A semiconductor transistor and a method for manufacturing the same
By using the combination of the third generation GaN/AlGaN material and silicon-based MOSFET in semiconductor transistors, the 2DEG conductive channel and N-i-P-i-N structure are used to solve the problems of voltage withstandness and process complexity in the prior art, and the breakdown voltage and Electronic mobility improves the frequency and rate performance of the device.
Patent Information
- Application Number
- CN202111188640.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-10-12
AI Technical Summary
Existing semiconductor transistors have shortcomings in voltage withstandness and process complexity, especially device design methods based on gallium nitride materials, resulting in complex production processes and limited improvement in voltage withstandness.
The third-generation semiconductor GaN/AlGaN, etc. are used as epitaxial layer materials, combined with the design advantages of silicon-based MOSFET and gallium nitride material HEMT, and the P-type and N-type regions are formed by doping, and the 2DEG on the surface of heterojunction material is used as the conductive channel. , and an N-i-P-i-N structure is formed when no voltage is applied to the gate, and an electrically conductive channel is formed by attracting electrons through an electric field to increase the breakdown voltage and electron mobility.
The breakdown voltage characteristics and electron mobility of semiconductor transistors are improved, the corresponding switching rate and frequency are improved, and the shortcomings of silicon-based materials in electron mobility, high voltage resistance and working temperature characteristics are solved.
Smart Images

Figure CN113948569B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor electronic information technology, and more particularly to a semiconductor transistor and a method for preparing the same. Background Art
[0002] With the development of semiconductor materials, the design and methods of transistors have been continuously improved. At present, the third-generation wide bandgap semiconductors have been widely used in the semiconductor field with their wide bandgap constant, higher electron mobility, strong radiation resistance, good breakdown electric field strength, high temperature resistance and other characteristics. Their chips have the characteristics of high reverse blocking voltage, low forward on-resistance, high operating frequency, etc. They are very ideal materials, especially based on the two-dimensional electron gas (2DEG) structure, so that the devices manufactured have very high electron mobility.
[0003] At present, the manufacturing process of silicon-based MOSFET is very mature, and silicon-based products also have huge advantages in price. Compared with materials such as the third-generation GaN, silicon lacks electron mobility, high voltage resistance and operating temperature characteristics. Based on the third-generation semiconductor material GaN, devices such as HEMT (or heterojunction field effect transistor HFET, modulation doped field effect transistor MODFET) have been developed and have achieved good results, but there are also problems such as low gate voltage resistance and complex process.
[0004] Therefore, how to combine the advantages of existing device structures and materials to obtain more optimized semiconductor transistors and their preparation methods is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0005] In view of this, the present invention provides a new semiconductor electronic transistor structure and manufacturing method, using (Si) silicon base or (SiC) silicon carbide as a substrate, using third-generation semiconductor GaN / AlGaN as an epitaxial layer material, combining the transistor design advantages and material advantages of silicon-based MOSFET and gallium nitride material HEMT, to form a new electronic transistor with excellent characteristics.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] A semiconductor transistor comprises an epitaxial layer, an S / D electrode region, a silicon dioxide layer and a G electrode;
[0008] Wherein, the S / D electrode region and the silicon dioxide layer are both located above the epitaxial layer, and the G electrode is located above the silicon dioxide layer;
[0009] The epitaxial layer includes a substrate and a GaN layer, a P-GaN layer, an i-GaN layer, an i-AlN layer and an n-AlGaN layer sequentially located above the substrate;
[0010] The S / D electrode region includes an S electrode and a D electrode, the S electrode and the D electrode are respectively located at two ends of the n-AlGaN layer, and the bottom thereof penetrates through the n-AlGaN layer and contacts the top surface of the i-AlN layer;
[0011] The silicon dioxide layer is located in the middle of the n-AlGaN layer, and the bottom thereof penetrates through the n-AlGaN layer and contacts with the top surface of the i-AlN layer.
[0012] Preferably, the above-mentioned semiconductor transistor further includes: a protective layer; the protective layer is arranged above the n-AlGaN layer and the silicon dioxide layer outside the S electrode, the D electrode and the G electrode, and both sides of the S electrode and the D electrode are covered by the protective layer.
[0013] Preferably, the substrate material is Si or SiC.
[0014] Preferably, the GaN layer has a thickness of 10-30 nm.
[0015] More preferably, the GaN layer includes a first GaN layer with a thickness of 5-20 nm and a second GaN layer with a thickness of 5-10 nm.
[0016] Preferably, the P-GaN layer includes a layer with a magnesium doping concentration of 10 15 -10 17 cm -3 The first P-GaN layer and a layer of magnesium doping concentration of 10 17 -10 20 cm -3 the thickness of the first P-GaN layer is 5-10 nm; the thickness of the second P-GaN layer is 200-300 nm.
[0017] Preferably, the thickness of the i-GaN layer is 2-3 nm.
[0018] Preferably, the thickness of the i-AlN layer is 1-2 nm.
[0019] Preferably, the thickness of the n-AlGaN layer is 20-40 nm.
[0020] More preferably, the n-AlGaN is n-AlGaN doped with silane, and the doping concentration of silane is about 10 19 -10 22 cm -3 .
[0021] Another object of the present invention is to provide a method for preparing the above-mentioned semiconductor transistor, comprising the following steps:
[0022] (1) growing a GaN layer, a P-GaN layer, an i-GaN layer, an i-AlN layer and an n-AlGaN layer in sequence on a substrate;
[0023] (2) etching an S electrode groove and a D electrode groove at both ends of the n-AlGaN layer, and etching a G electrode groove in the middle of the n-AlGaN layer;
[0024] (3) plating a layer of Ti / Al / Ni / Au metal alloy layer in the S electrode groove and the D electrode groove to obtain an S electrode and a D electrode;
[0025] (4) Plating a layer of silicon dioxide in the G electrode groove;
[0026] (5) coating a Ni / Au metal alloy layer on the silicon dioxide layer to obtain a G electrode;
[0027] (6) A protective layer is plated on the n-AlGaN layer and the silicon dioxide layer other than the S electrode, the D electrode and the G electrode, and both sides of the S electrode and the D electrode are covered by the protective layer.
[0028] Preferably, the thickness of each metal layer in the Ti / Al / Ni / Au metal alloy layer in step (3) is Ti: 10-50nm; Al: 150-300nm; Ni: 100-200nm; Au: 150-300nm;
[0029] The thickness of the silicon dioxide layer in step (4) is 10-30 nm;
[0030] The thickness of each metal layer in the Ni / Au metal alloy layer in step (5) is Ni: Au:
[0031] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0032] Through the brief description of the background technology, it can be seen that both silicon-based materials and gallium nitride materials have some characteristics of their own, so silicon-based transistors have great advantages in terms of price and manufacturing process, but first of all, due to the characteristics of the material itself, the electron mobility and high voltage resistance and operating temperature characteristics are received. At present, the electron mobility, strong radiation resistance, good breakdown electric field strength, high temperature resistance and other characteristics of gallium nitride materials are very good, but the current design method of devices based on gallium nitride makes the manufacturing process complicated, and there are also problems such as limited improvement in pressure resistance. The present invention uses the third-generation semiconductor gallium nitride and its compounds as epitaxial materials, and forms P-type and In the N-type region, the 2DEG on the surface of the heterojunction material is used as a conductive channel, and metal and oxide are used as the gate. When no voltage is applied to the gate, the source and drain are equivalent to a NiPiN structure and cannot be turned on. By applying voltage to the gate, the electrons in the N-AlGaN under the source and drain are attracted to the surface layer by the electric field, and the 2DEG formed by the AlGaN / GaN at the source and drain forms a conductive channel. The NiPiN structure can increase the breakdown voltage and improve the product voltage characteristics. The conductive channel of 2DEG can improve the electron mobility. Compared with the multi-sub conductive channel of the semiconductor itself, it improves the switching response rate and frequency. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0034] Figure 1 This is a diagram of the semiconductor transistor structure of the present invention.
[0035] Among them, in the figure:
[0036] 1. Substrate; 2. GaN layer; 3. P-GaN layer; 4. i-GaN layer; 5. i-AlN layer; 6. n-AlGaN layer; 7. S electrode; 8. D electrode; 9. Silicon dioxide layer; 10. G electrode; 11. Protective layer. DETAILED DESCRIPTION
[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Example 1
[0039] A semiconductor transistor comprises an epitaxial layer, an S / D electrode region, a silicon dioxide layer 9 and a G electrode 10;
[0040] The S / D electrode regions and the silicon dioxide layer 9 are both located above the epitaxial layer, and the G electrode 10 is located above the silicon dioxide layer 9;
[0041] The epitaxial layer includes a substrate 1 and a GaN layer 2, a P-GaN layer 3, an i-GaN layer 4, an i-AlN layer 5 and an n-AlGaN layer 6 which are sequentially located on the substrate 1;
[0042] The S / D electrode region includes an S electrode 7 and a D electrode 8, the S electrode 7 and the D electrode 8 are respectively located at two ends of the n-AlGaN layer 6, and the bottom thereof penetrates through the n-AlGaN layer 6 and contacts the top surface of the i-AlN layer 5;
[0043] The silicon dioxide layer 9 is located in the middle of the n-AlGaN layer 6, and the bottom thereof penetrates through the n-AlGaN layer 6 and contacts the top surface of the i-AlN layer 5;
[0044] In this embodiment, it further includes: a protective layer 11; the protective layer 11 is disposed above the n-AlGaN layer 6 and the silicon dioxide layer 9 other than the S electrode 7, the D electrode 8 and the G electrode 10, and both sides of the S electrode 7 and the D electrode 8 are covered by the protective layer 11;
[0045] In this embodiment, the material of substrate 1 is Si;
[0046] In this embodiment, the GaN layer 2 includes a first GaN layer with a thickness of 20 nm and a second GaN layer with a thickness of 10 nm;
[0047] In this embodiment, the P-GaN layer 3 includes a layer of magnesium doping concentration of 10 17 cm -3 The first P-GaN layer and a layer of magnesium doping concentration of 10 20 cm -3 The thickness of the first P-GaN layer is 10 nm; the thickness of the second P-GaN layer is 300 nm;
[0048] In this embodiment, the thickness of the i-GaN layer 4 is 3 nm;
[0049] In this embodiment, the thickness of the i-AlN layer 5 is 2 nm;
[0050] In this embodiment, the thickness of the n-AlGaN layer 6 is 40 nm; the doping concentration of silane in the n-AlGaN is 10 22 cm -3 ;
[0051] In this embodiment, the thickness of the silicon dioxide layer 9 is 30 nm;
[0052] In this embodiment, the materials of the S electrode 7 and the D electrode 8 are both Ti / Al / Ni / Au metal alloy layers, and the thickness of each metal layer is respectively Ti: 50nm; Al: 300nm; Ni: 200nm; Au: 300nm;
[0053] In this embodiment, the material of the G electrode 10 is a Ni / Au metal alloy layer, and the thickness of each metal layer is Ni: Au:
[0054] Example 2
[0055] A semiconductor transistor comprises an epitaxial layer, an S / D electrode region, a silicon dioxide layer 9 and a G electrode 10;
[0056] The S / D electrode regions and the silicon dioxide layer 9 are both located above the epitaxial layer, and the G electrode 10 is located above the silicon dioxide layer 9;
[0057] The epitaxial layer includes a substrate 1 and a GaN layer 2, a P-GaN layer 3, an i-GaN layer 4, an i-AlN layer 5 and an n-AlGaN layer 6 which are sequentially located on the substrate 1;
[0058] The S / D electrode region includes an S electrode 7 and a D electrode 8, the S electrode 7 and the D electrode 8 are respectively located at two ends of the n-AlGaN layer 6, and the bottom thereof penetrates through the n-AlGaN layer 6 and contacts the top surface of the i-AlN layer 5;
[0059] The silicon dioxide layer 9 is located in the middle of the n-AlGaN layer 6, and the bottom thereof penetrates through the n-AlGaN layer 6 and contacts the top surface of the i-AlN layer 5;
[0060] In this embodiment, it further includes: a protective layer 11; the protective layer 11 is disposed above the n-AlGaN layer 6 and the silicon dioxide layer 9 other than the S electrode 7, the D electrode 8 and the G electrode 10, and both sides of the S electrode 7 and the D electrode 8 are covered by the protective layer 11;
[0061] In this embodiment, the material of substrate 1 is Si;
[0062] In this embodiment, the GaN layer 2 includes a first GaN layer with a thickness of 5 nm and a second GaN layer with a thickness of 5 nm;
[0063] In this embodiment, the P-GaN layer 3 includes a layer of magnesium doping concentration of 10 15 cm -3 The first P-GaN layer and a layer of magnesium doping concentration of 10 17 cm-3 The thickness of the first P-GaN layer is 5 nm; the thickness of the second P-GaN layer is 200 nm;
[0064] In this embodiment, the thickness of the i-GaN layer 4 is 2 nm;
[0065] In this embodiment, the thickness of the i-AlN layer 5 is 1 nm;
[0066] In this embodiment, the thickness of the n-AlGaN layer 6 is 20 nm; the doping concentration of silane in the n-AlGaN is 10 19 cm -3 ;
[0067] In this embodiment, the thickness of the silicon dioxide layer 9 is 10 nm;
[0068] In this embodiment, the materials of the S electrode 7 and the D electrode 8 are both Ti / Al / Ni / Au metal alloy layers, and the thickness of each metal layer is respectively Ti: 10nm; Al: 150nm; Ni: 100nm; Au: 150nm;
[0069] In this embodiment, the material of the G electrode 10 is a Ni / Au metal alloy layer, and the thickness of each metal layer is Ni: Au:
[0070] Example 3
[0071] A semiconductor transistor comprises an epitaxial layer, an S / D electrode region, a silicon dioxide layer 9 and a G electrode 10;
[0072] The S / D electrode regions and the silicon dioxide layer 9 are both located above the epitaxial layer, and the G electrode 10 is located above the silicon dioxide layer 9;
[0073] The epitaxial layer includes a substrate 1 and a GaN layer 2, a P-GaN layer 3, an i-GaN layer 4, an i-AlN layer 5 and an n-AlGaN layer 6 which are sequentially located on the substrate 1;
[0074] The S / D electrode region includes an S electrode 7 and a D electrode 8, the S electrode 7 and the D electrode 8 are respectively located at two ends of the n-AlGaN layer 6, and the bottom thereof penetrates through the n-AlGaN layer 6 and contacts the top surface of the i-AlN layer 5;
[0075] The silicon dioxide layer 9 is located in the middle of the n-AlGaN layer 6, and the bottom thereof penetrates through the n-AlGaN layer 6 and contacts the top surface of the i-AlN layer 5;
[0076] In this embodiment, it further includes: a protective layer 11; the protective layer 11 is disposed above the n-AlGaN layer 6 and the silicon dioxide layer 9 other than the S electrode 7, the D electrode 8 and the G electrode 10, and both sides of the S electrode 7 and the D electrode 8 are covered by the protective layer 11;
[0077] In this embodiment, the substrate 1 is made of SiC;
[0078] In this embodiment, the GaN layer 2 includes a first GaN layer with a thickness of 10 nm and a second GaN layer with a thickness of 8 nm;
[0079] In this embodiment, the P-GaN layer 3 includes a layer of magnesium doping concentration of 10 16 cm -3 The first P-GaN layer and a layer of magnesium doping concentration of 10 18 cm -3 The thickness of the first P-GaN layer is 7 nm; the thickness of the second P-GaN layer is 250 nm;
[0080] In this embodiment, the thickness of the i-GaN layer 4 is 2 nm;
[0081] In this embodiment, the thickness of the i-AlN layer 5 is 2 nm;
[0082] In this embodiment, the thickness of the n-AlGaN layer 6 is 30 nm; the doping concentration of silane in the n-AlGaN is 10 21 cm -3 ;
[0083] In this embodiment, the thickness of the silicon dioxide layer 9 is 20 nm;
[0084] In this embodiment, the materials of the S electrode 7 and the D electrode 8 are both Ti / Al / Ni / Au metal alloy layers, and the thickness of each metal layer is Ti: 30nm; Al: 200nm; Ni: 150nm; Au: 200nm;
[0085] In this embodiment, the material of the G electrode 10 is a Ni / Au metal alloy layer, and the thickness of each metal layer is Ni: Au:
[0086] Example 4
[0087] The method for preparing the semiconductor transistor in Embodiment 1-3 comprises the following steps:
[0088] The present invention uses metal organic chemical vapor deposition (MOCVD) epitaxial growth technology, and adopts trimethyl gallium (TMGa), triethyl gallium (TEGa), trimethyl aluminum (TMAl) and ammonia (NH3), silane (SiH4) and bismuth magnesium (CpMg), nitrogen and hydrogen to provide gallium source, aluminum source and nitrogen source, silicon source, magnesium source and carrier gas required for growth, and the specific operation is as follows:
[0089] (1) The substrate was ultrasonically cleaned in acetone and ethanol for 4 minutes each, then rinsed with deionized water and dried in an oven;
[0090] (2) Place the treated substrate in an MOCVD device and bake at 1200°C for 15 minutes; cool to 500°C, introduce trimethylgallium (TMGa) and ammonia (NH3) at a pressure of 150 torr to grow a first GaN layer;
[0091] (3) Then the temperature is raised to 1020°C, and trimethylgallium (TMGa) and ammonia (NH3) are introduced at a pressure of 250 torr to grow the second GaN.
[0092] (4) Then, a first magnesium-doped P-GaN layer is grown by introducing CpMg, trimethylgallium (TMGa) and ammonia (NH3) at 1000°C and a pressure of 250 torr;
[0093] (5) Then, at a temperature of 980°C and a pressure of 230 torr, bismuthocene magnesium (CpMg), trimethylgallium (TMGa) and ammonia (NH3) are continuously introduced to grow a second P-GaN layer doped with magnesium;
[0094] (6) The temperature is then raised to 1020°C, and trimethylgallium (TMGa) and ammonia (NH3) are introduced at a pressure of 250 torr to grow a layer of undoped intrinsic i-GaN;
[0095] (7) The temperature is then raised to 1050°C, and trimethylaluminum (TMAl) and ammonia (NH3) are introduced at a pressure of 200 torr to grow a layer of undoped intrinsic i-AlN;
[0096] (8) The temperature is then raised to 1030°C, and trimethylgallium (TMGa), trimethylaluminum (TMAl) and ammonia (NH3) silane (SiH4) are introduced at a pressure of 250 torr to grow a layer of silane-doped n-AlGaN;
[0097] (9) Then, nitrogen gas was introduced at 950°C for annealing for 15 minutes;
[0098] (10) applying photoresist, and etching the electrode regions of the source S (S electrode), the gate G (G electrode), and the drain D (D electrode) by ICP through a photolithography MESA process, with the etching depth reaching the contact position between the n-AlGaN layer and the i-AlN layer;
[0099] (11) Applying photoresist, using MESA process, using the SD photolithography board with S electrode and D electrode to produce electrode patterns, and transferring the S and D electrode patterns to the two ends of the upper surface;
[0100] (12) using electron beam evaporation to deposit metal, coating a layer of Ti / Al / Ni / Au metal at the S and D electrode patterns to form a Ti / Al / Ni / Au metal combination, and forming an S electrode and a D electrode by a metal lift-off process;
[0101] (13) After cleaning with a degumming solution and deionized water, the G electrode region located in the middle of the n-AlGaN layer is formed by a photolithography MESA process, and the etching depth is up to the contact position between the n-AlGaN layer and the i-AlN layer.
[0102] (14) Then a layer of silicon dioxide (SiO2) oxide is deposited on the G electrode region by PECVD;
[0103] (15) Then, a G electrode pattern is produced on the G electrode area coated with SiO2 oxide by using a photomask with a G electrode pattern combined with a photolithography MESA process;
[0104] (16) Then, an electron beam evaporation process is used to evaporate metal Ni / Au respectively, and then the metal on the other evaporated area layers is stripped by a metal stripping technique to leave the G area metal, thereby forming a G electrode, and the G electrode is located on the SiO2 oxide;
[0105] (17) Then, combined with the MESA process, a SiO 2 passivation layer protection layer was grown on the surface using PECVD, covering all areas except the three electrode areas.
[0106] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0107] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A semiconductor transistor, characterized in that: It includes an epitaxial layer, an S / D electrode region, a silicon dioxide layer and a G electrode; Wherein, the S / D electrode region and the silicon dioxide layer are both located above the epitaxial layer, and the G electrode is located above the silicon dioxide layer; The epitaxial layer includes a substrate and a GaN layer, a P-GaN layer, an i-GaN layer, an i-AlN layer and an n-AlGaN layer sequentially located above the substrate; The S / D electrode region includes an S electrode and a D electrode, the S electrode and the D electrode are respectively located at two ends of the n-AlGaN layer, and the bottom thereof penetrates through the n-AlGaN layer and contacts the top surface of the i-AlN layer; The silicon dioxide layer is located in the middle of the n-AlGaN layer, and the bottom thereof penetrates through the n-AlGaN layer and contacts the top surface of the i-AlN layer; It also includes: a protective layer; the protective layer is arranged above the n-AlGaN layer and the silicon dioxide layer other than the S electrode, the D electrode and the G electrode, and both sides of the S electrode and the D electrode are covered by the protective layer; The P-GaN layer includes a layer of magnesium doping concentration of 10 15 -10 17 cm -3 The first P-GaN layer and a layer of magnesium doping concentration of 10 17 -10 20 cm -3 the thickness of the first P-GaN layer is 5-10 nm; the thickness of the second P-GaN layer is 200-300 nm.
2. A semiconductor transistor according to claim 1, characterized in that: The substrate material is Si or SiC.
3. A semiconductor transistor according to claim 2, characterized in that: The thickness of the GaN layer is 10-30 nm.
4. A semiconductor transistor according to claim 2, characterized in that: The thickness of the i-GaN layer is 2-3 nm.
5. A semiconductor transistor according to claim 2, characterized in that: The thickness of the i-AlN layer is 1-2 nm.
6. A semiconductor transistor according to claim 2, characterized in that: The thickness of the n-AlGaN layer is 20-40 nm.
7. A method for preparing a semiconductor transistor according to any one of claims 2 to 6, characterized in that: The following steps are involved: (1) growing a GaN layer, a P-GaN layer, an i-GaN layer, an i-AlN layer and an n-AlGaN layer in sequence on a substrate; (2) etching an S electrode groove and a D electrode groove at both ends of the n-AlGaN layer, and etching a G electrode groove in the middle of the n-AlGaN layer; (3) plating a layer of Ti / Al / Ni / Au metal alloy layer in the S electrode groove and the D electrode groove to obtain an S electrode and a D electrode; (4) Plating a layer of silicon dioxide in the G electrode groove; (5) coating a Ni / Au metal alloy layer on the silicon dioxide layer to obtain a G electrode; (6) A protective layer is plated on the n-AlGaN layer and the silicon dioxide layer other than the S electrode, the D electrode and the G electrode, and both sides of the S electrode and the D electrode are covered by the protective layer.
8. The method for preparing a semiconductor transistor according to claim 7, characterized in that: The thickness of each metal layer in the Ti / Al / Ni / Au metal alloy layer in step (3) is Ti: 10-50nm; Al: 150-300nm; Ni: 100-200nm; Au: 150-300nm; The thickness of the silicon dioxide layer in step (4) is 10-30 nm; The thickness of each metal layer in the Ni / Au metal alloy layer in step (5) is Ni: Au: