Porous cellulose medium and method for producing the same
The spraying process produces porous cellulose particles with particle sizes of 1 to 600 μm, which solves the problem of difficulty in increasing the pore size and volume in the prior art, and achieves efficient separation of macromolecules and improves the chromatographic separation efficiency.
Patent Information
- Application Number
- CN202080040912.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-06-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-06-19
AI Technical Summary
The existing porous cellulose media is difficult to increase the pore size and pore volume during the manufacturing process, resulting in low separation efficiency of macromolecular target molecules, especially for molecules with a weight average molecular weight of about 105.0 to 105.5 in standard samples. Separation.
The cellulose solution is sprayed into particles through the spraying process and solidified in the solidification phase. The gas supplied to the control nozzle is only gas supplied from the nozzle and the cellulose solution, and porous fibers with particle sizes of 1 to 600 μm are produced. The plasma particles are used to make porous cellulose media with large fine pore sizes, satisfying the specific particle size grading and gel partition coefficient relationships to improve separation efficiency.
It is possible to efficiently separate macromolecules with weight average molecular weight of about 105.0 to 105.5 in standard samples, providing a porous cellulose medium with large pore size and pore volume, and improving the efficiency of chromatographic separation.
Smart Images

Figure CN113905815B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to porous cellulose media and methods of making the same. Background Art
[0002] Polysaccharides represented by cellulose and their derivatives have been used for various purposes. For example, porous cellulose media can be used as adsorbents by themselves, and can also be given adsorption, separation, catalysis and other functions by chemically modifying their surfaces.
[0003] For example, Patent Document 1 discloses a method for producing porous cellulose beads, which is characterized by comprising the following steps: step a), mixing a low-temperature alkaline aqueous solution with cellulose to produce a cellulose fine dispersion; step b), adding a crosslinking agent to the cellulose fine dispersion to produce a mixed solution; step c), dispersing the mixed solution in a dispersion medium to produce an emulsion; and step d), contacting the emulsion with a coagulation solvent. It is believed that according to the method described in Patent Document 1, cellulose beads having a pore shape and pore size distribution suitable for an adsorbent and excellent adsorption capacity can be produced.
[0004] In addition, Patent Document 2 discloses a method for producing porous cellulose, characterized in that it is a method for dissolving cellulose in a mixed aqueous solution of 5 to 12% by weight of sodium hydroxide and 9 to 20% by weight of urea or 3 to 8% by weight of thiourea, wherein crystalline cellulose is used as the aforementioned cellulose, and the aforementioned mixed aqueous solution is precooled to 10 to 15° C., or the aforementioned cellulose is dissolved in the aforementioned mixed aqueous solution at 10 to 15° C. without precooling, and the dissolved crystalline cellulose is regenerated to produce porous cellulose. It is believed that according to the method described in Patent Document 2, crystalline cellulose can be dissolved by a method with fewer steps or at a lower cost than in the conventional method, and porous cellulose can be produced by regenerating crystalline cellulose in such a solution.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2016 / 167268
[0008] Patent Document 2: Japanese Patent Application Publication No. 2011-231152 Summary of the invention
[0009] Problems to be solved by the invention
[0010] The porous cellulose medium can be used as a chromatographic support, etc. Here, if the pore size of the support can be adjusted according to the size of the target molecule to be separated by the chromatographic support and the pore volume of the pore size is increased, the separation efficiency of the target molecule can be improved.
[0011] For example, when a porous cellulose medium is used as a chromatographic support, and a macromolecule such as a protein (for example, a molecule with a weight average molecular weight of 10 used as a standard sample for chromatography) is used as a chromatographic support, 5.0 ~10 5.5 In the case of using a target molecule (a high molecular weight of about 1000 Å) as a target molecule, in order to efficiently separate the target molecule, it is required to increase the pore diameter of the porous cellulose medium and increase the pore volume of the pore diameter. However, in the conventional method for manufacturing a porous cellulose medium, it is difficult to increase the pore volume for a large pore diameter, and it is not possible to efficiently separate, for example, a standard sample with a weight average molecular weight of 10 5.0 ~10 5.5 Large target molecules of about .
[0012] Under such circumstances, the main purpose of the present disclosure is to provide a large pore volume with a large pore diameter, which can efficiently 5.0 ~10 5.5 A new porous cellulose medium for separating large target molecules of about 100 μm.
[0013] Means for solving problems
[0014] The inventors of the present application have conducted intensive research to solve the above-mentioned problems. As a result, it was found that, in the particle formation step of a method for producing a porous cellulose medium, which includes a particle formation step of spraying a cellulose solution from a nozzle into a space to form particles, and a coagulation step of coagulating the particles in a coagulation phase, the gas supplied into the space where the cellulose solution is sprayed is controlled to be only the gas supplied from the nozzle together with the cellulose solution, thereby producing a porous cellulose medium with a large pore diameter and a large pore volume, and being able to efficiently perform a particle formation test on a standard sample with a weight average molecular weight of 10 5.0 ~10 5.5 More specifically, it was found that by adopting this manufacturing method, the following porous cellulose medium can be suitably manufactured, wherein the porous cellulose medium comprises porous cellulose particles having a particle size of 1 to 600 μm, the porous cellulose medium is classified with a sieve, the component sandwiched between the sieves with a mesh size of 53 μm and 106 μm is used as a support for size exclusion chromatography, and when pure water is used as a mobile phase and standard polyethylene oxide is supplied to the size exclusion chromatography, the weight average molecular weight Mw of the standard polyethylene oxide and the gel partition coefficient K av The following relations (A) and (B) are satisfied.
[0015] When 4.80≤logMw≤5.50, K av >-0.445×logMw+2.55 (A)
[0016] 5.75≤logMw, 0≤K av <0.19 (B)
[0017] The present disclosure was completed through further repeated studies based on these findings.
[0018] Item 1. A porous cellulose medium comprising porous cellulose particles having a particle size of 1 to 600 μm, wherein:
[0019] The porous cellulose medium was classified with a sieve, and the fraction sandwiched between the sieves with mesh sizes of 53 μm and 106 μm was used as a support for size exclusion chromatography. When pure water was used as a mobile phase and standard polyethylene oxide was supplied to the size exclusion chromatography, the weight average molecular weight Mw of the standard polyethylene oxide and the gel partition coefficient K av The following relations (A) and (B) are satisfied.
[0020] When 4.80≤logMw≤5.50, K av >-0.445×logMw+2.55 (A)
[0021] 5.75≤logMw, 0≤K av <0.19 (B)
[0022] Item 2. The porous cellulose medium according to Item 1, wherein the weight average molecular weight Mw and the gel partition coefficient K of the standard polyethylene oxide are av The following relationship (C) is satisfied.
[0023] When 4.80≤logMw≤5.50, -0.445×logMw+3>K av >-0.445×logMw+2.55
[0024] (C)
[0025] Item 3. A method for producing a porous cellulose medium, comprising the following steps:
[0026] a micronizing step of spraying the cellulose solution from a nozzle into the space to form microparticles; and
[0027] a solidification step, wherein the particles are solidified in a solidification phase;
[0028] In the atomization step, the gas supplied to the space into which the cellulose solution is sprayed is controlled to include only the gas supplied from the nozzle together with the cellulose solution.
[0029] Item 4. A method for producing a porous cellulose medium as described in Item 3, wherein the solvent of the aforementioned cellulose solution is at least one selected from the group consisting of a copper ethylenediamine solution, N-methylmorpholine oxide (NMMO) monohydrate, a caustic soda-urea aqueous solution, an aqueous solution of calcium thiocyanate, a N,N'-dimethylacetamide solution of lithium chloride, a dimethylformamide solution of lithium chloride, a dimethylimidazolium solution of lithium chloride, and a dimethyl sulfoxide solution of lithium chloride.
[0030] Item 5. The method for producing a porous cellulose medium according to Item 3 or 4, wherein the coagulated phase is composed of a component different from the solvent of the cellulose solution.
[0031] Item 6. A method for producing a porous cellulose medium as described in any one of Items 3 to 5, wherein the solidified phase is composed of a liquid phase or a vapor phase of at least one selected from the group consisting of alcohols, ketones, esters, ethers, water, inorganic acids, and inorganic salt aqueous solutions, or a combination of a gas phase of an inert gas and the liquid phase or vapor phase.
[0032] Effects of the Invention
[0033] According to the present disclosure, a large pore volume can be provided, and a standard sample with a weight average molecular weight of 10 can be efficiently 5.0 ~10 5.5 A novel porous cellulose medium for separating large target molecules of about 100 μm and a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] [ Figure 1 ] shows the logarithmic value (logMw) of the weight average molecular weight of standard polyethylene oxide and the gel partition coefficient K for the porous cellulose media of Examples 1 to 3 (each with different cellulose). av The straight lines of the given values 1 to 7 are also marked.
[0035] [ Figure 2 ] shows the logarithmic value (logMw) of the weight average molecular weight of standard polyethylene oxide and the gel partition coefficient K for the porous cellulose media of Examples 1, 4, and 5 (each with a different nozzle). av The straight lines of the given values 1 to 7 are also marked.
[0036] [ Figure 3] shows the logarithmic value (logMw) of the weight average molecular weight of standard polyethylene oxide and the gel partition coefficient K for the porous cellulose media of Examples 4 and 6 (each with a different coagulation bath composition). av The straight lines of the given values 1 to 7 are also marked.
[0037] [ Figure 4 ] shows the logarithmic value (logMw) of the weight average molecular weight of standard polyethylene oxide and the gel partition coefficient K for the porous cellulose media of Examples 4 and 7 (each with a different cellulose solution). av The straight lines of the given values 1 to 7 are also marked.
[0038] [ Figure 5 ] shows the logarithmic value (logMw) of the weight average molecular weight of standard polyethylene oxide and the gel partition coefficient K for the porous cellulose media of comparative reference examples 1 to 6. av The straight lines of the given values 1 to 4 are also marked.
[0039] [ Figure 6 ] shows the logarithmic value (logMw) of the weight average molecular weight of standard polyethylene oxide and the gel partition coefficient K for the porous cellulose media of comparative reference examples 7 to 11. av The straight lines of the given values 1-4 are also marked. DETAILED DESCRIPTION
[0040] 1.Porous cellulose media
[0041] The porous cellulose medium of the present disclosure contains porous cellulose particles having a particle size of 1 to 600 μm. In addition, the porous cellulose medium of the present disclosure is characterized in that the porous cellulose medium is classified by a sieve, and the fraction sandwiched between the sieves having a mesh size of 53 μm and 106 μm is used as a support for size exclusion chromatography, and when pure water is used as a mobile phase and standard polyethylene oxide is supplied to the size exclusion chromatography, the weight average molecular weight Mw of the standard polyethylene oxide and the gel partition coefficient K av The following relations (A) and (B) are satisfied.
[0042] Relationship (A): 4.80≤logMw≤5.50, K av >-0.445×logMw+2.55
[0043] Relationship (B): 5.75≤logMw, 0≤K av <0.19
[0044] The porous cellulose medium of the present disclosure is described in detail below. It should be noted that, as described later, regarding the relationship (A), the straight line K av = -0.445 × logMw + 2.55 is in, for example Figures 1 to 6 In the relationship (B), the straight line K av = 0.19 is in, for example Figures 1 to 6 In the porous cellulose medium of the present disclosure that satisfies both the relationship (A) and the relationship (B), the pore volume is large due to the large pore diameter, and the weight average molecular weight of the standard sample is 10. 5.0 ~10 5.5 The porous cellulose medium that satisfies both the relationship (A) and the relationship (B) is a novel porous cellulose medium that has not been known before. As described later, the porous cellulose medium of the present disclosure having such characteristics can be suitably manufactured, for example, by the method described in the item "2. Method for manufacturing porous cellulose" described later.
[0045] The porous cellulose medium of the present disclosure contains porous cellulose particles with a particle size of 1 to 600 μm. Specifically, the porous cellulose medium of the present disclosure is an aggregate of porous cellulose particles in a particle shape, and contains porous cellulose particles with a particle size of 1 to 600 μm. The porous cellulose medium of the present disclosure is not particularly limited as long as it contains porous cellulose particles with a particle size within this range and can measure the relationships (A) and (B) described later (i.e., contains a component sandwiched between a sieve with a mesh size of 53 μm and a sieve with a mesh size of 106 μm). However, the weight average molecular weight of the standard sample with a molecular weight of 10 is more efficiently measured. 5.0 ~10 5.5 From the viewpoint of separating large target molecules of about 5 μm, porous cellulose particles having a particle size of about 5 to 400 μm are preferably included, and porous cellulose particles having a particle size of about 10 to 250 μm are more preferably included. It should be noted that the particle size of the porous cellulose particles is a value set by a sieve. For example, if a porous cellulose medium is passed through a sieve with a mesh size of 250 μm and repeatedly washed with water on a sieve with a mesh size of 10 μm, porous cellulose particles having a particle size range of 10 to 250 μm can be extracted from the porous cellulose medium.
[0046] The porous cellulose medium of the present disclosure may contain porous cellulose particles having a particle size of less than 1 μm, or may contain porous cellulose particles having a particle size of more than 600 μm. The lower limit of the particle size of the porous cellulose medium of the present disclosure may be, for example, 1 μm or more, 5 μm or more, and the upper limit may be, for example, 600 μm or less, 500 μm or less, 400 μm or less, 300 μm or less, etc. The proportion of porous cellulose particles having a particle size of 10 to 250 μm in the porous cellulose medium of the present disclosure is preferably 80% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, particularly preferably 98% by mass or more, and may also be 100% by mass.
[0047] The porous cellulose medium of the present disclosure is classified by sieves, and the fraction sandwiched between the sieves with mesh sizes of 53 μm and 106 μm is used as a support for size exclusion chromatography. When pure water is used as a mobile phase and standard polyethylene oxide is supplied to the size exclusion chromatography, the weight average molecular weight Mw of the standard polyethylene oxide and the gel partition coefficient K av The following relations (A) and (B) are satisfied. Gel partition coefficient K av The determination of and the calculation method of its relationship with logMw are as follows.
[0048] Relationship (A): 4.80≤logMw≤5.50, K av >-0.445×logMw+2.55
[0049] Relationship (B) 5.75≤logMw, 0≤K av <0.19
[0050] <Gel partition coefficient K av Determination of and calculation of its relationship with logMw>
[0051] The porous cellulose medium was classified with a sieve, and the fraction sandwiched between the sieves with mesh sizes of 53 μm and 106 μm was used as a support for size exclusion chromatography. Pure water was used as the mobile phase and standard polyethylene oxide was supplied to the size exclusion chromatography to determine the gel partition coefficient K. av. Specifically, the graded porous cellulose medium is filled into a column (e.g., "Tricorn 10 / 100" manufactured by GE Healthcare Japan Co., Ltd.) in such a way that the bed height becomes 8 cm or more. Connect to a high performance liquid chromatography system to perform size exclusion chromatography. As markers, polyethylene oxide (e.g., TSKgel standard polyethylene oxide SE kit manufactured by TOSOH) and dextran (e.g., Blue dextran (Blue Dextran 2000 manufactured by GE Healthcare)) are dissolved in ultrapure water for use. While degassed ultrapure water is passed through the column at a flow rate of 0.1 mL / min, first, in order to determine the volume other than the bead portion in the column, a weight-average molecular weight of 2×10 6 The flow rate from injection to the peak observed on the RI monitor was calculated using a solution of dextran (Blue dextran (GE Healthcare Blue Dextran 2000)). Next, the flow rate was calculated using the solutions of each marker in the same manner. The measured values were substituted into the following formula to calculate K av The value of .
[0052] K av =(V R -V0) / (V t -V0)
[0053] [Wherein, V R represents the flow rate (mL) from the injection of each marker solution to the observation of the peak, V0 represents the flow rate from the injection of a marker solution with a weight average molecular weight of 2×10 6 The flow rate (mL) of the dextran solution from the beginning to the peak observation, V t Indicates the volume of beads in the column (mL). ]
[0054] In the porous cellulose medium of the present disclosure, the weight average molecular weight of the standard sample is more efficiently 5.0 ~10 5.5 From the perspective of separating large target molecules of about 100 μg / cm2, the weight average molecular weight Mw of the standard polyethylene oxide and the gel partition coefficient K are preferably av In addition to satisfying the aforementioned relations (A) and (B), the following relation (C) is also satisfied.
[0055] Relationship (C): 4.80≤logMw≤5.50, -0.445×logMw+3>K av >-0.445×logMw+2.55
[0056] Here, with respect to the relationship (C), the straight line K av= -0.445 × logMw + 3 is in, for example Figures 1 to 4 In other words, the relationship (C) becomes the straight line shown as the predetermined value 5 in the range of 4.80≤logMw≤5.50. Figures 1 to 4 The range of the curve graph is sandwiched between the straight line of the preset value 1 and the straight line of the preset value 5.
[0057] In addition, in the porous cellulose medium of the present disclosure, the weight average molecular weight of the standard sample is more efficiently 5.0 ~10 5.5 From the perspective of separating large target molecules, the weight average molecular weight Mw of standard polyethylene oxide and the gel partition coefficient K av It is more preferable to satisfy the following relationship (D), and it is even more preferable to satisfy the following relationship (E).
[0058] Relationship (D): 4.80≤logMw≤5.50, -0.521×logMw+3.2>K av >-0.445×logMw+2.55
[0059] Relationship (E): 4.80≤logMw≤5.50, -0.521×logMw+3.2>K av >-0.521×logMw+2.97
[0060] With respect to the relationship (D), the straight line K av = -0.445 × logMw + 2.55 As mentioned above, in e.g. Figures 1 to 6 In the example, the straight line K is shown as the default value 1. In addition, regarding the relationship (D), the straight line K av = -0.521 × logMw + 3.2 is in the case of Figures 1 to 6 In other words, the relationship (D) is expressed in the range of 4.80≤logMw≤5.50. Figures 1 to 6 The range between the straight line of the preset value 1 and the straight line of the preset value 7.
[0061] In addition, regarding the relationship (E), the straight line K av = -0.521 × logMw + 2.97 As mentioned above, in e.g. Figures 1 to 6 In the figure, the straight line K is shown as the default value 3. In addition, regarding the relationship (D), the straight line K av = -0.521 × logMw + 3.2 is in the case of Figures 1 to 6 In other words, the relationship (E) is expressed in the range of 4.80≤logMw≤5.50. Figures 1 to 6 The range between the straight line of the preset value 3 and the straight line of the preset value 7.
[0062] In addition, in the porous cellulose medium of the present disclosure, the weight average molecular weight of the standard sample is more efficiently 5.0 ~10 5.5 From the perspective of separating large target molecules, the weight average molecular weight Mw of standard polyethylene oxide and the gel partition coefficient K av It is preferable to satisfy the following relationship (F), and it is more preferable to satisfy the following relationship (G).
[0063] Relationship (F): 5.75≤logMw, 0≤K av <0.17
[0064] Relationship (G): 5.75≤logMw, -0.0482×logMw+0.3≤K av <0.17
[0065] With respect to the relationship (F), the straight line K av = 0.17 is in, for example Figures 1 to 6 In the figure, the straight line K is shown as the default value 4. In addition, regarding the relationship (G), the straight line K av =Kav=-0.0482×logMw+0.3 is in the case of Figures 1 to 6 The straight line shown as the default value 6 in FIG. That is, the relationship (G) is expressed when 5.75≤logMw Figures 1 to 4 The range between the straight line of the preset value 4 and the straight line of the preset value 6.
[0066] The porous cellulose medium of the present disclosure is composed of cellulose and may contain known components contained in known porous cellulose media within the limits of not impairing the effects of the present disclosure. For example, a porous cellulose medium containing unsubstituted cellulose and a polymer having glucose units other than unsubstituted cellulose may be prepared, and as the polymer, carboxymethyl cellulose, cellulose phosphate, etc. may be suitably used. Such a porous cellulose medium may be endowed with functionality (functionality possessed by the aforementioned polymer) that the porous cellulose itself composed of unsubstituted cellulose does not have. The porous cellulose medium of the present disclosure can usually be stored in a wet state. When drying, sugars, glycerol, etc. are added in appropriate amounts. When stored for a long time under wet conditions, preservatives such as alcohol and sodium azide are added to prevent corruption. In addition, drying may be performed in a state in which glycerol, sugars, urea, etc. are added.
[0067] In addition, the porous cellulose medium of the present disclosure can be particularly suitably used for size exclusion chromatography. This also means that by bonding appropriate ligands to the porous cellulose medium or by replacing or modifying the functional groups on the surface with other functional groups, it can also be used in various modes of chromatographic separation other than size exclusion, including ion exchange, hydrophobic, affinity and other modes.
[0068] In addition, the porous cellulose medium of the present disclosure can be used as a separation medium with further improved strength by cross-linking cellulose chains with covalent bonds using a cross-linking agent.
[0069] An adsorbent can also be produced by immobilizing an affinity ligand on the porous cellulose medium or cross-linked porous cellulose medium of the present disclosure. The adsorbent can also be used as a separation agent for affinity chromatography.
[0070] In the present disclosure, there are no particular restrictions on the method for producing a porous cellulose medium, as long as a porous cellulose medium that satisfies the aforementioned particle size and relationships (A) and (B) can be obtained, and the medium can be suitably produced by the production method shown in the following "2. Method for producing a porous cellulose medium".
[0071] 2. Method for producing porous cellulose medium
[0072] The method for producing a porous cellulose medium of the present disclosure is characterized in that it includes the following steps: a micronizing step of spraying a cellulose solution from a nozzle into a space to produce microparticles; and a coagulation step of coagulating the microparticles in a coagulation phase, wherein in the micronizing step, the gas supplied to the space where the cellulose solution is sprayed is controlled to be only the gas supplied from the nozzle together with the cellulose solution. By adopting such a production method, the porous cellulose medium of the present disclosure that satisfies the above-mentioned particle size and relations (A) and (B) can be suitably produced.
[0073] (Micro-refining process)
[0074] In the micronizing step, the cellulose solution is sprayed from a nozzle into a space to form microparticles. In the micronizing step, the gas supplied into the space where the cellulose solution is sprayed is controlled to be only the gas supplied from the nozzle together with the cellulose solution.
[0075] As a cellulose solution, there is no particular limitation as long as it is a liquid containing cellulose and coagulated in the coagulation phase described later. For example, it is a solution obtained by dissolving cellulose in a solvent. As a solvent, copper ethylenediamine solution, N-methylmorpholine oxide (NMMO) monohydrate, caustic alkali-urea aqueous solution, calcium thiocyanate aqueous solution, N, N'-dimethylacetamide solution of lithium chloride, dimethylformamide solution of lithium chloride, dimethylimidazolium solution of lithium chloride, dimethyl sulfoxide solution of lithium chloride, etc. can be cited. These solvents can be used only one, or two or more can be mixed and used. Among these, as a solvent, caustic alkali-urea aqueous solution (for example, urea-alkali hydroxide aqueous solution containing urea, thiourea, etc.) is preferred.
[0076] It should be noted that the so-called cellulose solution refers to a liquid containing cellulose that exhibits fluidity and solidifies when in contact with a coagulation phase. In the cellulose solution, any cellulose solution may be one in which cellulose molecules are dispersed, or in which a part of an aggregate remains, or in which only fine fibrous substances are dispersed (sometimes referred to as a dispersion). That is, in the method for producing a porous cellulose medium of the present disclosure, the so-called cellulose solution refers to a liquid containing cellulose, and is a concept that includes a dispersion in which cellulose is dispersed in a liquid and a solution in which cellulose is dissolved in a liquid. In the method for producing a porous cellulose medium of the present disclosure, it is sufficient that cellulose is contained in the cellulose solution, and its form may be any form of a dispersed state, a dissolved state, or a mixed state thereof.
[0077] Hereinafter, the method for preparing the cellulose solution will be specifically described by taking the case where a urea-alkali hydroxide aqueous solution is used as a solvent as an example.
[0078] The alkali contained in the aqueous alkali hydroxide solution is preferably lithium hydroxide, sodium hydroxide, potassium hydroxide, or quaternary ammonium hydroxide. Sodium hydroxide is most preferred in view of product safety, price, and good solubility or dispersion.
[0079] The alkali concentration of the alkali aqueous solution is not particularly limited, but is preferably 3 to 20% by mass. If the alkali concentration is within this range, the dispersibility, swelling and solubility of cellulose in the alkali aqueous solution are improved, which is preferred. The alkali concentration is more preferably 5 to 15% by mass, and even more preferably 6 to 10% by mass.
[0080] Urea or thiourea is further added to the above alkaline aqueous solution. The concentration of urea or thiourea is preferably 10 to 15% by mass. The three components (cellulose, alkali hydroxide, urea or thiourea) are added to water, but the order of addition is appropriately selected to optimize the dissolution state of cellulose. The slurry thus obtained is cooled under the conditions described below, thereby obtaining a more transparent cellulose solution than just after all the components are added.
[0081] The cellulose may be any cellulose as long as it becomes microparticles when sprayed from a nozzle in the form of a cellulose solution in the microparticle forming step and solidifies when in contact with a coagulation phase. However, from the viewpoints of excellent solubility, low viscosity of the solution and easy handling, so-called microcrystalline cellulose obtained by mild acid hydrolysis, cellulose regenerated from cellulose acetate by deacetylation, rayon fibers, etc. are preferred.
[0082] The molecular weight of cellulose is not particularly limited, but the degree of polymerization is preferably 1000 or less. If the degree of polymerization is 1000 or less, the dispersibility and swelling properties in an alkaline aqueous solution become high, which is preferred. In addition, if the degree of polymerization is 10 or more, the mechanical strength of the obtained cellulose beads becomes large, which is preferred. The more preferred range of the degree of polymerization is 50 or more and 500 or less, further preferably 100 or more and 400 or less, and particularly preferably 150 or more and 300 or less.
[0083] Furthermore, dissolving pulp can also be mentioned as an example of cellulose having improved solubility.
[0084] There are no particular restrictions on the mixing conditions of the aqueous alkali solution and cellulose as long as a cellulose solution can be obtained. For example, cellulose may be added to the aqueous alkali solution, or the aqueous alkali solution may be added to cellulose.
[0085] The cellulose may be pre-suspended in water before being mixed with the aqueous alkali solution.
[0086] In addition, the concentration of cellulose in the cellulose solution is preferably 1 to 10% by mass. If it is 1% by mass or more, the mechanical strength of the porous cellulose medium obtained becomes large, so it is preferred. If it is 10% by mass or less, the viscosity of the cellulose solution is low, and it is easy to spray from the nozzle in a manner of a predetermined particle size, so it is preferred. As the concentration of cellulose in the cellulose solution, 2 to 6% by mass is more preferred, and 3 to 5% by mass is further preferred. It should be noted that the cellulose concentration in the cellulose solution does not include the part that is not completely dissolved, dispersed, or swollen and has not become uniform.
[0087] The temperature when preparing the cellulose solution is not particularly limited. For example, the cellulose solution can be suitably formed by mixing an alkaline aqueous solution containing cellulose and urea or thiourea at room temperature, cooling at a low temperature while stirring, and then returning to a temperature that is easy to handle. As the temperature during low-temperature cooling, for example, 0°C to -30°C can be cited, and preferably -5°C to -15°C can be cited. In addition, from the viewpoint of further suitably producing the porous cellulose of the present disclosure that satisfies the aforementioned relationships (A) and (B) and has a specified particle size, the temperature of the cellulose solution sprayed from the nozzle is preferably about 0 to 50°C, and more preferably about 10 to 40°C. In addition, from the same viewpoint, the temperature of the space when the cellulose solution is sprayed from the nozzle into the space is preferably about 0 to 50°C, and more preferably about 10 to 40°C.
[0088] In the micronization process, the gas supplied to the space where the cellulose solution is sprayed is controlled to be only the gas supplied from the nozzle together with the cellulose solution. For example, the space where the cellulose solution is sprayed may be connected via an exhaust port, but the gas supplied from the nozzle to the space together with the cellulose solution may be controlled so that the gas is not supplied from the exhaust port to the outside, so that the gas supplied from the nozzle to the space together with the cellulose solution is led out to the outside via the exhaust port (that is, in the micronization process, the space where the cellulose solution is sprayed does not become a negative pressure side relative to the outside space). That is, the space where the cellulose solution is sprayed is isolated from the outside gas, and is a space where the concentration of the vapor of the solidified phase liquid is increased compared to an open system.
[0089] The gas supplied from the nozzle into the space together with the cellulose solution is preferably an inert gas, such as nitrogen, argon, etc. In addition, the gas supplied from the nozzle is preferably the same as the gas in the space.
[0090] From the viewpoint of further suitably manufacturing the porous cellulose medium of the present disclosure satisfying the aforementioned relationships (A) and (B) and having a specified particle size, the particle size of the cellulose solution sprayed from the nozzle is not particularly limited as long as the porous cellulose medium to be manufactured contains porous cellulose particles with a particle size of 1 to 600 μm, further 5 to 400 μm, and further 10 to 250 μm, and preferably is about 10 to 200 μm.
[0091] The nozzle is not particularly limited as long as it can spray a liquid with a particle size of about 10 to 200 μm, and a commercially available two-fluid nozzle, three-fluid nozzle, or the like can be used.
[0092] The micronization of the cellulose solution is preferably carried out by spraying the sprayed cellulose solution in a manner that causes it to fall due to gravity, from the perspective of the coagulation phase in the coagulation step described later. Specifically, it is preferred that the cellulose solution is sprayed from the nozzle into the space with the nozzle being arranged above the coagulation phase so that it contacts the coagulation phase by free fall due to gravity. From the perspective of further appropriately manufacturing the porous cellulose of the present disclosure that satisfies the aforementioned relationships (A) and (B) and has a specified particle size, the height from the surface of the coagulation phase to the front end of the nozzle is preferably 0.1m to 20m, and more preferably 1m to 20m.
[0093] (Solidification process)
[0094] In the coagulation step, the fine particles of the cellulose solution formed in the above-mentioned fine particle formation step are coagulated in a coagulation phase.
[0095] When the fine particles of the cellulose solution are coagulated in the coagulation phase, the fine particles of the cellulose solution are brought into contact with the coagulation phase as described above.
[0096] As the coagulation phase, a coagulation phase known as a substance for coagulating a cellulose solution can be used, for example, a liquid phase or a vapor phase of at least one selected from the group consisting of alcohol, ketone, ester, ether, water, inorganic acid, and inorganic salt aqueous solution, or a combination of a gas phase of an inert gas and the aforementioned liquid phase or vapor phase can be used. The components constituting the coagulation phase can be one or more. The coagulation phase is preferably composed of a component different from the solvent of the cellulose solution.
[0097] Among these, the solidified phase is preferably a liquid phase of water or alcohol, and a liquid phase of alcohol is particularly preferably used. In addition, a mixed solvent of water and alcohol (alcohol aqueous solution) is also preferably used.
[0098] The alcohol is not particularly limited, but is preferably an alcohol having 6 or less carbon atoms, more preferably an alcohol having 4 or less carbon atoms, and most preferably methanol.
[0099] The temperature of the coagulation phase is preferably about -30°C to 50°C, more preferably about -20°C to 40°C, from the viewpoint of more appropriately producing the porous cellulose of the present disclosure that satisfies the above-mentioned relationships (A) and (B) and has a predetermined particle size.
[0100] The obtained porous cellulose medium can be washed by an appropriate method using alcohol such as water, methanol, ethanol, etc., and is usually stored in a wet state. As mentioned above, when the porous cellulose medium is dried, a suitable amount of sugar, glycerol, etc. is added. When stored for a long time under wet conditions, a preservative such as alcohol or sodium azide is added to prevent corruption. In addition, it can also be dried in a state where glycerol, sugar, urea, etc. are added.
[0101] Example
[0102] The following are examples and comparative examples to explain the present disclosure in detail. However, each configuration and combination thereof in each embodiment is an example, and addition, omission, substitution, and other changes of the configuration may be appropriately made without departing from the scope of the present disclosure. The present disclosure is not limited by the examples, but only by the scope of the claims.
[0103] <Example 1>
[0104] (Preparation of cellulose solution)
[0105] In a flask, sodium hydroxide was dissolved in water, cooled to room temperature, and powdered cellulose (Asahi Kasei CEOLUS PH101, degree of polymerization: about 200) was dispersed therein while stirring. Urea was further added, dissolved, and then cooled to -15°C over about 1 hour while stirring, and then heated to room temperature using a water bath to form a nearly transparent solution. The amount of each reagent added was weighed and added so that sodium hydroxide was 7% by mass, powdered cellulose was 4% by mass, and urea was 12% by mass in the state of a cellulose solution.
[0106] (Micronization)
[0107] The obtained cellulose solution (temperature is 25°C) is sprayed vertically from top to bottom in a mist form together with nitrogen from a three-fluid nozzle (the particle size of the sprayed cellulose solution is about 10 to 200 μm), and is made to fall into liquid methanol (temperature is 25°C) as a solidified phase. The spraying space is a closed space (filled with nitrogen at a temperature of 25°C) except for the exhaust port from which the nitrogen flowing from the nozzle is released, and the liquid methanol is set below the three-fluid nozzle. A filter is set at the exhaust port to prevent the sprayed cellulose from leaking from the spraying space, and the spraying space is designed in a way that does not actively make the spraying space a negative pressure compared to the outside. After spraying, the fine powder obtained in the liquid methanol is recovered. The fine powder is passed through a sieve with a mesh of 250 μm and repeatedly washed with water on a sieve with a mesh of 10 μm, thereby obtaining a porous cellulose medium (particle size is 10 to 250 μm).
[0108] <Example 2>
[0109] A porous cellulose medium (particle size of 10 to 250 μm) was prepared by the same procedure as in Example 1 except that the powdered cellulose in Example 1 was regenerated cellulose and the cellulose concentration at the time of the cellulose solution was 3% by mass.
[0110] <Example 3>
[0111] A porous cellulose medium (particle size of 10 to 250 μm) was prepared by the same procedure as in Example 1, except that the powdered cellulose in Example 1 was changed to Nippon Paper KC FLOCK W-200 (polymerization degree of about 250) and the cellulose concentration at the time point of the cellulose solution was 3% by mass.
[0112] <Example 4>
[0113] A porous cellulose medium (particle size: 10 to 250 μm) was prepared by the same procedure as in Example 1 except that the spray nozzle in Example 1 was changed to a two-fluid nozzle.
[0114] <Example 5>
[0115] A porous cellulose medium (particle size: 10 to 250 μm) was prepared by the same procedure as in Example 1 except that the spray nozzle in Example 1 was a two-fluid nozzle of a different type from that in Example 4.
[0116] <Example 6>
[0117] A porous cellulose medium (particle size of 10 to 250 μm) was prepared by the same procedure as in Example 4, except that the composition of the liquid methanol provided below the nozzle in Example 4 was changed to a mixed liquid of equal amounts of water and methanol.
[0118] <Example 7>
[0119] A porous cellulose medium (particle size of 10 to 250 μm) was prepared by the same procedure as in Example 4 except that the sodium hydroxide in Example 4 was replaced with lithium hydroxide, the lithium hydroxide concentration at the time of the cellulose solution was 8 mass %, and the urea concentration was 15 mass %.
[0120] <Comparative Reference Example 1>
[0121] The gel partition coefficient K is read from the results (graph) shown in Example 2 of Patent Document 1. av and logMw values are plotted. Figure 5 Graph of the curve.
[0122] <Comparative Reference Example 2>
[0123] The gel partition coefficient K was calculated by reading the numerical value from the results (graph) shown in Example 3 of Patent Document 1. av and logMw values are plotted. Figure 5 Graph of the curve.
[0124] <Comparative Reference Example 3>
[0125] The gel partition coefficient K is read from the results (graph) shown in Example 4 of Patent Document 1. av and logMw values are plotted. Figure 5 Graph of the curve.
[0126] <Comparative Reference Example 4>
[0127] The gel partition coefficient K is read from the results (graph) shown in Example 5 of Patent Document 1. av and logMw values are plotted. Figure 5 Graph of the curve.
[0128] <Comparative Reference Example 5>
[0129] The gel partition coefficient K was calculated by reading the numerical value from the results (graph) shown in Example 7 of Patent Document 1. av and logMw values are plotted. Figure 5 Graph of the curve.
[0130] <Comparative Reference Example 6>
[0131] The gel partition coefficient K was calculated by reading the numerical value from the results (graph) shown in Example 8 of Patent Document 1. av and logMw values are plotted. Figure 5 Graph of the curve.
[0132] <Comparative Reference Example 7>
[0133] The gel partition coefficient K was calculated by reading the numerical value from the results (graph) shown in Patent Document 2 for Comparative Example 1. av and logMw values are plotted. Figure 6 Graph of the curve.
[0134] <Comparative Reference Example 8>
[0135] The gel partition coefficient K was calculated by reading the numerical value from the results (graph) shown in Example 4 of Patent Document 2. av and logMw values are plotted. Figure 6 Graph of the curve.
[0136] <Comparative Reference Example 9>
[0137] The gel partition coefficient K was calculated by reading the numerical value from the results (graph) shown in Example 1 of Patent Document 2. av and logMw values are plotted. Figure 6 Graph of the curve.
[0138] <Comparative Reference Example 10>
[0139] The gel partition coefficient K is read from the results (graph) shown in Patent Document 2 for Example 2. av and logMw values are plotted. Figure 6 Graph of the curve.
[0140] <Comparative Reference Example 11>
[0141] The gel partition coefficient K was calculated by reading the numerical value from the results (graph) shown in Patent Document 1 for Comparative Example 2. av and logMw values are plotted. Figure 6 Graph of the curve.
[0142] <Gel partition coefficient K av Determination of and calculation of its relationship with logMw>
[0143] The porous cellulose medium obtained in the example was classified with a sieve, and the fraction sandwiched between the sieves with mesh sizes of 53 μm and 106 μm was used as a support for size exclusion chromatography. Pure water was used as a mobile phase and standard polyethylene oxide was supplied to the size exclusion chromatography to determine the gel partition coefficient K. av . Specifically, the graded porous cellulose medium is filled into a column ("Tricorn 10 / 100" manufactured by GE Healthcare Japan Co., Ltd.) in such a way that the bed height becomes 8 cm or more. It is connected to a high performance liquid chromatography system to perform size exclusion chromatography. As markers, polyethylene oxide (TSKgel standard polyethylene oxide SE kit manufactured by TOSOH) and dextran (Blue Dextran 2000 manufactured by GE Healthcare) are dissolved in ultrapure water for use. While degassed ultrapure water is passed through the column at a flow rate of 0.1 mL / min, first, in order to determine the volume other than the bead portion in the column, a weight-average molecular weight of 2×10 6 The flow rate from the injection to the peak observed on the RI monitor was calculated using a solution of dextran (Blue dextran (GE Healthcare Blue Dextran 2000)). Next, the flow rate was calculated using the solutions of each marker in the same manner. The measured values were substituted into the following formula to calculate K av The value of .
[0144] K av =(V R -V0) / (V t -V0)
[0145] [Wherein, V Rrepresents the flow rate (mL) from the injection of each marker solution to the observation of the peak, V0 represents the flow rate from the injection of a marker solution with a weight average molecular weight of 2×10 6 The flow rate (mL) of the dextran solution from the beginning to the peak observation, V t Indicates the volume of beads in the column (mL). ]
[0146] The results are shown together with the straight lines for the preset values 1 to 7 shown below. Figures 1 to 4 It should be noted that, regarding Comparative Reference Examples 1 to 11, numerical values were also obtained from Patent Documents 1 and 2, and the gel partition coefficient K av The relationship between , and logMw is shown in Figure 5 , 6 .
[0147] Straight line with given value 1: When 4.80≤logMw≤5.50, K av =-0.445×logMw+2.55
[0148] Straight line of given value 2: When 5.75≤logMw, K av =0.19
[0149] Straight line of given value 3: When 4.80≤logMw≤5.50, K av =-0.521×logMw+2.97
[0150] Straight line of the given value 4: When 5.75≤logMw, K av =0.17
[0151] Straight line with a given value of 5: When 4.80≤logMw≤5.50, K av =-0.445×logMw+3
[0152] Straight line of the given value 6: When 5.75≤logMw, K av =-0.0482×logMw+0.3
[0153] Straight line with a given value of 7: When 4.80≤logMw≤5.50, K av =-0.521×logMw+3.2
Claims
1. A porous cellulose medium comprising porous cellulose particles having a particle size of 1 to 600 μm, wherein: The porous cellulose medium was classified with a sieve, and the fraction sandwiched between the sieves with mesh sizes of 53 μm and 106 μm was used as a support for size exclusion chromatography. When pure water was used as a mobile phase and standard polyethylene oxide was supplied to the size exclusion chromatography, the weight average molecular weight Mw of the standard polyethylene oxide and the gel partition coefficient K av The following relations (A) and (B) are satisfied: When 4.80≤logMw≤5.50, K av >-0.445×logMw+2.55(A) 5.75≤logMw, 0≤K av <0.19(B).
2. The porous cellulose medium according to claim 1, wherein The weight average molecular weight Mw and gel partition coefficient K of the standard polyethylene oxide av The following relationship (C) is satisfied: When 4.80≤logMw≤5.50, -0.445×logMw+3>K av >-0.445×logMw+2.55(C).
3. The method for producing a porous cellulose medium according to claim 1 or 2, comprising the following steps: a micronizing step of spraying the cellulose solution from a nozzle into the space to form microparticles; and a solidification step, wherein the particles are solidified in a solidification phase, In the micronizing step, the gas supplied to the space into which the cellulose solution is sprayed is controlled to include only the gas supplied from the nozzle together with the cellulose solution.
4. The method for producing a porous cellulose medium according to claim 3, wherein: The solvent of the cellulose solution is at least one selected from the group consisting of a copper ethylenediamine solution, N-methylmorpholine oxide (NMMO) monohydrate, a caustic soda-urea aqueous solution, a calcium thiocyanate aqueous solution, a lithium chloride N,N'-dimethylacetamide solution, a lithium chloride dimethylformamide solution, a lithium chloride dimethylimidazolium solution, and a lithium chloride dimethyl sulfoxide solution.
5. The method for producing a porous cellulose medium according to claim 3 or 4, wherein: The coagulated phase is composed of a component different from the solvent of the cellulose solution.
6. The method for producing a porous cellulose medium according to claim 3 or 4, wherein: The solidified phase is composed of a liquid phase or a vapor phase of at least one selected from the group consisting of alcohols, ketones, esters, ethers, water, inorganic acids, and inorganic salt aqueous solutions, or a combination of a gas phase of an inert gas and the liquid phase or vapor phase.