled to be 600t / h, the molten salt temperature rise is ≤12°C, and the molten salt circulation volume at the rear end of the salt bath tank is controlled to be 550t / h, and the molten salt temperature rise is ≤5°C.

[0077] The roller slow cooling process adopts the roller insulation cover to be closed, and the wire rod coming out of the salt bath tank is conveyed by rollers into the insulation cover for slow cooling treatment, so as to promote further softening of the wire rod structure. Specifically: the initial roller speed is 0.35m / s, and the wire rod is cooled to 365℃ at a cooling rate of 0.65℃ / s, and then the roller speed is increased to 0.7m / s for conveying until it is coiled; the coiling process is used to coil the wire rod into a coil by a coiling drum, and the coiling temperature is 326℃. After packaging and warehousing, the finished cold heading steel wire rod is obtained.

[0078] Comparative Example 9:

[0079] A method for manufacturing a hot-rolled high-carbon wire rod, which differs from Example 4 in that: the method is manufactured according to the process flow of controlled rolling and controlled cooling → wire spinning → online molten salt isothermal phase change control → air cooling → coiling, wherein the air cooling is performed by opening a roller heat preservation cover, and conveying the wire rod out of a salt bath tank by a roller, cooling the wire rod to 325°C at a cooling rate of 2.9°C / s, and obtaining the finished wire rod after coiling off the line.

[0080] The organization and performance of the wire rods obtained in the above embodiments and comparative examples were tested: the tensile test was carried out according to "GB-T 228.1-2021 Metal Material Tensile Test Part 1: Room Temperature Test Method" to obtain the tensile strength and cross-sectional shrinkage rate, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The same-circle mechanical fluctuation range test method: 2 circles of wire rods were taken 5m away from the end of the coil, and each circle of wire rods was divided into 8 sections on average with the overlap area as the base point. One tensile specimen was taken from each section. The extreme difference in strength of the tensile specimens after the tensile test was the same-circle mechanical fluctuation. The comparison results obtained are shown in Table 1 below:

[0081] Table 1. Comparison of the microstructure and properties of cold heading steel wire rods with different compositions and manufacturing methods

[0082]

[0083] From the comparison results of Example 1 and Comparative Example 1, it can be seen that compared with increasing the rolling and spinning temperature and then using Stelmor air cooling for rapid cooling, a higher level of network carbide will be produced, and troostite and ferrite structures will be obtained, resulting in a higher strength of the wire rod but a lower cross-sectional shrinkage rate. The present invention adopts a high C-Si-Mn-low Cr-low Mo component design, combined with online molten salt isothermal phase transformation control and roller slow cooling technology process design, which can quickly skip the temperature range in which carbides precipitate from austenite along grain boundaries in a network and austenite is transformed into ferrite, and the network carbide can reach level 0, and the wire rod can be controlled to quickly enter the pearlite phase region for isothermal phase transformation as much as possible. After a long period of molten salt isothermal treatment, the pearlite structure is tempered and softened as much as possible, promoting pearlite The lamellar melt is transformed into a fused pearlite structure, and the high-temperature softening and tempering state are regulated by Mo's inhibitory effect on the coarsening of precipitated phases such as Cr. The microstructure is mainly tempered pearlite, containing a small amount of ferrite and fused pearlite, and the product tensile strength Rm can reach 1165~1215MPa, and the cross-sectional shrinkage rate Z is 53%~58%. It is used in the manufacture of 12.9-grade non-quenched and tempered fasteners and bolts and other application fields, and has good market application prospects; it can be seen from the comparison results of Example 1 and Comparative Example 2 that compared with the low-temperature spinning, which is unfavorable for the control of network carbides and the uniformity of composition, the present invention uses a higher rolling temperature and a larger reduction to further promote the alloy homogenization and grain refinement of the high-carbon component system, and has good industrial adaptability.

[0084] From the comparison results of Examples 1 to 4 and Comparative Example 3, it can be seen that the higher the molten salt isothermal temperature, the larger the lamellar spacing of the tempered pearlite, the higher the ferrite content in the organization, which is beneficial to the melting of the pearlite lamellae, but too high a molten salt isothermal temperature will lead to too high a ferrite content in the organization, which is not conducive to the strength of the matrix; from the comparison results of Example 2 and Comparative Example 4, it can be seen that the lower the molten salt isothermal temperature, the smaller the lamellar spacing of the tempered pearlite, the lower the ferrite content in the organization, the strength of the cold heading steel wire rod increases, and the plasticity decreases; from the comparison results of Example 2 and Comparative Example 5, it can be seen that too low a molten salt isothermal temperature will lead to the generation of bainite or even martensite abnormal organizations in the organization, which seriously affects the plasticity of the wire rod, cannot be rolled, and is easy to be brittle.

[0085] From the comparison results of Examples 1 to 4 and Comparative Example 6, it can be seen that the longer the treatment time, the better the tempering softening effect of pearlite, the more the melted pearlite structure, the more uniform the structure, the lower the strength of the cold heading steel wire rod, and the higher the plasticity; from the comparison results of Example 3 and Comparative Example 7, it can be seen that although the longer the treatment time is beneficial to softening, too long a treatment time will accelerate the precipitation and coarsening of Cr, and significantly reduce the plasticity of the wire rod; from the comparison results of Example 3 and Comparative Example 8, it can be seen that the shorter the time, the weaker the high-temperature softening effect of the pearlite structure, which is not conducive to the melting of the pearlite lamellae, and the strength of the cold heading steel wire rod increases, while the plasticity decreases.

[0086] From the comparison results of Example 4 and Comparative Example 9, it can be seen that compared with air cooling which is not conducive to softening the structure, slow cooling through rollers can further utilize the high temperature state of the wire rod after it leaves the molten salt through slow cooling, continue the softening and melting effect in the later stage of the online molten salt isothermal phase change, and further improve the plasticity of the wire rod.

[0087] The series of detailed descriptions listed above are only specific descriptions of the feasible embodiments of the present invention, and they are not intended to limit the scope of protection of the present invention. For example, the steel billet is obtained by converter smelting, refining, and continuous casting. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

Claims

1. A 12.9 grade non-quenched and tempered hot-rolled high carbon cold heading steel wire rod, characterized in that: The chemical composition and mass percentage of the cold heading steel wire rod include C: 0.72% to 0.76%, Si: 0.20% to 0.35%, Mn: 0.60% to 0.90%, Cr: 0.34% to 0.42%, Mo: 0.10% to 0.30%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities; Its microstructure includes tempered pearlite with a volume percentage of ≥93%, and the rest is ferrite and fused pearlite; The manufacturing method thereof comprises: The wire rod is produced by controlled rolling and controlled cooling according to the chemical composition of the 12.9 grade non-quenched and tempered hot-rolled high-carbon cold heading steel wire rod. After the wire rod is spun into a wire rod at a spinning temperature of ≥940°C, it is subjected to online molten salt isothermal phase transformation control, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥38°C / s for isothermal phase transformation, and at the same time, the pearlite formed by the phase transformation is promoted to undergo high-temperature softening, and the pearlite lamellae are promoted to be melted and transformed into melted pearlite. Finally, it is slowly cooled by a roller to produce a cold heading steel wire rod with a microstructure including tempered pearlite, ferrite and melted pearlite; during the online molten salt isothermal phase transformation control, the molten salt isothermal temperature is controlled to be 510-560°C, and the processing time is 400-700s.

2. The 12.9 grade non-quenched and tempered hot-rolled high carbon cold heading steel wire rod according to claim 1, characterized in that: The interlamellar spacing of the tempered pearlite is 150-185 nm, the volume percentage of the ferrite is 1%-5%, and the network carbide of the cold heading steel wire rod is level 0.

3. The 12.9 grade non-quenched and tempered hot-rolled high carbon cold heading steel wire rod according to claim 1, characterized in that: The cold heading steel wire rod has a diameter of 10.0-22.0 mm, a tensile strength of 1165-1215 MPa, a cross-sectional shrinkage of 53%-58%, and a same-circle mechanical fluctuation of ≤28 MPa.

4. A method for manufacturing a 12.9 grade non-quenched and tempered hot-rolled high carbon cold heading steel wire rod, characterized in that: The manufacturing method comprises: producing a wire rod by controlled rolling and controlled cooling according to the chemical composition of the 12.9 grade non-quenched and tempered hot-rolled high-carbon cold heading steel wire rod as claimed in claim 1, after the wire rod is spun into a wire rod at a spinning temperature of ≥940°C, the wire rod is subjected to online molten salt isothermal phase transformation control, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥38°C / s for isothermal phase transformation, and at the same time, the pearlite formed by the phase transformation is promoted to undergo high-temperature softening, and the pearlite lamellae are promoted to be melted and transformed into melted pearlite, and finally, the wire rod is subjected to roller slow cooling to be made into a cold heading steel wire rod having a microstructure including tempered pearlite with a volume percentage of ≥93%, and the rest being ferrite and melted pearlite; during the online molten salt isothermal phase transformation control, the molten salt isothermal temperature is controlled to be 510~560°C, and the processing time is 400~700s.

5. The method for manufacturing 12.9 grade non-quenched and tempered hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: When heating the steel billet before controlled rolling and controlled cooling, the steel billet soaking temperature is controlled to be ≤1140°C and the soaking time is controlled to be ≤2h.

6. The method for manufacturing 12.9 grade non-quenched and tempered hot-rolled high carbon cold heading steel wire rod according to claim 5, characterized in that: During the controlled rolling and controlled cooling, the initial rolling temperature is controlled to be 1075-1125° C., and the initial rolling reduction is 40%-50%.

7. The method for manufacturing 12.9 grade non-quenched and tempered hot-rolled high carbon cold heading steel wire rod according to claim 6, characterized in that: During the controlled rolling and controlled cooling, the final rolling temperature is controlled to be ≥960°C, and the final rolling reduction is 38%~46%.

8. The method for manufacturing 12.9 grade non-quenched and tempered hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: During the online molten salt isothermal phase change control, the front end molten salt circulation volume of the salt bath tank is controlled to be 600-800 t / h, the molten salt temperature rise is ≤12°C, the rear end molten salt circulation volume of the salt bath tank is controlled to be 350-550 t / h, and the molten salt temperature rise is ≤5°C.

9. The method for manufacturing 12.9 grade non-quenched and tempered hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: The roller slow cooling adopts the roller heat preservation cover to close, and the wire rod is cooled to 350-400°C at a cooling rate of 0.25-1.0°C / s, and then the roller speed is increased to 0.6-0.8m / s for transportation to the coil.

Citation Information

Cited By

  • Wire rod for non-quenched and tempered fastener, production method of wire rod and fastener

    CN121472708A

  • A wire rod for non-quenched and tempered fastener, a production method thereof, and a fastener

    CN121472708B