Synthetic leather for waterproof and breathable water-based polyurethane mesh shoes and preparation method thereof
By preparing the water-based polyurethane surface layer, bottom layer and viscose slurry, and combining micro-porous films with microporous films, the existing water-based polyurethane upper is solved by insufficient strength and poor waterproof and breathable performance. The problem has achieved efficient waterproof and breathable effect and improved the market prospects.
Patent Information
- Application Number
- CN202111455171.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-01
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-12-01
AI Technical Summary
The existing water-based polyurethane uppers have weak strength and are difficult to achieve effective waterproof and breathable dual functions, which affects its market prospects.
The slurry preparation part includes water-based polyurethane top layer slurry, water-based polyurethane bottom layer slurry and viscose slurry. By scraping, drying, cooling, and applying microfiber synthetic leather bass and polytetrafluoroethylene microporous films, Perform micropore processing to form micropores of 0.001-0.1mm to achieve waterproof and breathable effect.
It significantly improves the strength and waterproof and breathable performance of synthetic leather for waterproof and breathable water-based polyurethane mesh shoes, expanding its market application prospects.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of synthetic leather, and more particularly to a waterproof and breathable water-based polyurethane mesh shoe synthetic leather and a preparation method thereof. Background Art
[0002] Polyurethane synthetic leather has become the best substitute for expensive natural leather products due to its excellent wear resistance, good tear strength and elongation, flat surface, full feel, comfort, good recovery and moderate price, and is widely used in clothing, footwear, luggage, furniture and other industries. The polyurethane synthetic leather that meets the requirements needs not only good physical properties, but also good moisture permeability and air permeability, soft, full and light feel, and a style and appearance that is more similar to natural leather.
[0003] A Chinese patent with announcement number CN105178053B discloses a process for producing waterborne polyurethane upper leather, which comprises the following steps: (1) coating a waterborne composite slurry bottom layer on a release paper, and transferring the layer to a medium-wave infrared heating oven for drying; (2) coating a waterborne composite slurry top layer on the waterborne composite slurry bottom layer, transferring the layer to a medium-wave infrared heating oven for drying, and then laminating the layer with a waterborne polyurethane ultrafine fiber synthetic leather base for drying to obtain a waterborne polyurethane upper leather semi-finished product; (3) subjecting the waterborne polyurethane upper leather semi-finished product to water washing, scratch resistance, waterproofing, and antifouling treatment, and then removing the release paper to obtain the waterborne polyurethane upper leather.
[0004] However, the strength of the waterborne polyurethane upper leather produced by the waterborne polyurethane upper leather production process is relatively weak, and it is difficult to achieve the dual functions of effective waterproofing and breathability, which in turn affects the market prospects of the waterborne polyurethane upper leather and needs to be improved. Summary of the invention
[0005] In view of the shortcomings of the prior art, the first purpose of the present invention is to provide a method for preparing a waterproof and breathable water-based polyurethane mesh shoe synthetic leather. The method for preparing the waterproof and breathable water-based polyurethane mesh shoe synthetic leather has the effect of obtaining a waterproof and breathable water-based polyurethane mesh shoe synthetic leather with dual functions of effective waterproofing and breathability, thereby significantly improving the market prospects of the waterproof and breathable water-based polyurethane mesh shoe synthetic leather.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing waterproof and breathable water-based polyurethane mesh shoes synthetic leather, comprising a slurry preparation part, a synthetic leather preparation part and a product processing part;
[0008] The slurry preparation part includes preparing waterborne polyurethane surface slurry, waterborne polyurethane bottom slurry and viscose slurry;
[0009] The synthetic leather preparation part includes the following steps: coating water-based polyurethane bottom slurry, drying, cooling, coating water-based polyurethane surface slurry, drying, cooling, coating viscose slurry, semi-drying, laminating ultrafine fiber synthetic leather bass, drying, coating viscose slurry, semi-drying, laminating polytetrafluoroethylene microporous film, drying, cooling, separation, microporous processing and rolling, and obtaining finished synthetic leather;
[0010] in:
[0011] The waterborne polyurethane surface slurry comprises, by weight, 60-80 parts of waterborne polyurethane, 20-26 parts of hydrophilic polyether polyurethane, 16-18 parts of isocyanate, 5-7 parts of dimethylolbutyric acid, 0.1-0.2 parts of thickener and 60-80 parts of water;
[0012] The waterborne polyurethane primer slurry comprises, by weight, 60-80 parts of waterborne polyurethane, 18-22 parts of polycaprolactone diol polyurethane, 2-3 parts of zinc oxide, 2-3 parts of tert-butyl hydroperoxide, 0.6-0.8 parts of carbon black, 0.1-0.2 parts of thickener and 60-80 parts of water;
[0013] The viscose slurry comprises 80-100 parts by weight of water-based acrylic resin, 12-16 parts by weight of 10-40 μm glass microbeads, 0.3-0.5 parts by weight of thickener and 120-200 parts by weight of water.
[0014] By adopting the above technical solution, a waterproof and breathable water-based polyurethane mesh shoe synthetic leather with high strength and waterproof and breathable properties can be effectively obtained.
[0015] The present invention is further configured as follows: the product processing part includes changing the color, embossing and / or surface treatment of the surface of the finished synthetic leather.
[0016] The present invention is further configured as follows: in the synthetic leather preparation part, the drying adopts an infrared heating oven; the cooling is natural cooling to room temperature; the separation is separation from the release paper, and the release paper is used to scrape the water-based polyurethane bottom layer slurry.
[0017] The present invention is further configured as follows: the drying temperature range of the waterborne polyurethane bottom slurry in the infrared heating oven is: 52-64°C in the first zone, 64-78°C in the second zone, and 105-118°C in the third zone; the duration is: 75s in the first zone, 55s in the second zone, and 40s in the third zone; and the sizing amount of the waterborne polyurethane bottom slurry is 100-120g / m 2The drying temperature range of the waterborne polyurethane surface slurry in the infrared heating oven is: 58-70°C in the first zone, 70-82°C in the second zone, 110-125°C in the third zone, and 130-140°C in the fourth zone. The duration is: 70s in the first zone, 50s in the second zone, and 35s in the third zone. The sizing amount of the waterborne polyurethane surface slurry is 90-115g / m 2 .
[0018] The present invention is further configured as follows: the viscose slurry, the ultrafine fiber synthetic leather base and the polytetrafluoroethylene microporous film are dried in the infrared heating oven at a temperature of 45-65° C. and for a duration of 30 seconds.
[0019] The present invention is further configured as follows: the micropore processing adopts a laser breathable micropore processor, and forms a plurality of micropores with a pore size of 0.001-0.1 mm and a pore spacing of 0.5-10 mm on the waterproof and breathable water-based polyurethane mesh shoe synthetic leather.
[0020] The present invention is further configured as follows: the preparation of the aqueous polyurethane base slurry adopts the following steps: a1, 60-80 parts by weight of aqueous polyurethane and 18-22 parts of polycaprolactone diol polyurethane are heated to 68-72°C and stirred for 1 hour to obtain a base prepolymer; b2, 2-3 parts of zinc oxide and 0.6-0.8 parts of carbon black are added to the base prepolymer, and after stirring and mixing evenly, 60-80 parts of water are added, and a base slurry emulsion is obtained after high-speed stirring; b3, 2-3 parts of tert-butyl hydroperoxide and 0.1-0.2 parts of thickener are added to the base slurry emulsion, and stirring is continued for 1-2 hours to obtain an aqueous polyurethane base slurry.
[0021] The present invention is further configured as follows: the preparation of the aqueous polyurethane surface layer slurry adopts the following steps: b1, mixing 60-80 parts of aqueous polyurethane and 16-18 parts of isocyanate by weight, heating to 75-85°C and stirring for 1 hour to obtain a surface layer prepolymer; b2, adding 5-7 parts of dihydroxymethylbutyric acid to the surface layer prepolymer, stirring and mixing evenly, and then adding 60-80 parts of water, stirring at high speed to obtain a surface layer slurry emulsion; b3, adding 0.1-0.2 parts of a thickener to the surface layer slurry emulsion, and continuously stirring for 1-2 hours to obtain an aqueous polyurethane surface layer slurry.
[0022] The present invention is further configured as follows: the preparation of the viscose slurry adopts the following steps: c1, mixing 80-100 parts by weight of water-based acrylic resin, 12-16 parts of 10-40 μm glass beads and 120-200 parts of water, heating to 68-78°C and stirring for 0.5h to obtain a mixed preliminary material; c2, adding 0.3-0.5 parts of a thickener to the mixed preliminary material, and continuously stirring for 0.5-1h to obtain a viscose slurry.
[0023] The second object of the present invention is to provide a waterproof and breathable water-based polyurethane mesh shoe synthetic leather, including the waterproof and breathable water-based polyurethane mesh shoe synthetic leather prepared by the preparation method of the waterproof and breathable water-based polyurethane mesh shoe synthetic leather as described above.
[0024] In summary, the present invention has the following beneficial effects: a water-based polyurethane surface layer slurry, a water-based polyurethane bottom layer slurry and a viscose slurry are prepared by adopting corresponding formula compositions, and then a waterproof and breathable water-based polyurethane mesh shoe synthetic leather with micropores is obtained under the corresponding preparation method; since the waterproof and breathable water-based polyurethane mesh shoe synthetic leather has the effect of absorbing water and swelling when water droplets adhere, the formed water-based polyurethane surface layer and the water-based polyurethane bottom layer both have the effect of absorbing water and swelling, thereby further reducing the pore size of the micropores to prevent water droplets from passing through, and since the volume of gas molecules is significantly smaller than the volume of water droplets, the micropores have the function of effectively allowing gas molecules to pass through while preventing water droplets from passing through; at the same time, the polytetrafluoroethylene microporous film has an effective waterproof and breathable function, and the dual functions of effective waterproofing and breathability are achieved by combining the water-based polyurethane surface layer and the water-based polyurethane bottom layer, thereby significantly improving the market prospects of the waterproof and breathable water-based polyurethane mesh shoe synthetic leather. DETAILED DESCRIPTION
[0025] To make the technical solutions and advantages of the present invention clearer, the present invention will be further described in detail below. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0026] The waterproof and breathable water-based polyurethane mesh shoe synthetic leather and its preparation method according to the embodiment of the present invention are specifically described below:
[0027] A method for preparing waterproof and breathable water-based polyurethane mesh shoes synthetic leather, comprising a slurry preparation part, a synthetic leather preparation part and a product processing part. The slurry preparation part includes preparing water-based polyurethane surface slurry, water-based polyurethane bottom slurry and viscose slurry. The synthetic leather preparation part includes sequentially scraping water-based polyurethane bottom slurry, drying, cooling, applying water-based polyurethane surface slurry, drying, cooling, applying viscose slurry, semi-drying, laminating microfiber synthetic leather bass, drying, applying viscose slurry, semi-drying, laminating polytetrafluoroethylene microporous film, drying, cooling, separation, microporous processing and rolling, and obtaining finished synthetic leather. The product processing part includes changing the color, embossing and / or surface treatment of the surface of the finished synthetic leather. The fineness of the microfiber synthetic leather bass is 0.1-1dtex, and it has a flying woven mesh. Therefore, after passing through the slurry preparation part, the synthetic leather preparation part and the product processing part, a waterproof and breathable water-based polyurethane mesh shoes synthetic leather with high strength and waterproof and breathable properties will be obtained.
[0028] The synthetic leather preparation part is dried in an infrared heating oven. The cooling is natural cooling to room temperature. The separation is separation from the release paper. The release paper is used to scrape the water-based polyurethane bottom slurry. In the micro-pore processing, a laser breathable micro-pore processor is used to form a plurality of micro-pores with a pore size of 0.001-0.1 mm and a pore spacing of 0.5-10 mm on the waterproof and breathable water-based polyurethane mesh shoe synthetic leather.
[0029] It should be noted that the waterborne polyurethane base slurry includes 60-80 parts by weight of waterborne polyurethane, 18-22 parts of polycaprolactone diol polyurethane, 2-3 parts of zinc oxide, 2-3 parts of tert-butyl hydroperoxide, 0.6-0.8 parts of carbon black, 0.1-0.2 parts of thickener and 60-80 parts of water. The preparation of the waterborne polyurethane base slurry adopts the following steps: a1, heating 60-80 parts of waterborne polyurethane and 18-22 parts of polycaprolactone diol polyurethane by weight to 68-72°C and stirring for 1 hour to obtain a base prepolymer; b2, adding 2-3 parts of zinc oxide and 0.6-0.8 parts of carbon black to the base prepolymer, stirring and mixing evenly, and then adding 60-80 parts of water, stirring at high speed to obtain a base slurry emulsion; b3, adding 2-3 parts of tert-butyl hydroperoxide and 0.1-0.2 parts of thickener to the base slurry emulsion, and continuously stirring for 1-2 hours to obtain a waterborne polyurethane base slurry. The drying temperature range of the waterborne polyurethane bottom slurry in the infrared heating oven is: 52-64°C in the first zone, 64-78°C in the second zone, and 105-118°C in the third zone. The duration is: 75s in the first zone, 55s in the second zone, and 40s in the third zone. The sizing amount of the waterborne polyurethane bottom slurry is 100-120g / m 2 .
[0030] The waterborne polyurethane surface slurry comprises, by weight, 60-80 parts of waterborne polyurethane, 20-26 parts of hydrophilic polyether polyurethane, 16-18 parts of isocyanate, 5-7 parts of dimethylolbutyric acid, 0.1-0.2 parts of thickener and 60-80 parts of water. The preparation of the waterborne polyurethane surface layer slurry adopts the following steps: b1, 60-80 parts of waterborne polyurethane, 20-26 parts of hydrophilic polyether polyurethane and 16-18 parts of isocyanate are mixed, heated to 75-85°C and stirred for 1 hour to obtain a surface layer prepolymer; b2, 5-7 parts of dihydroxymethylbutyric acid are added to the surface layer prepolymer, and after stirring and mixing evenly, 60-80 parts of water are added, and the surface layer slurry emulsion is obtained after high-speed stirring; b3, 0.1-0.2 parts of thickener are added to the surface layer slurry emulsion, and stirring is continued for 1-2 hours to obtain a waterborne polyurethane surface layer slurry. The drying temperature range of the waterborne polyurethane surface slurry in the infrared heating oven is: 58-70°C in the first zone, 70-82°C in the second zone, 110-125°C in the third zone, and 130-140°C in the fourth zone. The duration is: 70s in the first zone, 50s in the second zone, and 35s in the third zone. The sizing amount of the waterborne polyurethane surface slurry is 90-115g / m 2 .
[0031] The viscose slurry includes 80-100 parts by weight of water-based acrylic resin, 12-16 parts of 10-40 μm glass beads, 0.3-0.5 parts of thickener and 120-200 parts of water. The preparation of the viscose slurry adopts the following steps: c1, 80-100 parts by weight of water-based acrylic resin, 12-16 parts of 10-40 μm glass beads and 120-200 parts of water are mixed, heated to 68-78°C and stirred for 0.5h to obtain a mixed initial material; c2, 0.3-0.5 parts of thickener are added to the mixed initial material, and the viscose slurry is obtained after continuous stirring for 0.5-1h. Among them, the drying temperature of the viscose slurry in the infrared heating oven is 45-65°C, and the duration is 30s.
[0032] Meanwhile, in the synthetic leather preparation section, the drying temperatures of the ultrafine fiber synthetic leather base and the polytetrafluoroethylene microporous film in the infrared heating oven were both 45-65°C, and the drying duration was both 30s.
[0033] The present application also provides a waterproof and breathable water-based polyurethane mesh shoe synthetic leather, including a waterproof and breathable water-based polyurethane mesh shoe synthetic leather prepared by the above method for preparing the waterproof and breathable water-based polyurethane mesh shoe synthetic leather.
[0034] Embodiment 1
[0035] A method for preparing waterproof and breathable water-based polyurethane mesh shoes synthetic leather, comprising a slurry preparation part, a synthetic leather preparation part and a product processing part. The slurry preparation part includes preparing water-based polyurethane surface slurry, water-based polyurethane bottom slurry and viscose slurry. The synthetic leather preparation part includes sequentially scraping water-based polyurethane bottom slurry, drying, cooling, applying water-based polyurethane surface slurry, drying, cooling, applying viscose slurry, semi-drying, laminating microfiber synthetic leather bass, drying, applying viscose slurry, semi-drying, laminating polytetrafluoroethylene microporous film, drying, cooling, separation, microporous processing and rolling, and obtaining finished synthetic leather. The product processing part includes changing the color, embossing and / or surface treatment of the surface of the finished synthetic leather. Therefore, after passing through the slurry preparation part, the synthetic leather preparation part and the product processing part, a waterproof and breathable water-based polyurethane mesh shoes synthetic leather with high strength and waterproof and breathable properties will be obtained.
[0036] The synthetic leather preparation part is dried in an infrared heating oven. The cooling is natural cooling to room temperature. The separation is separation from the release paper. The release paper is used to scrape the water-based polyurethane bottom slurry. In the micro-pore processing, a laser breathable micro-pore processor is used to form a plurality of micro-pores with a pore size of 0.001 mm and a pore spacing of 0.5 mm on the waterproof and breathable water-based polyurethane mesh shoe synthetic leather.
[0037] It should be noted that the waterborne polyurethane bottom slurry includes 60 parts of waterborne polyurethane, 18 parts of polycaprolactone diol polyurethane, 2 parts of zinc oxide, 2 parts of tert-butyl hydroperoxide, 0.6 parts of carbon black, 0.1 parts of thickener and 60 parts of water by weight. The preparation of the waterborne polyurethane bottom slurry adopts the following steps: a1, heating 60 parts of waterborne polyurethane and 18 parts of polycaprolactone diol polyurethane by weight to 68°C and stirring for 1 hour to obtain a bottom prepolymer; b2, adding 2 parts of zinc oxide and 0.6 parts of carbon black to the bottom prepolymer, stirring and mixing evenly, and then adding 60 parts of water, stirring at high speed to obtain a bottom slurry emulsion; b3, adding 2 parts of tert-butyl hydroperoxide and 0.1 parts of thickener to the bottom slurry emulsion, and stirring for 1 hour to obtain a waterborne polyurethane bottom slurry. The drying temperature range of the waterborne polyurethane bottom slurry in the infrared heating oven is: 52-64°C in the first zone, 64-78°C in the second zone, and 105-118°C in the third zone. The duration is: 75s in the first zone, 55s in the second zone, and 40s in the third zone. The sizing amount of the waterborne polyurethane bottom slurry is 100g / m 2 .
[0038] The waterborne polyurethane surface slurry includes 60 parts of waterborne polyurethane, 20 parts of hydrophilic polyether polyurethane, 16 parts of isocyanate, 5 parts of dimethylolbutyric acid, 0.1 parts of thickener and 60 parts of water by weight. The preparation of the waterborne polyurethane surface slurry adopts the following steps: b1, 60 parts of waterborne polyurethane, 20 parts of hydrophilic polyether polyurethane and 16 parts of isocyanate by weight are mixed, heated to 75°C and stirred for 1 hour to obtain a surface prepolymer; b2, 5 parts of dimethylolbutyric acid are added to the surface prepolymer, and after stirring and mixing evenly, 60 parts of water are added, and the surface slurry emulsion is obtained after high-speed stirring; b3, 0.1 parts of thickener are added to the surface slurry emulsion, and the waterborne polyurethane surface slurry is obtained after continuous stirring for 1 hour. The drying temperature range of the waterborne polyurethane surface slurry in the infrared heating oven is: 58-70°C in the first zone, 70-82°C in the second zone, 110-125°C in the third zone, and 130-140°C in the fourth zone. The duration is: 70s in the first zone, 50s in the second zone, and 35s in the third zone. The sizing amount of the waterborne polyurethane surface slurry is 90g / m 2 .
[0039] The viscose slurry includes 80 parts by weight of water-based acrylic resin, 12 parts of 10-40 μm glass beads, 0.3 parts of thickener and 120 parts of water. The preparation of the viscose slurry adopts the following steps: c1, 80 parts by weight of water-based acrylic resin, 12 parts of 10-40 μm glass beads and 120 parts of water are mixed, heated to 68°C and stirred for 0.5 hours to obtain a mixed initial material; c2, 0.3 parts of thickener are added to the mixed initial material, and the viscose slurry is obtained after continuous stirring for 0.5 hours. Among them, the drying temperature of the viscose slurry in the infrared heating oven is 45°C, and the duration is 30 seconds.
[0040] Meanwhile, in the synthetic leather preparation section, the drying temperature of the ultrafine fiber synthetic leather base and the polytetrafluoroethylene microporous film in the infrared heating oven was 45°C, and the drying time was 30s.
[0041] The present application also provides a waterproof and breathable water-based polyurethane mesh shoe synthetic leather, including a waterproof and breathable water-based polyurethane mesh shoe synthetic leather prepared by the above method for preparing the waterproof and breathable water-based polyurethane mesh shoe synthetic leather.
[0042] Embodiment 2
[0043] A method for preparing waterproof and breathable water-based polyurethane mesh shoes synthetic leather, comprising a slurry preparation part, a synthetic leather preparation part and a product processing part. The slurry preparation part includes preparing water-based polyurethane surface slurry, water-based polyurethane bottom slurry and viscose slurry. The synthetic leather preparation part includes sequentially scraping water-based polyurethane bottom slurry, drying, cooling, applying water-based polyurethane surface slurry, drying, cooling, applying viscose slurry, semi-drying, laminating microfiber synthetic leather bass, drying, applying viscose slurry, semi-drying, laminating polytetrafluoroethylene microporous film, drying, cooling, separation, microporous processing and rolling, and obtaining finished synthetic leather. The product processing part includes changing the color, embossing and / or surface treatment of the surface of the finished synthetic leather. Therefore, after passing through the slurry preparation part, the synthetic leather preparation part and the product processing part, a waterproof and breathable water-based polyurethane mesh shoes synthetic leather with high strength and waterproof and breathable properties will be obtained.
[0044] The synthetic leather preparation part is dried in an infrared heating oven. The cooling is natural cooling to room temperature. The separation is separation from the release paper. The release paper is used to scrape the water-based polyurethane bottom slurry. In the micro-pore processing, a laser breathable micro-pore processor is used to form a plurality of micro-pores with a pore size of 0.01 mm and a pore spacing of 5 mm on the waterproof and breathable water-based polyurethane mesh shoe synthetic leather.
[0045] It should be noted that the waterborne polyurethane bottom slurry includes 70 parts of waterborne polyurethane, 20 parts of polycaprolactone diol polyurethane, 2.5 parts of zinc oxide, 2.5 parts of tert-butyl hydroperoxide, 0.7 parts of carbon black, 0.15 parts of thickener and 70 parts of water by weight. The preparation of the waterborne polyurethane bottom slurry adopts the following steps: a1, heating 70 parts of waterborne polyurethane and 20 parts of polycaprolactone diol polyurethane by weight to 70°C and stirring for 1 hour to obtain a bottom prepolymer; b2, adding 2.5 parts of zinc oxide and 0.7 parts of carbon black to the bottom prepolymer, stirring and mixing evenly, and then adding 70 parts of water, stirring at high speed to obtain a bottom slurry emulsion; b3, adding 2.5 parts of tert-butyl hydroperoxide and 0.15 parts of thickener to the bottom slurry emulsion, and continuously stirring for 1.5 hours to obtain a waterborne polyurethane bottom slurry. The drying temperature range of the waterborne polyurethane bottom slurry in the infrared heating oven is: 52-64°C in the first zone, 64-78°C in the second zone, and 105-118°C in the third zone. The duration is: 75s in the first zone, 55s in the second zone, and 40s in the third zone. The sizing amount of the waterborne polyurethane bottom slurry is 110g / m 2 .
[0046] The waterborne polyurethane surface slurry includes 70 parts of waterborne polyurethane, 23 parts of hydrophilic polyether polyurethane, 17 parts of isocyanate, 6 parts of dimethylolbutyric acid, 0.15 parts of thickener and 70 parts of water by weight. The preparation of the waterborne polyurethane surface slurry adopts the following steps: b1, 70 parts of waterborne polyurethane, 23 parts of hydrophilic polyether polyurethane and 17 parts of isocyanate by weight are mixed, heated to 80°C and stirred for 1 hour to obtain a surface prepolymer; b2, 6 parts of dimethylolbutyric acid are added to the surface prepolymer, and after stirring and mixing evenly, 70 parts of water are added, and the surface slurry emulsion is obtained after high-speed stirring; b3, 0.15 parts of thickener are added to the surface slurry emulsion, and the waterborne polyurethane surface slurry is obtained after continuous stirring for 1.5 hours. The drying temperature range of the waterborne polyurethane surface slurry in the infrared heating oven is: 58-70°C in the first zone, 70-82°C in the second zone, 110-125°C in the third zone, and 130-140°C in the fourth zone. The duration is: 70s in the first zone, 50s in the second zone, and 35s in the third zone. The sizing amount of the waterborne polyurethane surface slurry is 100g / m 2 .
[0047] The viscose slurry includes 90 parts by weight of water-based acrylic resin, 14 parts of 10-40 μm glass beads, 0.4 parts of thickener and 160 parts of water. The preparation of the viscose slurry adopts the following steps: c1, 90 parts by weight of water-based acrylic resin, 14 parts of 10-40 μm glass beads and 160 parts of water are mixed, heated to 73°C and stirred for 0.5 hours to obtain a mixed initial material; c2, 0.4 parts of thickener are added to the mixed initial material, and the viscose slurry is obtained after continuous stirring for 0.7 hours. Among them, the drying temperature of the viscose slurry in the infrared heating oven is 55°C, and the duration is 30 seconds.
[0048] Meanwhile, in the synthetic leather preparation section, the drying temperature of the ultrafine fiber synthetic leather base and the polytetrafluoroethylene microporous film in the infrared heating oven was 55°C, and the drying time was 30s.
[0049] The present application also provides a waterproof and breathable water-based polyurethane mesh shoe synthetic leather, including a waterproof and breathable water-based polyurethane mesh shoe synthetic leather prepared by the above method for preparing the waterproof and breathable water-based polyurethane mesh shoe synthetic leather.
[0050] Embodiment 3
[0051] A method for preparing waterproof and breathable water-based polyurethane mesh shoes synthetic leather, comprising a slurry preparation part, a synthetic leather preparation part and a product processing part. The slurry preparation part includes preparing water-based polyurethane surface slurry, water-based polyurethane bottom slurry and viscose slurry. The synthetic leather preparation part includes sequentially scraping water-based polyurethane bottom slurry, drying, cooling, applying water-based polyurethane surface slurry, drying, cooling, applying viscose slurry, semi-drying, laminating microfiber synthetic leather bass, drying, applying viscose slurry, semi-drying, laminating polytetrafluoroethylene microporous film, drying, cooling, separation, microporous processing and rolling, and obtaining finished synthetic leather. The product processing part includes changing the color, embossing and / or surface treatment of the surface of the finished synthetic leather. Therefore, after passing through the slurry preparation part, the synthetic leather preparation part and the product processing part, a waterproof and breathable water-based polyurethane mesh shoes synthetic leather with high strength and waterproof and breathable properties will be obtained.
[0052] The synthetic leather preparation part is dried in an infrared heating oven. The cooling is natural cooling to room temperature. The separation is separation from the release paper. The release paper is used to scrape the water-based polyurethane bottom slurry. In the micro-pore processing, a laser breathable micro-pore processor is used to form a plurality of micro-pores with a pore size of 0.1 mm and a pore spacing of 10 mm on the waterproof and breathable water-based polyurethane mesh shoe synthetic leather.
[0053] It should be noted that the waterborne polyurethane bottom slurry includes 80 parts of waterborne polyurethane, 22 parts of polycaprolactone diol polyurethane, 3 parts of zinc oxide, 3 parts of tert-butyl hydroperoxide, 0.8 parts of carbon black, 0.2 parts of thickener and 80 parts of water by weight. The preparation of the waterborne polyurethane bottom slurry adopts the following steps: a1, 80 parts of waterborne polyurethane and 22 parts of polycaprolactone diol polyurethane by weight are heated to 72°C and stirred for 1 hour to obtain a bottom prepolymer; b2, 3 parts of zinc oxide and 0.8 parts of carbon black are added to the bottom prepolymer, and after stirring and mixing evenly, 80 parts of water are added, and the bottom slurry emulsion is obtained after high-speed stirring; b3, 3 parts of tert-butyl hydroperoxide and 0.2 parts of thickener are added to the bottom slurry emulsion, and the waterborne polyurethane bottom slurry is obtained after continuous stirring for 2 hours. The drying temperature range of the waterborne polyurethane bottom slurry in the infrared heating oven is: 52-64°C in the first zone, 64-78°C in the second zone, and 105-118°C in the third zone. The duration is: 75s in the first zone, 55s in the second zone, and 40s in the third zone. The sizing amount of the waterborne polyurethane bottom slurry is 120g / m 2 .
[0054] The waterborne polyurethane surface slurry comprises 80 parts of waterborne polyurethane, 26 parts of hydrophilic polyether polyurethane, 18 parts of isocyanate, 7 parts of dimethylolbutyric acid, 0.2 parts of thickener and 80 parts of water by weight. The preparation of the waterborne polyurethane surface slurry adopts the following steps: b1, 80 parts of waterborne polyurethane, 26 parts of hydrophilic polyether polyurethane and 18 parts of isocyanate by weight are mixed, heated to 85°C and stirred for 1 hour to obtain a surface prepolymer; b2, 7 parts of dimethylolbutyric acid are added to the surface prepolymer, and after stirring and mixing evenly, 80 parts of water are added, and the surface slurry emulsion is obtained after high-speed stirring; b3, 0.2 parts of thickener are added to the surface slurry emulsion, and the waterborne polyurethane surface slurry is obtained after continuous stirring for 2 hours. The drying temperature range of the waterborne polyurethane surface slurry in the infrared heating oven is: 58-70°C in the first zone, 70-82°C in the second zone, 110-125°C in the third zone, and 130-140°C in the fourth zone. The duration is: 70s in the first zone, 50s in the second zone, and 35s in the third zone. The sizing amount of the waterborne polyurethane surface slurry is 115g / m 2 .
[0055] The viscose slurry includes 100 parts by weight of water-based acrylic resin, 16 parts of 10-40 μm glass beads, 0.5 parts of thickener and 200 parts of water. The preparation of the viscose slurry adopts the following steps: c1, mixing 100 parts by weight of water-based acrylic resin, 16 parts of 10-40 μm glass beads and 200 parts of water, heating to 78°C and stirring for 0.5 hours to obtain a mixed initial material; c2, adding 0.5 parts of thickener to the mixed initial material, and continuously stirring for 1 hour to obtain the viscose slurry. Among them, the drying temperature of the viscose slurry in the infrared heating oven is 65°C, and the duration is 30 seconds.
[0056] Meanwhile, in the synthetic leather preparation section, the drying temperatures of the ultrafine fiber synthetic leather base and the polytetrafluoroethylene microporous film in the infrared heating oven were both 65°C, and the drying duration was both 30s.
[0057] The present application also provides a waterproof and breathable water-based polyurethane mesh shoe synthetic leather, including a waterproof and breathable water-based polyurethane mesh shoe synthetic leather prepared by the above method for preparing the waterproof and breathable water-based polyurethane mesh shoe synthetic leather.
[0058] It should be noted that the thickener used above is a conventional material in synthetic leather slurry, which will not be described here. In addition, when the aqueous polyurethane surface layer prepared by the aqueous polyurethane surface layer slurry has micropores, the air permeability effect of gas circulation is achieved through the micropores, and when it encounters water, it expands and reduces the pore size of the micropores, further preventing water droplets from passing through, thereby achieving an effective waterproof effect; correspondingly, when the aqueous polyurethane bottom layer prepared by the aqueous polyurethane bottom layer slurry has micropores, the air permeability effect of gas circulation is achieved through the micropores, and when it encounters water, it expands and reduces the pore size of the micropores, further preventing water droplets from passing through, thereby achieving an effective waterproof effect. At the same time, the overall structural strength is effectively improved.
[0059] In summary, the present application adopts corresponding formula compositions to prepare water-based polyurethane surface slurry, water-based polyurethane bottom slurry and viscose slurry, and then obtains waterproof and breathable water-based polyurethane mesh shoes synthetic leather with micropores under the corresponding preparation method. When water droplets adhere to the waterproof and breathable water-based polyurethane mesh shoes synthetic leather, the formed water-based polyurethane surface layer and water-based polyurethane bottom layer both have the effect of absorbing water and swelling, thereby further reducing the pore size of the micropores to prevent water droplets from passing through. Since the volume of gas molecules is significantly smaller than the volume of water droplets, the micropores can effectively allow gas molecules to pass through while preventing water droplets from passing through. At the same time, the polytetrafluoroethylene microporous film has effective waterproof and breathable functions, and is combined with the water-based polyurethane surface layer and the water-based polyurethane bottom layer to achieve the dual functions of effective waterproofing and breathability, thereby significantly improving the market prospects of waterproof and breathable water-based polyurethane mesh shoes synthetic leather.
[0060] The "first", "second", "third", "fourth", etc. (if any) referred to in this application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments described herein can be implemented in an order other than that described herein. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods or devices.
[0061] It should be noted that the descriptions involving "first", "second", etc. in this application are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.
[0062] Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, according to the idea of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A method for preparing waterproof and breathable water-based polyurethane mesh shoes synthetic leather, characterized in that: It includes slurry preparation part, synthetic leather preparation part and product processing part; The slurry preparation part includes preparing waterborne polyurethane surface slurry, waterborne polyurethane bottom slurry and viscose slurry; The synthetic leather preparation part includes the following steps: coating water-based polyurethane bottom slurry, drying, cooling, coating water-based polyurethane surface slurry, drying, cooling, coating viscose slurry, semi-drying, laminating ultrafine fiber synthetic leather bass, drying, coating viscose slurry, semi-drying, laminating polytetrafluoroethylene microporous film, drying, cooling, separation, microporous processing and rolling, and obtaining finished synthetic leather; in: The waterborne polyurethane surface slurry comprises 60-80 parts by weight of waterborne polyurethane, 20-26 parts of hydrophilic polyether polyurethane, 16-18 parts of isocyanate, 5-7 parts of dimethylolbutyric acid, 0.1-0.2 parts of thickener and 60-80 parts of water; and the preparation of the waterborne polyurethane surface slurry adopts the following steps: b1, 60-80 parts by weight of waterborne polyurethane, 20-26 parts of hydrophilic polyether polyurethane, 16-18 parts of isocyanate, 5-7 parts of dimethylolbutyric acid, 0.1-0.2 parts of thickener and 60-80 parts of water. b. Add 5-7 parts of dimethylolbutyric acid to the surface prepolymer, stir and mix evenly, then add 60-80 parts of water, stir at high speed to obtain a surface slurry emulsion; b. Add 0.1-0.2 parts of thickener to the surface slurry emulsion, stir for 1-2 hours, and obtain a waterborne polyurethane surface slurry; The waterborne polyurethane primer slurry comprises 60-80 parts by weight of waterborne polyurethane, 18-22 parts of polycaprolactone diol polyurethane, 2-3 parts of zinc oxide, 2-3 parts of tert-butyl hydroperoxide, 0.6-0.8 parts of carbon black, 0.1-0.2 parts of thickener and 60-80 parts of water; and the waterborne polyurethane primer slurry is prepared by the following steps: a1, 60-80 parts by weight of waterborne polyurethane and 18-22 parts of polycaprolactone diol polyurethane are mixed; b. Add 2-3 parts of zinc oxide and 0.6-0.8 parts of carbon black to the bottom prepolymer, stir and mix well, then add 60-80 parts of water, stir at high speed to obtain bottom slurry emulsion; b. Add 2-3 parts of tert-butyl hydroperoxide and 0.1-0.2 parts of thickener to the bottom slurry emulsion, stir for 1-2 hours to obtain waterborne polyurethane bottom slurry; The viscose slurry comprises 80-100 parts by weight of water-based acrylic resin, 12-16 parts by weight of 10-40 μm glass microbeads, 0.3-0.5 parts by weight of thickener and 120-200 parts by weight of water.
2. The method for preparing the waterproof and breathable water-based polyurethane mesh shoe synthetic leather according to claim 1, characterized in that: The product processing part includes changing the color, embossing and / or surface treatment of the surface of the finished synthetic leather.
3. The method for preparing the waterproof and breathable water-based polyurethane mesh shoe synthetic leather according to claim 1, characterized in that: In the synthetic leather preparation part, the drying is carried out by using an infrared heating oven; the cooling is carried out by naturally cooling to room temperature; the separation is carried out by separating from the release paper, and the release paper is used to scrape the water-based polyurethane base slurry.
4. The method for preparing the waterproof and breathable water-based polyurethane mesh shoe synthetic leather according to claim 3, characterized in that: The drying temperature range of the waterborne polyurethane bottom slurry in the infrared heating oven is: 52-64°C in the first zone, 64-78°C in the second zone, and 105-118°C in the third zone. The duration is: 75s in the first zone, 55s in the second zone, and 40s in the third zone. The sizing amount of the waterborne polyurethane bottom slurry is 100-120g / m 2 The drying temperature range of the waterborne polyurethane surface slurry in the infrared heating oven is: 58-70°C in the first zone, 70-82°C in the second zone, 110-125°C in the third zone, and 130-140°C in the fourth zone. The duration is: 70s in the first zone, 50s in the second zone, and 35s in the third zone. The sizing amount of the waterborne polyurethane surface slurry is 90-115g / m 2 .
5. The method for preparing the waterproof and breathable water-based polyurethane mesh shoe synthetic leather according to claim 4, characterized in that: The viscose slurry, ultrafine fiber synthetic leather base and polytetrafluoroethylene microporous film are dried in an infrared heating oven at a temperature of 45-65° C. and for a duration of 30 seconds.
6. The method for preparing the waterproof and breathable water-based polyurethane mesh shoe synthetic leather according to claim 1, characterized in that: The micro-hole processing adopts a laser breathable micro-hole processor, and forms a plurality of micro-holes with a hole diameter of 0.001-0.1 mm and a hole spacing of 0.5-10 mm on the waterproof and breathable water-based polyurethane mesh shoe synthetic leather.
7. The method for preparing the waterproof and breathable water-based polyurethane mesh shoe synthetic leather according to claim 1, characterized in that: The viscose slurry is prepared by the following steps: c1, mixing 80-100 parts by weight of water-based acrylic resin, 12-16 parts of 10-40 μm glass beads and 120-200 parts of water, heating to 68-78° C. and stirring for 0.5 h to obtain a mixed preliminary material; c2, adding 0.3-0.5 parts of a thickener to the mixed preliminary material, and continuously stirring for 0.5-1 h to obtain a viscose slurry.
8. A waterproof and breathable water-based polyurethane mesh shoe synthetic leather, characterized by: The invention comprises a waterproof and breathable water-based polyurethane mesh shoe synthetic leather prepared by the method for preparing the waterproof and breathable water-based polyurethane mesh shoe synthetic leather as claimed in any one of claims 1 to 7.
Citation Information
Patent Citations
A water-based polyurethane shoe upper leather production process
CN105178053B
Water swelling polyurethane elastomer sealing product material and preparation method
CN101565602A
Foaming synthetic leather manufacturing technology based on waterborne polyurethane (WPU)
CN102409554A
Production process of waterborne polyurethane instep leather
CN105178053A
Rubber capable of expanding when encountering water and oil and preparation method of rubber
CN112961490A