A bamboo-plastic composite board material for container bottom plate

By using a combination of materials such as modified bamboo pulp fiber and thermotropic liquid crystal polymer on the container floor, the problems of easy corrosion and insufficient impact resistance of materials in the existing technology have been solved, and a high-strength and waterproof bamboo plastic has been achieved. Composite board material extends service life.

CN113930039BActive Publication Date: 2024-10-01YIYANG TAOHUAJIANG BAMBOO PROD DEV CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111367039.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-18
Publication Date
2024-10-01
Estimated Expiration
2041-11-18

AI Technical Summary

Technical Problem

Existing container floor materials are susceptible to water vapor erosion and decay during transportation, have poor impact resistance, and have a short service life.

Method used

Bamboo plastic composite board materials including modified bamboo pulp fiber, HDPE, LLDPE, sarin resin, maleic anhydride grafted polypropylene and thermotropic liquid crystal polymer are used to modify the bamboo pulp fiber and thermotropic liquid crystal polymer through MMA grafting. Preparation method of liquid crystal polymer to form an ordered microfiber structure to improve mechanical properties and impact resistance.

Benefits of technology

The mechanical properties, tensile strength, notched impact strength and flexural strength of the bamboo-plastic composite board material are significantly improved, and the water absorption rate is low, and it has excellent waterproof and impact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003361044160000071
    Figure BDA0003361044160000071
  • Figure BDA0003361044160000081
    Figure BDA0003361044160000081
Patent Text Reader

Abstract

The present invention relates to the field of composite materials, in particular to a bamboo-plastic composite board material for container bottom plates, comprising the following components: modified bamboo pulp fiber, HDPE, LLDPE, sarin resin, maleic anhydride grafted polypropylene, polyethylene wax, and thermotropic liquid crystal polymer. Tests show that the bamboo-plastic composite board material prepared by the present invention has excellent mechanical properties, wherein the tensile strength is ≥66.5MPa and the notched impact strength is ≥23.4kJ·m ‑2 , bending strength ≥98.0MPa, and low water absorption, with excellent waterproof properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of composite materials, in particular to a bamboo-plastic composite board material for a container bottom plate. Background Art

[0002] Containers are widely used in various fields as a tool for loading and transporting goods and facilitating loading and unloading with mechanical equipment. The container floor, as a carrier for carrying goods, can be used to fix the goods and prevent the goods from directly scratching or colliding with the container during transportation. Currently, most container floors are made of wood or bamboo. Although they are cheap, they are not corrosion-resistant and are easily corroded and rotten by water vapor during sea transportation. Bamboo-plastic composite board materials have high strength and corrosion resistance, and are gradually being used to manufacture container floors. However, they have poor impact resistance and are easily damaged during loading and unloading of goods and transportation bumps, and have a short service life. Summary of the invention

[0003] Purpose of the invention: In view of the above technical problems, the present invention provides a bamboo-plastic composite board material for container bottom plates.

[0004] The technical solutions adopted are as follows:

[0005] A bamboo-plastic composite board material for a container bottom plate comprises the following components:

[0006] Modified bamboo pulp fiber, HDPE, LLDPE, Surlyn resin, maleic anhydride grafted polypropylene, polyethylene wax, thermotropic liquid crystal polymer.

[0007] Further, it comprises the following components in parts by weight:

[0008] 40-60 parts of modified bamboo pulp fiber, 25-30 parts of HDPE, 25-30 parts of LLDPE, 0.5-1 parts of sarling resin, 2-4 parts of maleic anhydride grafted polypropylene, 0.1-1 parts of polyethylene wax, and 5-10 parts of thermotropic liquid crystal polymer.

[0009] Furthermore, the modified bamboo pulp fiber is MMA grafted modified bamboo pulp fiber.

[0010] Furthermore, the preparation method of the MMA grafted modified bamboo pulp fiber is as follows:

[0011] S1: DMAP and triethylamine were added to THF, and nitrogen was introduced after stirring for 10-30 minutes. Then, bamboo pulp fiber was added, and stirring was continued for 10-30 minutes. Then, the reaction solution was cooled to ≤0°C, 2-bromoisobutyryl bromide was added, and the reaction was restored to room temperature for 10-30 minutes. Then, the temperature was raised to 60-65°C for reaction for 10-20 hours, and then filtered. The obtained solid was extracted with anhydrous ethanol for 8-10 hours and then dried to obtain an intermediate;

[0012] S2: Add copper bromide, pentamethyldiethylenetriamine and L-ascorbic acid into DMF, introduce nitrogen, stir evenly, then add MMA and the intermediate, react for 5-10 hours, filter, wash the obtained solid with water and anhydrous ethanol in turn, and dry.

[0013] Furthermore, the molar ratio of the copper bromide, pentamethyldiethylenetriamine and L-ascorbic acid is 1:2-2.1:3-3.1.

[0014] Furthermore, the preparation method of the thermotropic liquid crystal polymer is as follows:

[0015] S1: Under nitrogen protection, p-hydroxybenzoic acid, biphenol, terephthalic acid, isophthalic acid, acetic anhydride and magnesium acetate are mixed, the temperature is raised to 140-150°C for reaction for 3-4h in the first stage, the temperature is raised to 250-270°C for reaction for 30-40min in the second stage, the temperature is raised to 295-300°C for reaction for 30-40min in the third stage, the temperature is raised to 350-355°C for reaction for 30-40min in the fourth stage, and then vacuumized to 80-100Pa, kept warm for reaction for 1-3h, and returned to room temperature to obtain a prepolymer;

[0016] S2: After the prepolymer is dried, solid phase polymerization is carried out at 300-320°C under nitrogen protection until the system viscosity reaches 25-32 Pa·s, and then the temperature is restored to room temperature.

[0017] Furthermore, the molar ratio of p-hydroxybenzoic acid, biphenol, terephthalic acid and isophthalic acid is 10-12:3-4:3-4:1.

[0018] Furthermore, the first stage heating rate, the second stage heating rate, the third stage heating rate, and the fourth stage heating rate are the same or different, and are 1-2°C / min.

[0019] The present invention also provides a method for preparing a bamboo-plastic composite board material for a container bottom plate:

[0020] HDPE, LLDPE, maleic anhydride grafted polypropylene, thermotropic liquid crystal polymer and sarling resin are added into a twin-screw extruder for melt blending and granulation, the extruder speed is 40-50r / min, the temperature is 200-220°C, and then the same twin-screw extruder is used to melt blend and granulate the obtained blended pellets with modified bamboo pulp fiber and polyethylene wax, the extruder speed is 40-50r / min, the temperature is 195-198°C, and finally extruded through a single screw extruder.

[0021] Furthermore, the aspect ratio of the twin-screw extruder is 30-35, and the aspect ratio of the single-screw extruder is 40-45.

[0022] Beneficial effects of the present invention:

[0023] The invention provides a bamboo-plastic composite board material for a container bottom plate. HDPE has the advantages of high crystallinity, high Vicat softening point, high strength, etc., but its poor processing performance limits its application. LLDPE and HDPE have similar molecular structures. The two are blended to make up for the defect of poor processing performance of HDPE. Compared with bamboo powder, bamboo pulp fiber has a high aspect ratio and a complete fiber structure, which can give full play to the excellent mechanical reinforcement effect of bamboo. After being grafted and modified with MMA, it has better interface compatibility with HDPE and LLDPE. The mesogen units in the thermotropic liquid crystal polymer can be oriented to form an ordered The microfibers are fixed in the system network of the bamboo-plastic composite board material and produce two-phase separation. The microfibers can bear stress and disperse stress like the macro-fiber reinforced matrix, and the tight and loose network structure can also effectively absorb energy, disperse and buffer stress, and play a role in in-situ reinforcement and toughening, thereby improving the impact resistance. The sarling resin can play a role in volume expansion, improve the interface morphology, make the internal structure more compact, and enhance the mechanical properties. After testing, the bamboo-plastic composite board material prepared by the present invention has excellent mechanical properties, among which the tensile strength is ≥66.5MPa and the notched impact strength is ≥23.4kJ·m -2 , bending strength ≥98.0MPa, and low water absorption, with excellent waterproof properties. DETAILED DESCRIPTION

[0024] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0025] In the present invention, MMA is methyl methacrylate, HDPE is high-density polyethylene, LLDPE is linear low-density polyethylene, DMAP is 4-dimethylaminopyridine, THF is tetrahydrofuran, and DMF is N,N-dimethylformamide.

[0026] Embodiment 1:

[0027] A bamboo-plastic composite board material for a container bottom plate comprises the following components in parts by weight:

[0028] 60 parts of MMA grafted modified bamboo pulp fiber, 25 parts of HDPE, 25 parts of LLDPE, 0.5 parts of Surlyn resin, 2 parts of maleic anhydride grafted polypropylene, 0.5 parts of polyethylene wax, and 8 parts of thermotropic liquid crystal polymer.

[0029] The preparation method of MMA grafted modified bamboo pulp fiber is as follows:

[0030] 5 g DMAP and 15 mL triethylamine were added to 500 mL THF, stirred for 20 min, nitrogen was introduced, and 10 g bamboo pulp fiber was added. After continuing to stir for 20 min, the reaction solution was cooled to 0°C, 10 mL 2-bromoisobutyryl bromide was added, and the reaction was restored to room temperature for 20 min. The temperature was raised to 65°C and the reaction was performed for 20 h before filtering. The obtained solid was extracted with anhydrous ethanol for 10 h and dried to obtain 12 g of the intermediate. Copper bromide, pentamethyldiethylenetriamine and L-ascorbic acid in a molar ratio of 1:2:3 were added to DMF, nitrogen was introduced, and the mixture was stirred evenly. Then MMA and the intermediate were added. The reaction was performed for 10 h and the mixture was filtered. The obtained solid was washed with water and anhydrous ethanol in turn and dried.

[0031] The preparation method of thermotropic liquid crystal polymer is as follows:

[0032] Under nitrogen protection, p-hydroxybenzoic acid, biphenol, terephthalic acid, isophthalic acid, acetic anhydride and magnesium acetate in a molar ratio of 10:3:3:1 are mixed, the temperature is raised to 145°C for reaction for 4h in the first stage, the temperature is raised to 270°C for reaction for 40min in the second stage, the temperature is raised to 300°C for reaction for 40min in the third stage, the temperature is raised to 355°C for reaction for 30min in the fourth stage, and then vacuumed to 100Pa, kept warm for reaction for 2h, and returned to room temperature to obtain a prepolymer, wherein the first stage heating rate, the second stage heating rate, the third stage heating rate and the fourth stage heating rate are the same, all of which are 1.5°C / min. After the prepolymer is dried, solid-phase polymerization is carried out at 320°C under nitrogen protection until the viscosity of the system reaches 30Pa·s, and then the room temperature is returned.

[0033] Preparation method of the above-mentioned bamboo-plastic composite board material for container bottom plate:

[0034] HDPE, LLDPE, maleic anhydride grafted polypropylene, thermotropic liquid crystal polymer, and sarling resin are added to a twin-screw extruder with an aspect ratio of 30 for melt blending and granulation. The extruder speed is 50r / min and the temperature is 220°C. The same twin-screw extruder is then used to melt blend and granulate the obtained blended pellets with modified bamboo pulp fiber and polyethylene wax. The extruder speed is 40r / min and the temperature is 198°C. Finally, the mixture is extruded through a single screw extruder with an aspect ratio of 45.

[0035] Embodiment 2:

[0036] The method is basically the same as Example 1, except that the prepared bamboo-plastic composite board material for container bottom plate includes the following components in parts by weight:

[0037] 60 parts of MMA grafted modified bamboo pulp fiber, 30 parts of HDPE, 30 parts of LLDPE, 0.5 parts of Surlyn resin, 4 parts of maleic anhydride grafted polypropylene, 1 part of polyethylene wax, and 10 parts of thermotropic liquid crystal polymer.

[0038] Embodiment 3:

[0039] The method is basically the same as Example 1, except that the prepared bamboo-plastic composite board material for container bottom plate includes the following components in parts by weight:

[0040] 40 parts of MMA grafted modified bamboo pulp fiber, 25 parts of HDPE, 25 parts of LLDPE, 0.5 parts of Surlyn resin, 2 parts of maleic anhydride grafted polypropylene, 0.1 parts of polyethylene wax, and 5 parts of thermotropic liquid crystal polymer.

[0041] Embodiment 4:

[0042] The method is basically the same as Example 1, except that the prepared bamboo-plastic composite board material for container bottom plate includes the following components in parts by weight:

[0043] 40 parts of MMA grafted modified bamboo pulp fiber, 30 parts of HDPE, 25 parts of LLDPE, 0.5 parts of Surlyn resin, 4 parts of maleic anhydride grafted polypropylene, 0.1 parts of polyethylene wax, and 10 parts of thermotropic liquid crystal polymer.

[0044] Embodiment 5:

[0045] The method is basically the same as Example 1, except that the prepared bamboo-plastic composite board material for container bottom plate includes the following components in parts by weight:

[0046] 60 parts of MMA grafted modified bamboo pulp fiber, 25 parts of HDPE, 30 parts of LLDPE, 0.5 parts of Surlyn resin, 2 parts of maleic anhydride grafted polypropylene, 1 part of polyethylene wax, and 5 parts of thermotropic liquid crystal polymer.

[0047] Comparative Example 1:

[0048] The method is basically the same as Example 1, except that the bamboo pulp fiber is not subjected to MMA grafting modification treatment.

[0049] Comparative Example 2:

[0050] The method is basically the same as Example 1, except that no thermotropic liquid crystal polymer is added.

[0051] Comparative Example 3:

[0052] The method is substantially the same as Example 1, except that no sarling resin is added.

[0053] Performance Test:

[0054] The bamboo-plastic composite board materials prepared in Examples 1-5 and Comparative Examples 1-3 of the present invention were used as samples, and the tensile strength of the samples was tested according to GB / T1040.1-2006 standard, and the cantilever beam notched impact strength of the samples was tested according to GB / T1043.1-2008 standard; the bending strength test was carried out according to LY / T 2565-2015 standard;

[0055] Determination of water absorption rate: Weigh a certain mass (recorded as m1) of bamboo-plastic composite board material particles, soak them in water for a certain period of time at room temperature, take them out, dry the surface water with absorbent paper, and weigh them again (recorded as m2). Calculate the water absorption rate of the bamboo-plastic composite material according to the following formula:

[0056] Water absorption rate = [(m2-m1) / m1] × 100%

[0057] The test results are shown in Table 1 below:

[0058] Table 1:

[0059]

[0060]

[0061] As shown in Table 1 above, the bamboo-plastic composite board material prepared by the present invention has excellent mechanical properties, wherein the tensile strength is ≥66.5MPa and the notched impact strength is ≥23.4kJ·m -2 , bending strength ≥98.0MPa, and low water absorption, with excellent waterproof properties.

[0062] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A bamboo-plastic composite board material for container bottom plate, It is characterized in that The composition comprises the following components in parts by weight: 40-60 parts of modified bamboo pulp fiber, 25-30 parts of HDPE, 25-30 parts of LLDPE, 0.5-1 parts of sarling resin, 2-4 parts of maleic anhydride grafted polypropylene, 0.1-1 parts of polyethylene wax, 5-10 parts of thermotropic liquid crystal polymer; The modified bamboo pulp fiber is MMA grafted modified bamboo pulp fiber; The preparation method of the MMA grafted modified bamboo pulp fiber is as follows: S1: DMAP and triethylamine were added to THF, and nitrogen was introduced after stirring for 10-30 minutes. Then, bamboo pulp fiber was added, and stirring was continued for 10-30 minutes. Then, the reaction solution was cooled to ≤0°C, 2-bromoisobutyryl bromide was added, and the reaction was restored to room temperature for 10-30 minutes. Then, the temperature was raised to 60-65°C for reaction for 10-20 hours, and then filtered. The obtained solid was extracted with anhydrous ethanol for 8-10 hours and then dried to obtain an intermediate; S2: Add copper bromide, pentamethyldiethylenetriamine and L-ascorbic acid to DMF, introduce nitrogen, stir evenly, then add MMA and the intermediate, react for 5-10 hours, filter, wash the obtained solid with water and anhydrous ethanol in turn, and dry; The molar ratio of copper bromide, pentamethyldiethylenetriamine and L-ascorbic acid is 1:2-2.1:3-3.1; The preparation method of the thermotropic liquid crystal polymer is as follows: S1: Under nitrogen protection, p-hydroxybenzoic acid, biphenol, terephthalic acid, isophthalic acid, acetic anhydride and magnesium acetate are mixed, the temperature is raised to 140-150°C for reaction for 3-4h in the first stage, the temperature is raised to 250-270°C for reaction for 30-40min in the second stage, the temperature is raised to 295-300°C for reaction for 30-40min in the third stage, the temperature is raised to 350-355°C for reaction for 30-40min in the fourth stage, and then vacuumized to 80-100Pa, kept warm for reaction for 1-3h, and returned to room temperature to obtain a prepolymer; S2: After the prepolymer is dried, solid phase polymerization is carried out at 300-320°C under nitrogen protection until the system viscosity reaches 25-32 Pa·s, and then the mixture is returned to room temperature; The molar ratio of p-hydroxybenzoic acid, biphenol, terephthalic acid and isophthalic acid is 10-12:3-4:3-4:1; The first stage heating rate, the second stage heating rate, the third stage heating rate and the fourth stage heating rate are the same or different, and are 1-2°C / min; The preparation method of the bamboo-plastic composite board material for the container bottom plate is as follows: HDPE, LLDPE, maleic anhydride grafted polypropylene, thermotropic liquid crystal polymer and sarling resin are added into a twin-screw extruder for melt blending and granulation, the extruder speed is 40-50r / min, the temperature is 200-220°C, and then the same twin-screw extruder is used to melt blend and granulate the obtained blended pellets with modified bamboo pulp fiber and polyethylene wax, the extruder speed is 40-50r / min, the temperature is 195-198°C, and finally extruded through a single screw extruder.

2. The bamboo-plastic composite board material for container bottom plate according to claim 1, It is characterized in that The length-to-diameter ratio of the twin-screw extruder is 30-35, and the length-to-diameter ratio of the single-screw extruder is 40-45.

Citation Information

Patent Citations

  • Thermotropic high-polymer liquid crystal reinforced / toughened polyolefin-base wood-plastic composite material and preparation method thereof

    CN104530739A

  • Preparation method for resin-based bamboo fiber composite material

    CN104788889A