Macroporous alumina carrier and preparation method thereof, hydrodesulfurization catalyst and preparation method thereof

By using sodium polyacrylate and styrene butadiene rubber latex in the alumina support, combined with low-temperature vulcanization technology, the problems of catalyst coking and spinel structure are solved, and the activity and stability of gasoline hydrodesulfurization catalyst are improved.

CN114073944BActive Publication Date: 2024-11-29PETROCHINA CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202010826742.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-17
Publication Date
2024-11-29
Estimated Expiration
2040-08-17

AI Technical Summary

Technical Problem

The existing macroporous alumina support can easily lead to the catalyst coking and carbon deposit during the dehydrogenation of organic liquids, and the activated metal and alumina form a spinel passivation structure, affecting the catalytic activity.

Method used

Sodium polyacrylate and styrene butadiene rubber latex are used as pore reamers, and different acid-base pore reamers are arranged to alternately add the alumina solution to prepare a large-porous alumina support, and use this as a support to prepare a gasoline hydrodesulfurization catalyst. The formation of spinel structure is avoided through low-temperature vulcanization and dispersion regulation.

Benefits of technology

Alumina support with rich macroporous structures is achieved at low pore reamer usage, which improves the desulfurization activity and selectivity of the catalyst, reduces the risk of coking and carbon deposits, and enhances the stability of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114073944B_ABST
    Figure CN114073944B_ABST
Patent Text Reader

Abstract

The present invention relates to a macroporous alumina carrier, wherein the pore size distribution of the macroporous alumina carrier is 80-240 nm, the macropore ratio is 10-50%, the macropore volume is 0.2-0.6 mL / g, and the macropores are radially unevenly distributed in the alumina carrier. The present invention also relates to a method for preparing a macroporous alumina carrier. The present invention also relates to a gasoline hydrodesulfurization catalyst, which uses the above macroporous alumina carrier as a carrier. The present invention also relates to a method for preparing a gasoline hydrodesulfurization catalyst. The catalyst does not undergo high-temperature calcination, but is sulfurized in two stages at low temperature, has a good sulfurization effect, a high catalyst desulfurization activity, and good selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hydrodesulfurization catalyst and a macroporous alumina carrier, and in particular to a macroporous alumina carrier and a preparation method thereof, and a hydrodesulfurization catalyst and a preparation method thereof. Background Art

[0002] As the main source of energy and raw materials for daily chemicals, petroleum and its products support the economic development of the entire country. Catalytic processes and reactions are an indispensable part of petroleum processing. In order to improve the conversion efficiency in petroleum processing, the development of efficient catalysts has always been the common pursuit of scientific researchers.

[0003] Alumina, as a traditional catalyst carrier material, has the characteristics of mature technology, adjustable pore structure, low cost and easy processing and molding. It is widely used in the preparation of petroleum refining and chemical catalysts. As an important component of the catalyst, the carrier can improve the dispersion effect of the active components on the one hand, and on the other hand, its pore structure provides diffusion channels for reactant molecules and product molecules, thereby improving the utilization efficiency of metals. Macroporous carrier materials have the characteristics of low mass transfer resistance and high efficiency. In recent years, as the core component of the catalyst, macroporous alumina, molecular sieves, activated carbon, etc. have been widely studied to improve the utilization efficiency of the catalyst. According to the synthesis process, macroporous materials can be divided into two categories: one is the direct synthesis of new carrier materials with macroporous structures during the synthesis process, and the other is the post-modification of the materials to obtain carrier materials with macroporous structures. The research on the synthesis method of the second type of macroporous carrier materials mainly obtains macroporous structures through template agents, hydrothermal methods, etc., which has the advantages of simple production process and low cost. The relevant processing technology has been applied in industry.

[0004] There are many related documents on the synthesis of macroporous alumina materials by template method. According to the different types of templates, they can be divided into two methods: hard template method and soft template method. The hard template method represented by activated carbon can obtain better macroporous alumina. US4448896 discloses a carbon black as a pore-enlarging agent, which can obtain macroporous alumina with a pore size distribution of 15-300nm. However, due to the uneven distribution of particle diameter of carbon black, it is difficult to prepare macroporous alumina with concentrated pore size distribution.

[0005] Chinese application CN201410347665.X discloses a method for preparing large-pore volume, high-strength alumina. By adding pore-enlarging agents such as polyacrylamide, polyvinyl alcohol, alkyl cellulose, sesbania powder, starch, etc., an alumina carrier containing large pores is obtained. The amount of the pore-enlarging agent used accounts for 10-30% of the alumina, but the specific pore size range is not disclosed.

[0006] Chinese application CN200410050717.3 discloses a method for preparing alumina with expanded pores of starch. When the amount of starch added is 10-20% of alumina, the alumina prepared by the method has the characteristics of high strength, large pore size and concentrated pore size distribution compared with the prior art. However, the high amount of starch added increases the production cost on the one hand, and the large amount of starch decomposition leads to more serious environmental pollution on the other hand. Although the hard template method can obtain a better macroporous alumina carrier, the amount of template used is preferably greater than 20%, which greatly increases the processing cost, and the decomposition of a large amount of template does not meet the development requirements of low-carbon and environmental protection.

[0007] Chinese application CN 201010509425.7 discloses a method for pore expansion by hydrothermal and template agent to prepare an alumina carrier with a macroporous structure. Through the hydrothermal auxiliary pore expansion effect, the amount of template agent can be reduced to 3-10%.

[0008] Chinese application CN 200310103035.X discloses a method for preparing macroporous alumina, using polyvinyl alcohol, polypropylene alcohol, and polyethylene glycol soft templates for pore expansion. By adding 1% polyethylene glycol, the pore volume with a pore size greater than 100 nm accounts for 26.2% of the total pore volume. The soft template has the advantages of low dosage and good pore expansion effect, but the alcohol soft template with a higher molecular weight has poor solubility in water, which limits its use in expanding ultra-macroporous alumina.

[0009] Macroporous alumina has been successfully applied to multiple catalyst systems, and has different degrees of improvement on the activity, selectivity and stability of the catalyst. The present invention uses sodium polyacrylate and styrene-butadiene rubber emulsion as pore expanders, and configures pore expander solutions with different acidity and alkalinity and adds them alternately to alumina, so that an alumina carrier with a rich macroporous structure can be obtained with a lower amount of pore expander.

[0010] In organic liquid dehydrogenation catalysts, the active metal components play a role in dehydrogenation, while the strong acid centers of the carrier play a role in cracking and isomerization, which is an important cause of catalyst coking and carbon deposition. Therefore, the key to dehydrogenation catalysts is to strengthen the dehydrogenation active sites while weakening the strong acid centers on the surface of the catalyst.

[0011] As Al2O3 has strong mechanical strength and good thermal stability, it is widely used as a catalyst carrier in the petrochemical industry, and can be used in reforming, isomerization, hydrogenation, dehydrogenation, desulfurization, denitrification and other processes. However, the surface of the alumina carrier is highly acidic, and in the process of organic liquid dehydrogenation catalysis, it is easy to break the CC bond, resulting in catalyst coking and carbon deposition. In addition, the alumina carrier can interact strongly with metals and can form a spinel passivation structure with active metals such as Ni, thereby affecting its catalytic activity. Summary of the invention

[0012] Based on the above, the purpose of the present invention is to provide a macroporous alumina carrier and a preparation method thereof, as well as a gasoline hydrodesulfurization catalyst using macroporous alumina as a carrier and a preparation method thereof. The macropores in the macroporous alumina carrier provided by the present invention are radially unevenly distributed in the carrier, and the acidity distribution of the carrier is adjusted at the same time.

[0013] To this end, the present invention provides a macroporous alumina carrier, wherein the pore size distribution of the macroporous alumina carrier is 80-240nm, the macropore ratio is 10-50%, the macropore volume is 0.2-0.6mL / g, and the macropores are radially unevenly distributed in the alumina carrier.

[0014] The macroporous alumina carrier of the present invention preferably has a pore size distribution of 90 to 240 nm, a macropore ratio of 26 to 44%, and a macropore volume of 0.2 to 0.6 mL / g.

[0015] The macroporous alumina carrier of the present invention preferably has a pore size distribution of 90-150 nm or 130-200 nm, a macropore ratio of 26-44%, a macropore volume of 0.2-0.6 mL / g, and a specific surface area of ​​210-330 m 2 / g.

[0016] The macroporous alumina carrier of the present invention preferably further comprises 0.5-5.5wt% of CoSnO3.

[0017] The macroporous alumina carrier described in the present invention is preferably further comprised of La2Sn3O7 and CoSnO3. Based on the carrier, the content of La2Sn3O7 in the carrier is 0.5-4.5wt%, the content of CoSnO3 is 0.5-3.5wt%, and the content of alumina is 75-95wt%.

[0018] The macroporous alumina carrier of the present invention preferably has a La2Sn3O7 content of 0.5-3.5wt%, a CoSnO3 content of 0.5-3.0wt%, and an alumina content of 76.0-88.0wt%.

[0019] To this end, the present invention also provides a method for preparing a macroporous alumina carrier, which is the method for preparing the above-mentioned macroporous alumina carrier, comprising the following steps:

[0020] (1) preparing a mixed solution containing sodium polyacrylate and styrene-butadiene rubber emulsion: adding sodium polyacrylate to deionized water, then adding styrene-butadiene rubber emulsion, then adding acid solution to adjust the pH value to 4-7, and then stirring and dividing into 2-5 portions;

[0021] (2) preparing a sodium polyacrylate acid solution: adding sodium polyacrylate to deionized water, adding acid solution to adjust the pH value to 4-7, and the pH value is 0.5-2 units higher than the pH value of the mixed solution containing sodium polyacrylate and styrene-butadiene rubber emulsion prepared in step (1), and dividing the sodium polyacrylate acid solution into 2-5 portions;

[0022] (3) Preparing a carrier: Pseudo-boehmite and a binder are mixed uniformly to obtain a pseudo-boehmite mixture, which is divided into 2-5 portions. One portion of the pseudo-boehmite mixture is taken, and one portion of a mixture containing sodium polyacrylate and styrene-butadiene rubber emulsion and deionized water are added in sequence and kneaded uniformly. Then one portion of a sodium polyacrylate acid solution is added, and then a second portion of the pseudo-boehmite mixture is added. The above-mentioned adding process is repeated until the pseudo-boehmite mixture, the mixture containing sodium acrylate and styrene-butadiene rubber emulsion, and the sodium polyacrylate acid solution are all added. The finally kneaded material is subjected to extrusion molding, drying, and calcination to obtain an alumina carrier having a macroporous structure.

[0023] In the method for preparing the macroporous alumina carrier of the present invention, preferably, in step (3), CoSnO3 and / or La2Sn3O7 are added when the pseudo-boehmite and the binder are mixed.

[0024] The method for preparing the macroporous alumina carrier of the present invention is preferably such that in the mixed solution containing sodium polyacrylate and styrene-butadiene rubber emulsion, the content of sodium polyacrylate is 10-40wt%, and the content of styrene-butadiene rubber emulsion is 2-10wt%.

[0025] The method for preparing the macroporous alumina carrier of the present invention is preferably such that in step (3), the amount of each portion of the sodium polyacrylate acid solution added is 0.5-35.0wt% per portion of pseudo-boehmite, calculated as sodium polyacrylate; and the amount of each portion of the mixed solution containing sodium polyacrylate and styrene-butadiene rubber emulsion added is 0.1-30.0wt% per portion of pseudo-boehmite, calculated as the total amount of sodium polyacrylate and styrene-butadiene rubber.

[0026] The method for preparing the macroporous alumina carrier of the present invention is preferably such that in step (3), the amount of each portion of the sodium polyacrylate acid solution added is 10.5-25.0 wt% per portion of pseudo-boehmite, calculated as sodium polyacrylate; and the amount of each portion of the mixed solution containing sodium polyacrylate and styrene-butadiene rubber emulsion added is 0.2-8.5 wt% per portion of pseudo-boehmite, calculated as the total amount of sodium polyacrylate and styrene-butadiene rubber.

[0027] To this end, the present invention also provides a gasoline hydrodesulfurization catalyst, which uses the above-mentioned macroporous alumina carrier as a carrier, cobalt, molybdenum and phosphorus as active components, and based on the catalyst, the molybdenum content of the active components is 5.0-17.0wt%, the cobalt content is 2.0-7.0wt%, and the phosphorus content is 0.1-3.5wt%.

[0028] The molybdenum and cobalt in the active components exist in the form of MoCoS, and the catalyst contains more than 3 wt% of S.

[0029] In the gasoline hydrodesulfurization catalyst of the present invention, preferably, Co is measured by weight of CoO, and the content of Co in the carrier is lower than the amount of Co loaded on the catalyst.

[0030] To this end, the present invention also provides a method for preparing a gasoline hydrodesulfurization catalyst, which is the above-mentioned method for preparing a gasoline hydrodesulfurization catalyst, comprising the following steps:

[0031] (1) Preparation of catalyst precursor: After impregnating the carrier with an impregnation solution containing Co, Mo, P and S, aging for more than 4 hours to obtain a catalyst precursor;

[0032] (2) Sulfidation: Under closed conditions, reflux the catalyst precursor at 60-80°C for 0.3-2.0 hours, then add a reducing agent and continue to react at 100-150°C for 0.5-10 hours, cool to room temperature, filter, wash with deionized water, and vacuum dry at 80-150°C to obtain the final catalyst product.

[0033] In the method for preparing the gasoline hydrodesulfurization catalyst of the present invention, it is preferred that in step (1), the amount of sulfur added to the impregnation liquid is 85-140% of the theoretical sulfur loading of the catalyst.

[0034] To this end, the present invention also provides a gasoline hydrodesulfurization catalyst, which uses the above-mentioned macroporous alumina carrier as a carrier and cobalt, molybdenum, nickel and phosphorus as active components; based on the catalyst and the mass of the oxides, the molybdenum content in the active components is 5.0-17.0wt%, the cobalt content is 2.0-7.0wt%, the nickel content is 2-5.5wt%, and the phosphorus content is 0.1-3.5wt%. The molybdenum and cobalt in the active components exist in the form of MoCoS, and the nickel and cobalt mainly exist in the form of NiCoS. The catalyst contains more than 3wt% of S, preferably 3-15wt% of sulfur, and more preferably 3-8wt% of sulfur.

[0035] The gasoline hydrodesulfurization catalyst of the present invention preferably has a molybdenum content of 6.0-14.0wt%, a cobalt content of 2.0-5.0wt%, a nickel content of 3-5.5wt% and a phosphorus content of 0.1-3.0wt% in the active components.

[0036] To this end, the present invention also provides a method for preparing a gasoline hydrodesulfurization catalyst, which is the above-mentioned method for preparing a gasoline hydrodesulfurization catalyst, and the method comprises the following steps:

[0037] (1) Preparation of catalyst precursor: After impregnating the carrier with an impregnation solution containing Co, Mo, Ni, P and S, aging for more than 4 hours to obtain a catalyst precursor;

[0038] (2) Sulfidation: Under closed conditions, reflux the catalyst precursor at 60-80°C for 0.3-2.0 hours, then add a reducing agent and continue to react at 100-150°C for 0.5-10 hours, cool to room temperature, filter, wash with deionized water, and vacuum dry at 80-150°C to obtain the final catalyst product.

[0039] In the method for preparing the gasoline hydrodesulfurization catalyst of the present invention, it is preferred that in step (1), the amount of sulfur added to the impregnation liquid is 85-140% of the theoretical sulfur loading of the catalyst.

[0040] The macroporous alumina carrier and its preparation method, as well as the gasoline hydrodesulfurization catalyst and its preparation method provided by the present invention are specifically described as follows:

[0041] The macroporous alumina carrier of the present invention has a pore size distribution of 80-240nm, a macropore ratio of 10-50%, a macropore volume of 0.2-0.6mL / g, and the macropores are unevenly distributed in the radial direction of the carrier.

[0042] More preferably, the macroporous alumina carrier has a pore size distribution of 90 to 240 nm, a macropore ratio of 26 to 44%, and a macropore volume of 0.2 to 0.6 mL / g. More preferably, the macroporous alumina carrier has a pore size distribution of 90 to 150 nm, or 130 to 200 nm, a macropore ratio of 26 to 44%, a macropore volume of 0.2 to 0.6 mL / g, and a specific surface area of ​​210-330 m 2 / g

[0043] The method for preparing a macroporous alumina carrier of the present invention comprises the following steps:

[0044] (1) preparing sodium polyacrylate and styrene-butadiene rubber emulsion: adding sodium polyacrylate to deionized water, then adding styrene-butadiene rubber emulsion, adding acid solution to adjust the pH value to between 4 and 7, and then stirring and dividing into 2 to 5 portions;

[0045] (2) preparing a sodium polyacrylate acid solution: adding an acid solution to adjust the pH value to between 4 and 7, and the pH value is 0.5 to 2 units higher than the pH value of the sodium polyacrylate and styrene-butadiene rubber emulsion prepared in step (1), preferably 1.0 to 2 units higher, and the sodium polyacrylate acid solution is divided into 2 to 5 portions;

[0046] (3) Preparing a carrier: Add pseudo-boehmite and a binder such as sesbania powder into a kneader and mix evenly to obtain a pseudo-boehmite mixture, which is divided into 2-5 portions. Take one portion of the pseudo-boehmite mixture, first add one portion of sodium polyacrylate and styrene-butadiene rubber emulsion and deionized water to the pseudo-boehmite powder in sequence and knead evenly; then add one portion of sodium polyacrylate acid solution, and then add a second portion of pseudo-boehmite and a certain amount of acid solution, and knead evenly; then add one portion of sodium polyacrylate and styrene-butadiene rubber emulsion, and repeat the above-mentioned adding process until all the pseudo-boehmite, sodium polyacrylate solution, styrene-butadiene rubber emulsion, and sodium polyacrylate acid solution are added; the repeatedly kneaded materials are extruded, dried, and calcined to obtain an alumina carrier with a macroporous structure.

[0047] In the above method, the alumina carrier containing macropores is alternately mixed with a mixture of sodium acrylate and styrene-butadiene rubber emulsion with different pH values ​​and different contents, a sodium polyacrylate acid solution and pseudo-boehmite, etc. The prepared macropores are unevenly distributed in the radial direction of the carrier, and the acid distribution of the carrier is adjusted at the same time.

[0048] The pH value of the sodium polyacrylate acid solution prepared in step (2) of the present invention is 0.5-2 units higher than the pH value of the sodium polyacrylate and styrene-butadiene rubber emulsion prepared in step (1). Sodium polyacrylate has different water absorption properties under different pH conditions. Sodium acrylate and styrene-butadiene rubber emulsions and sodium polyacrylate acid solutions with different pH values ​​and different amounts are alternately mixed with pseudo-boehmite, etc., and the prepared macropores are unevenly distributed in the radial direction of the carrier, and the acid distribution of the carrier is adjusted at the same time. The macropores are controlled to be unevenly distributed in the radial direction of the carrier by adjusting the ratio of sodium polyacrylate and styrene-butadiene rubber emulsion, the pH value of the two solutions, and the addition amount of the two solutions, and the acid distribution of the carrier is adjusted at the same time. There is no restriction on the types of styrene-butadiene rubber and sodium polyacrylate. Sodium polyacrylate whose water absorption rate is affected by pH value is preferred.

[0049] The division of steps (1) to (3) in the preparation method of the carrier of the present invention can be equal or unequal, so as to achieve uneven distribution of the macropores of the alumina carrier in the radial direction of the carrier and adjust the acidity distribution of the carrier.

[0050] The source and properties of the pseudo-boehmite powder are not limited, and the powder can be produced by carbonization, nitric acid, sulfuric acid, ammonia, etc. The pseudo-boehmite is suitable for different specific surface areas, pore volumes, and pore diameters.

[0051] The acid used in steps (1) to (3) is any organic or inorganic acid commonly used in the art, such as acetic acid, citric acid, nitric acid, hydrochloric acid, etc. The amount of acid added in step (3) is 0.5-8wt%, preferably 2-5wt% of the pseudo-boehmite.

[0052] The amount of the sodium polyacrylate acid solution added is 0.5 to 35.0 wt % of the added pseudo-boehmite, calculated as sodium polyacrylate, preferably 10.5 to 25.0 wt %, and more preferably 21.5 to 35.0 wt %.

[0053] In the mixture of sodium polyacrylate and styrene butadiene rubber emulsion, sodium polyacrylate accounts for 10-40% of the mixture, and the addition amount of sodium polyacrylate and styrene butadiene rubber emulsion is 0.1-30.0wt% of the added pseudo-boehmite, preferably 0.1-25.0wt%, more preferably 0.2-8.5wt%. It is more effective to promote the uneven distribution of macropores of the alumina carrier in the radial direction of the carrier, and adjust the acid distribution of the carrier at the same time.

[0054] The extrusion molding, drying and calcination obtain an alumina carrier containing a macroporous structure. The kneading or extrusion process is a conventional method in the field. After the extrusion molding, the alumina carrier is dried at 80-200°C for 2-8 hours and calcined at 550-700°C for 4-6 hours to finally obtain a macroporous alumina carrier. The prepared macropores are unevenly distributed in the radial direction of the carrier, and the acidity distribution of the carrier is adjusted at the same time.

[0055] The present invention also provides a gasoline hydrodesulfurization catalyst, which uses a macroporous aluminum oxide carrier as a carrier and cobalt, molybdenum and phosphorus as active components. Based on the catalyst, the active component molybdenum content in the catalyst is 5.0-17.0wt%, the cobalt content is 2.0-7.0wt%, and the phosphorus content is 0.1-3.5wt%, and the molybdenum and cobalt in the active components are mainly present in the form of MoCoS, and the catalyst contains more than 3wt% of S.

[0056] Of course, the catalyst of the present invention inevitably produces MoCoS active phase, MoS2, CoS2 phase, and the presence of molybdenum oxide and cobalt oxide. In order to form as much MoCoS active phase as possible, unlike directly introducing oxides such as cobalt and tin, the present invention introduces CoSnO3 into an alumina carrier, and then prepares a supported cobalt-molybdenum hydrodesulfurization catalyst, effectively controlling the growth of the supported cobalt grains, inhibiting the aggregation of cobalt grains, promoting the formation of MoCoS active phase, and being beneficial to improving the desulfurization activity of the catalyst. In the alumina carrier, the content of CoO in terms of cobalt oxide is lower than the content of CoO supported by the catalyst, which helps to improve the dispersibility of the active components on the carrier surface, improve the utilization rate of the active components, and have good catalyst stability.

[0057] The Co-Mo-S active phase in the catalyst of the present invention has high dispersion, and is prepared at low temperature to avoid the formation of a spinel structure between metal and alumina. The catalyst does not undergo high-temperature calcination, but is sulfurized in two stages at low temperature, so the sulfurization effect is good, the catalyst has high desulfurization activity, and good selectivity.

[0058] The preparation method of the hydrodesulfurization catalyst of the present invention comprises the following steps: impregnating a macroporous alumina carrier with an impregnation solution containing Co, Mo, P and S, aging for more than 4 hours, and obtaining a catalyst precursor; and the sulfurization process: under closed conditions, reflux the obtained catalyst precursor at 60-80° C. for 0.3-2.0 hours, then adding a reducing agent solution, continuing to react at 100-150° C. for 0.5-10 hours, cooling to room temperature, filtering, washing with deionized water, and vacuum drying at 80-150° C. to obtain a final catalyst product. Preferably, the vacuum drying temperature is 100-120° C.

[0059] The sulfurized catalyst of the present invention has a low sulfurization temperature, which avoids the formation of a spinel structure between the active metal and the carrier alumina, thereby improving the reaction activity of the catalyst.

[0060] In the impregnation solution, the amount of sulfur-containing compound added is 85-140% of the theoretical sulfur loading of the catalyst, and preferably the amount of sulfur-containing compound added is 95-130% of the theoretical sulfur loading of the catalyst.

[0061] Further preferably, the alumina carrier contains CoSnO3, the content of CoSnO3 is 0.5-5.5 wt%, and the Co content of the alumina carrier, expressed as CoO, is lower than the amount of Co loaded on the catalyst (expressed as CoO).

[0062] In the present invention, the preparation of CoSnO3 is not limited. The CoSnO3 can be prepared according to the following method: dissolve the tin source and the cobalt source respectively, mix and stir evenly, add alkali solution and react at 120-180°C for 7-24h, and after cooling, wash and dry the obtained reactant to obtain a precursor powder. The precursor powder is calcined at 560-800°C for 2-6h to obtain CoSnO3, which is then dispersed by ultrasound for later use.

[0063] The gasoline hydrodesulfurization catalyst of the present invention uses a macroporous alumina carrier as a carrier, cobalt, molybdenum and phosphorus as active components, the carrier contains CoSnO3, the CoSnO3 content is 0.5-5.5wt%, and the Co content in the alumina carrier is lower than the amount of Co loaded on the catalyst (both calculated as CoO).

[0064] Based on the catalyst, the molybdenum content in the active components is 5.0-17.0wt%, the cobalt content is 2.0-7.0wt%, and the phosphorus content is 0.1-3.5wt% based on the mass of the oxide. The active metal components of the catalyst, molybdenum and cobalt, are mainly present in the form of MoCoS, and the catalyst contains more than 3wt% S.

[0065] The preparation method of the macroporous alumina carrier containing CoSnO3 is as follows:

[0066] (1) preparing sodium polyacrylate and styrene-butadiene rubber emulsion: adding sodium polyacrylate to deionized water, then adding styrene-butadiene rubber emulsion, adding acid solution to adjust the pH value to between 4 and 7, and then stirring and dividing into 2 to 5 portions;

[0067] (2) preparing a sodium polyacrylate acid solution: adding acid to adjust the pH value to between 4 and 7, and the pH value is 0.5 to 2 units higher than the pH value of the sodium polyacrylate and styrene-butadiene rubber emulsion prepared in step (1), and the sodium polyacrylate acid solution is divided into 2 to 5 portions;

[0068] (3) Preparation of carrier: Add pseudo-boehmite and a binder such as sesbania powder and CoSnO3 into a kneader and mix evenly, and divide it into 2-5 portions. Take one portion of the pseudo-boehmite mixture, first add one portion of sodium polyacrylate and styrene-butadiene rubber emulsion and deionized water in sequence to the pseudo-boehmite mixture powder and knead evenly; then add sodium polyacrylate acid solution, and then add the second portion of the pseudo-boehmite mixture and a certain amount of acid solution, and knead evenly; then add sodium polyacrylate and styrene-butadiene rubber emulsion, and repeat the above-mentioned adding process until all the pseudo-boehmite mixture, sodium acrylate and styrene-butadiene rubber emulsion and sodium polyacrylate acid solution are added; the repeatedly kneaded materials are extruded, dried and calcined to obtain a macroporous alumina carrier containing CoSnO3.

[0069] The above catalyst calcination process is to calcine at 480-700°C for 4-10 hours to obtain an alumina carrier containing CoSnO3.

[0070] Due to the diversification and inferior quality of gasoline sources, the content of impurities such as gum, sulfur, and arsenic in gasoline has a significant impact on the activity of the catalyst, and may even result in no obvious temperature rise in the catalyst bed and catalyst deactivation. In order to improve the anti-impurity performance of the catalyst, the catalyst is further improved. The present invention also provides a gasoline hydrodesulfurization catalyst, which includes a carrier and an active component. A macroporous alumina carrier is used as the carrier. Based on the carrier, the carrier contains La2Sn3O7 and CoSnO3, the La2Sn3O7 content is 0.5-4.5wt%, the CoSnO3 content is 0.5-3.5wt%, and the alumina content is 75-95wt%. Cobalt, molybdenum and phosphorus are used as active components. Based on the catalyst, the active component molybdenum content in the catalyst is 5.0-17.0wt%, the cobalt content is 2.0-7.0wt%, the nickel content is 2-5.5wt%, and the phosphorus content is 0.1-3.5wt%. In the active components of the catalyst, molybdenum and cobalt are mainly present in the form of MoCoS, and nickel and cobalt are mainly present in the form of NiCoS. The catalyst contains more than 3wt% of S, preferably 3-15wt% of sulfur, and more preferably 3-15wt% of sulfur.

[0071] Further preferably, the catalyst carrier includes La2Sn3O7 with a content of 0.5-3.5wt%, CoSnO3 with a content of 0.5-3.0wt%, and 76.0-88.0wt% Al2O3; the molybdenum content in the active components is 6.0-14.0wt%, the cobalt content is 2.0-5.0wt%, the nickel content is 3-5.5wt%, and the phosphorus content is 0.1-3.0wt%.

[0072] The present invention also provides a method for preparing a gasoline hydrodesulfurization catalyst, which comprises the following steps:

[0073] (1) preparing sodium polyacrylate and styrene-butadiene rubber emulsion: adding a certain amount of sodium polyacrylate into deionized water, then adding styrene-butadiene rubber emulsion, adding acid solution to adjust the pH value to between 4 and 7, and then stirring and dividing into 2 to 5 portions;

[0074] (2) preparing a sodium polyacrylate acid solution: adding acid to adjust the pH value to between 4 and 7, and the pH value is 0.5 to 2 units higher than the pH value of the sodium polyacrylate and styrene-butadiene rubber emulsion prepared in step (1), and the sodium polyacrylate acid solution is divided into 2 to 5 portions;

[0075] (3) Preparation of carrier: Pseudo-boehmite and sesbania powder, La2Sn3O7 and CoSnO3 are added into a kneader and mixed evenly to obtain a mixture containing pseudo-boehmite, which is divided into 2-5 portions. Take one portion of the mixture containing pseudo-boehmite, first add one portion of sodium polyacrylate and styrene-butadiene rubber emulsion and deionized water to the mixture containing pseudo-boehmite in sequence and knead evenly; then add sodium polyacrylate acid solution, and then add the second portion of the mixture containing pseudo-boehmite and a certain amount of acid solution, and knead evenly; then add sodium polyacrylate and styrene-butadiene rubber emulsion, and repeat the above-mentioned adding process until all the pseudo-boehmite mixture, sodium acrylate and styrene-butadiene rubber emulsion and sodium polyacrylate acid solution are added; the repeatedly kneaded materials are extruded, dried and calcined to obtain a macroporous alumina carrier containing CoSnO3.

[0076] (4) Preparation of catalyst precursor: impregnating the carrier with an impregnation solution containing Co, Mo, Ni, P and S, and aging for more than 4 hours to obtain a catalyst precursor;

[0077] (5) Sulfurization: Under closed conditions, reflux the catalyst precursor at 60-80°C for 0.3-2.0 hours, then add a reducing agent, continue to react at 100-150°C for 0.5-10 hours, cool to room temperature, filter, wash with deionized water, and vacuum dry at 80-150°C to obtain the final catalyst product.

[0078] In the method for preparing the gasoline hydrodesulfurization catalyst of the present invention, it is preferred that in step (4), the amount of sulfur added to the impregnation liquid is 85-140% of the theoretical sulfur loading of the catalyst.

[0079] In the present invention, the preparation of La2Sn3O7 is not limited. For example, it can be prepared according to the following method: a lanthanum salt solution is mixed with sodium stannate, the pH is adjusted to 10.5-12 with alkaline solution, and La2Sn3O7 is obtained by aging, filtering, washing, drying, and calcining at 800-950°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0080] Figure 1 This is the pore size distribution diagram of the carrier mercury injection analysis. DETAILED DESCRIPTION

[0081] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.

[0082] The raw materials and reagents used in the present invention are all commercially available products.

[0083] Example 1

[0084] 1. Preparation of macroporous alumina carrier

[0085] Take 450g of pseudo-boehmite and 14g of sesbania powder, add them into a kneader and mix evenly, divide them into 3 portions, one portion of 170g, one portion of 120g, and one portion of 140g, and set aside.

[0086] Weigh 19.8 grams of sodium polyacrylate and add it to deionized water, then add 29.7 grams of styrene-butadiene rubber latex, add acetic acid to adjust the pH value to about 5.5, and divide it into 3 parts after stirring. Sodium polyacrylate accounts for 40% of the mixture of sodium polyacrylate and styrene-butadiene rubber latex, and the mixture of sodium polyacrylate and styrene-butadiene rubber latex accounts for 11% of pseudo-boehmite. Weigh 67.5 grams of sodium polyacrylate, add acetic acid to adjust the pH value to about 6.5, and divide the sodium polyacrylate acid solution into 3 parts, and sodium polyacrylate accounts for 15% of pseudo-boehmite.

[0087] Take a portion of 170g pseudo-boehmite and add it to a container. First, add a portion of sodium polyacrylate and styrene-butadiene rubber emulsion and deionized water to the pseudo-boehmite powder in sequence and knead evenly; then add sodium polyacrylate acid solution, and then add a second portion of 120g pseudo-boehmite and a certain amount of acid solution, and knead evenly; then add sodium polyacrylate and styrene-butadiene rubber emulsion, and repeat the above-mentioned feeding process until all pseudo-boehmite, sodium acrylate, styrene-butadiene rubber emulsion and sodium polyacrylate acid solution are added; the repeatedly kneaded materials are extruded, dried at 120°C, and calcined at 570°C to obtain the alumina carrier Support-1 with a macroporous structure. The physical properties of the final carrier are shown in Table 1.

[0088] 2. Preparation of hydrodesulfurization catalyst 1

[0089] The macroporous alumina carrier Support-1 is used as a carrier, and molybdenum, cobalt, phosphorus and sulfur solutions are prepared according to the active components of the catalyst, molybdenum 12.4wt%, cobalt 2.6wt% and phosphorus 0.5wt% in terms of oxides. The macroporous alumina carrier is impregnated with an impregnation solution containing cobalt nitrate, ammonium molybdate, ammonium phosphomolybdate and ammonium sulfide, and the amount of ammonium sulfide added accounts for 115% of the theoretical sulfur loading of the catalyst. The catalyst is aged for more than 5 hours to obtain a catalyst precursor; the catalyst sulfurization process: the obtained catalyst precursor is added to a round-bottom flask with reflux, the temperature is raised to 70°C and refluxed for 1.0 hour, 56mL of hydrazine hydrate solution is added to the round-bottom flask, and the final catalyst 1 product is obtained by vacuum drying at 130°C. The sulfurization temperature of the sulfurized catalyst of the present invention is low, which avoids the formation of spinel structure between the active metal and the carrier alumina, thereby improving the catalyst reaction activity. The prepared macropores are unevenly distributed in the radial direction of the carrier, and the acid distribution of the carrier is adjusted at the same time.

[0090] Example 2

[0091] 1. Preparation of macroporous alumina carrier

[0092] The preparation process of the macroporous alumina carrier is the same as that of Example 1, except that the pseudo-boehmite, sodium polyacrylate, styrene-butadiene rubber emulsion, and sodium polyacrylate solution are all substantially equally divided into 4 parts, the pH value of sodium polyacrylate and styrene-butadiene rubber emulsion is adjusted to about 5.1, and the pH value of the sodium polyacrylate solution is adjusted to about 6.7, sodium polyacrylate accounts for 20% of the mixture of sodium polyacrylate and styrene-butadiene rubber emulsion, and the mixture of sodium polyacrylate and styrene-butadiene rubber emulsion accounts for 15% of the pseudo-boehmite. Sodium polyacrylate accounts for 22% of the pseudo-boehmite. The final alumina carrier Support-2.

[0093] 2. Preparation of hydrodesulfurization catalyst 2

[0094] The preparation process of the hydrodesulfurization catalyst is the same as that of Example 1, with 13.0 wt% molybdenum, 2.3 wt% cobalt, 0.9 wt% phosphorus, and the amount of ammonium sulfide added accounting for 105% of the theoretical sulfur loading of the catalyst.

[0095] Example 3

[0096] 1. Preparation of macroporous alumina carrier

[0097] The preparation process of the macroporous alumina carrier is the same as that in Example 1. 450g of pseudo-boehmite, 14g of sesbania powder and 14.2g of CoSnO3 are added to a kneader and mixed evenly. The CoSnO3 content in the carrier is 4.5wt%. It is divided into 3 portions, the first portion is 120g, the second portion is 170g, and the third portion is 140g, for later use.

[0098] Dissolve 23.9g SnCl4·5H2O in deionized water to obtain solution (a), and dissolve 23.5g CoCl2·6H2O in deionized water to obtain solution (b). Add solution (b) to solution (a) under stirring and stir evenly, then add NaOH solution and stir evenly, transfer the obtained mixture into a reaction tank, react at 130℃ for 10h, and after cooling, wash and dry the obtained reactant to obtain a precursor powder. The precursor powder is calcined at 700℃ for 2.5h to obtain CoSnO3. CoSnO3 is ground and ultrasonically dispersed for use.

[0099] Sodium polyacrylate and styrene butadiene rubber emulsion and sodium polyacrylate solution are basically divided into 3 parts, the pH value of sodium polyacrylate and styrene butadiene rubber emulsion is adjusted to about 5.8, and the pH value of sodium polyacrylate solution is adjusted to about 6.7. Sodium polyacrylate accounts for 25% of the mixture of sodium polyacrylate and styrene butadiene rubber emulsion, and the mixture of sodium polyacrylate and styrene butadiene rubber emulsion accounts for 25% of pseudo-boehmite. Sodium polyacrylate accounts for 9% of pseudo-boehmite. The final alumina carrier Support-3.

[0100] 2. Preparation of hydrodesulfurization catalyst 3

[0101] The preparation process of the hydrodesulfurization catalyst is the same as that of Example 1, with a molybdenum content of 10.3wt%, a cobalt content of 4.0wt%, a phosphorus content of 0.8wt%, and an amount of ammonium sulfide added accounting for 120% of the theoretical sulfur loading of the catalyst.

[0102] Example 4

[0103] 1. Preparation of macroporous alumina carrier

[0104] First, 57.5g Co(NO3)2·6H20 was dissolved in deionized water at room temperature; then 69g SnCl4·5H2O was dissolved in deionized water, and the SnCl4·5H2O solution was added to the cobalt nitrate solution under stirring, and then the NaOH solution was added and stirred evenly, and the obtained mixture was transferred into a reaction tank, reacted at 130°C for 10h, and after cooling, the obtained reactant was washed and dried to obtain a precursor powder. The precursor powder was calcined at 650°C for 3.5h to obtain CoSnO3. CoSnO3 was ground and ultrasonically dispersed for use. The preparation process of the macroporous alumina carrier is the same as that of Example 3. The pseudo-boehmite, sodium polyacrylate, styrene-butadiene rubber emulsion, and sodium polyacrylate solution are basically divided into three parts. The pH value of sodium polyacrylate and styrene-butadiene rubber emulsion is adjusted to about 5.8, and the pH value of sodium polyacrylate solution is adjusted to about 6.7. Sodium polyacrylate accounts for 25% of the mixture of sodium polyacrylate and styrene-butadiene rubber emulsion, and the mixture of sodium polyacrylate and styrene-butadiene rubber emulsion accounts for 25% of the pseudo-boehmite. Sodium polyacrylate accounts for 9% of the pseudo-boehmite. The CoSnO3 content in the carrier is 3.0wt%, and the final alumina carrier Support-4.

[0105] 2. Preparation of hydrodesulfurization catalyst 4

[0106] The preparation process of the hydrodesulfurization catalyst is the same as that of Example 1, with a molybdenum content of 11.2wt%, a cobalt content of 2.1wt%, a phosphorus content of 0.4wt%, and an amount of ammonium sulfide added accounting for 120% of the theoretical sulfur loading of the catalyst.

[0107] Example 5

[0108] 1. Preparation of macroporous alumina carrier

[0109] The method of containing macroporous alumina carrier is the same as that of Example 3, except that La2Sn3O7 is added, the content of La2Sn3O7 is 3.3wt%, the content of CoSnO3 is 1.7wt%, and the content of alumina is 95wt%.

[0110] 2. Preparation of hydrodesulfurization catalyst 5

[0111] The preparation process of the hydrodesulfurization catalyst is the same as that of Example 3, with a molybdenum content of 11.8wt%, a cobalt content of 2.4wt%, a phosphorus content of 0.6wt%, and a phosphorus content of 0.8wt%. The amount of ammonium sulfide added accounts for 125% of the theoretical sulfur loading of the catalyst.

[0112] Comparative Example 1

[0113] The preparation process is the same as that of Example 1, except that sodium polyacrylate and styrene-butadiene rubber are not added, and the final alumina carrier is Reference.

[0114] Table 1 Physical properties of the final carrier

[0115]

[0116] In Table 1, the macropore ratio is calculated as follows: macropore volume / (macropore volume+nitrogen adsorption and desorption volume)×100%.

[0117] Table 2 Evaluation results of catalytic cracking gasoline

[0118] Analyze Project Sulfur content, mg / kg Desulfurization rate, % Olefin content, v% raw material 162.3 \ 28.5 Catalyst 1 14.7 90.6 24.7 Catalyst 2 14.8 91.3 24.2 Catalyst 3 15.0 92.6 25.2 Catalyst 4 14.8 91.3 25.0 Catalyst 5 13.3 91.8 24.3 Contrast agent 1 31.2 80.8 20.6

[0119] Table 2 shows the evaluation results of the catalyst reaction performance using catalytic cracking gasoline (sulfur content of 110.5 mg / kg, olefin content of 38.2 v%, arsenic content of 121 μg / kg and colloid content of 1.37 mg / mL). The catalysts 1-5 prepared by the present invention have better desulfurization activity and selectivity in the selective hydrodesulfurization reaction of catalytic cracking gasoline. Reaction conditions: 50 ml isothermal bed reactor, temperature 270 ° C, pressure 2.0 MPa, space velocity 3.5 h -1 , hydrogen-oil volume ratio 350:1.

[0120] The Co-Mo-S active phase in the catalyst of the present invention has high dispersion and is prepared at low temperature to avoid the formation of spinel structure between metal and alumina. The catalyst does not undergo high-temperature calcination and is sulfurized in two stages at low temperature. The sulfurization effect is good, the catalyst has high desulfurization activity and good selectivity.

[0121] The catalysts of Examples 3 and 4 effectively control the growth of the cobalt grains loaded, inhibit the aggregation of cobalt grains, promote the modification of the MoS active phase by Co, thereby forming MoCoS, which is beneficial to improving the desulfurization activity, selectivity and stability of the catalyst. The hydrodesulfurization effect is better for raw materials with high sulfur content, and the olefin reduction is low. The catalyst of Example 5 adopts catalytic cracking gasoline (sulfur content is 152mg / kg, olefin content is 36.3v%, arsenic content is 163μg / kg and colloid content is 7.6mg / mL) to carry out performance evaluation after 100h, the catalyst desulfurization rate is more than 90.6%, the olefin content is more than 24.2%, and the catalyst has strong resistance to colloid and impurities such as arsenic and lead.

[0122] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.

Claims

1. A method for preparing a macroporous alumina carrier, characterized in that: The steps include: (1) preparing a mixed solution containing sodium polyacrylate and styrene-butadiene rubber emulsion: adding sodium polyacrylate to deionized water, then adding styrene-butadiene rubber emulsion, and then adding acid solution to adjust the pH value to 4-7, and then stirring and dividing into 2-5 portions; (2) preparing a sodium polyacrylate acid solution: adding sodium polyacrylate to deionized water, adding acid to adjust the pH value to 4-7, and the pH value is 0.5-2 higher than the pH value of the mixed solution containing sodium polyacrylate and styrene-butadiene rubber emulsion prepared in step (1), and dividing the sodium polyacrylate acid solution into 2-5 portions; (3) Preparing a carrier: Pseudo-boehmite and a binder are mixed evenly to obtain a pseudo-boehmite mixture, which is divided into 2-5 portions. One portion of the pseudo-boehmite mixture is added with one portion of a mixed solution containing sodium polyacrylate and styrene-butadiene rubber emulsion and deionized water in sequence, and kneaded evenly. Then, one portion of a sodium polyacrylate acid solution is added, and the above-mentioned adding process is repeated until the pseudo-boehmite mixture, the mixed solution containing sodium acrylate and styrene-butadiene rubber emulsion, and the sodium polyacrylate acid solution are all added. The finally kneaded material is subjected to extrusion molding, drying, and calcination to obtain an alumina carrier having a macroporous structure. Alternately mixing a mixture containing sodium polyacrylate and styrene-butadiene rubber latex, a sodium polyacrylate acid solution and a mixture containing pseudo-boehmite; In the preparation method, the division in steps (1) to (3) is equal or unequal; The pore size distribution of the macroporous alumina carrier is 80-240 nm, the macropore ratio is 10-50%, the macropore volume is 0.2-0.6 mL / g, and the macropores are radially unevenly distributed in the macroporous alumina carrier.

2. The method for preparing a macroporous alumina carrier according to claim 1, characterized in that: The macroporous alumina carrier has a pore size distribution of 90-240 nm, a macropore ratio of 26-44%, and a macropore volume of 0.2-0.6 mL / g.

3. The method for preparing a macroporous alumina carrier according to claim 2, characterized in that: The macroporous alumina carrier has a pore size distribution of 90-150 nm or 130-200 nm, a macropore ratio of 26-44%, a macropore volume of 0.2-0.6 mL / g, and a specific surface area of ​​210-330 m 2 / g.

4. The method for preparing a macroporous alumina carrier according to claim 1, characterized in that: The macroporous alumina carrier also contains 0.5-5.5 wt% of CoSnO3.

5. The method for preparing a macroporous alumina carrier according to claim 1, characterized in that: The macroporous alumina carrier further comprises La2Sn3O7 and CoSnO3. Based on the carrier, the content of La2Sn3O7 in the carrier is 0.5-4.5 wt%, the content of CoSnO3 is 0.5-3.5 wt%, and the content of alumina is 75-95 wt%.

6. The method for preparing a macroporous alumina carrier according to claim 5, characterized in that: The content of La2Sn3O7 in the carrier is 0.5-3.5 wt%, the content of CoSnO3 is 0.5-3.0 wt%, and the content of aluminum oxide is 76.0-88.0 wt%.

7. The method for preparing a macroporous alumina carrier according to claim 1, characterized in that: In step (3), CoSnO3 and / or La2Sn3O7 are added when the pseudo-boehmite and the binder are mixed.

8. The method for preparing a macroporous alumina carrier according to claim 1, characterized in that: In the mixed solution containing sodium polyacrylate and styrene-butadiene rubber emulsion, the content of sodium polyacrylate is 10-40 wt %, and the content of styrene-butadiene rubber emulsion is 2-10 wt %.

9. The method for preparing a macroporous alumina carrier according to claim 8, characterized in that: In step (3), the amount of each portion of the sodium polyacrylate acid solution added is 0.5 to 35.0 wt% per portion of pseudo-boehmite, calculated as sodium polyacrylate; and the amount of each portion of the mixed solution containing sodium polyacrylate and styrene-butadiene rubber emulsion added is 0.1 to 30.0 wt% per portion of pseudo-boehmite, calculated as the total amount of sodium polyacrylate and styrene-butadiene rubber.

10. The method for preparing a macroporous alumina carrier according to claim 9, characterized in that: In step (3), the amount of each portion of the sodium polyacrylate acid solution added is 10.5 to 25.0 wt% of each portion of pseudo-boehmite, calculated as sodium polyacrylate; and the amount of each portion of the mixed solution containing sodium polyacrylate and styrene-butadiene rubber emulsion added is 0.2 to 8.5 wt% of each portion of pseudo-boehmite, calculated as the total amount of sodium polyacrylate and styrene-butadiene rubber.

11. A gasoline hydrodesulfurization catalyst, characterized in that: The macroporous alumina carrier obtained by the preparation method according to any one of claims 1 to 10 is used as a carrier, cobalt, molybdenum and phosphorus are used as active components, and the catalyst is used as a reference. The molybdenum content in the active component is 5.0-17.0 wt %, the cobalt content is 2.0-7.0 wt %, and the phosphorus content is 0.1-3.5 wt %, based on the mass of the oxide. The molybdenum and cobalt in the active components exist in the form of MoCoS, and the catalyst contains more than 3 wt% of S.

12. The gasoline hydrodesulfurization catalyst according to claim 11, characterized in that: Co is based on the weight of CoO, and the content of Co in the carrier is lower than the amount of Co supported on the catalyst.

13. A method for preparing a gasoline hydrodesulfurization catalyst, which is the method for preparing a gasoline hydrodesulfurization catalyst according to any one of claims 11 to 12, characterized in that: The steps include: (1) Preparation of catalyst precursor: impregnating a carrier with an impregnation solution containing Co, Mo, P and S, and aging for more than 4 hours to obtain a catalyst precursor; (2) Sulfidation: Under closed conditions, reflux the catalyst precursor at 60-80 °C for 0.3-2.0 hours, then add a reducing agent and continue to react at 100-150 °C for 0.5-10 hours, cool to room temperature, filter, wash with deionized water, and vacuum dry at 80-150 °C to obtain the final catalyst product.

14. The method for preparing a gasoline hydrodesulfurization catalyst according to claim 13, characterized in that: In step (1), the amount of sulfur added to the impregnation solution is 85-140% of the theoretical sulfur loading of the catalyst.

15. A gasoline hydrodesulfurization catalyst, characterized in that: A macroporous alumina carrier obtained by the preparation method according to any one of claims 1 to 10 is used as a carrier, and cobalt, molybdenum, nickel and phosphorus are used as active components; based on the catalyst and the mass of the oxides, the molybdenum content in the active components is 5.0-17.0 wt %, the cobalt content is 2.0-7.0 wt %, the nickel content is 2-5.5 wt %, and the phosphorus content is 0.1-3.5 wt %. In the active components, molybdenum and cobalt exist in the form of MoCoS, nickel and cobalt mainly exist in the form of NiCoS, and the catalyst contains more than 3 wt % of S.

16. The gasoline hydrodesulfurization catalyst according to claim 15, characterized in that: The catalyst contains 3-15 wt% sulfur.

17. The gasoline hydrodesulfurization catalyst according to claim 16, characterized in that: The catalyst contains 3-8 wt% sulfur.

18. The gasoline hydrodesulfurization catalyst according to claim 16, characterized in that: The active component has a molybdenum content of 6.0-14.0 wt %, a cobalt content of 2.0-5.0 wt %, a nickel content of 3-5.5 wt %, and a phosphorus content of 0.1-3.0 wt %.

19. A method for preparing a gasoline hydrodesulfurization catalyst, which is the method for preparing a gasoline hydrodesulfurization catalyst according to any one of claims 15 to 18, characterized in that: The preparation method comprises the following steps: (1) Preparation of catalyst precursor: impregnating a carrier with an impregnation solution containing Co, Mo, Ni, P and S, and aging for more than 4 hours to obtain a catalyst precursor; (2) Sulfidation: Under closed conditions, reflux the catalyst precursor at 60-80 °C for 0.3-2.0 hours, then add a reducing agent and continue to react at 100-150 °C for 0.5-10 hours, cool to room temperature, filter, wash with deionized water, and vacuum dry at 80-150 °C to obtain the final catalyst product.

20. The method for preparing a gasoline hydrodesulfurization catalyst according to claim 19, characterized in that: In step (1), the amount of sulfur added to the impregnation solution is 85-140% of the theoretical sulfur loading of the catalyst.

Citation Information

Patent Citations

  • Preparation methods for macroporous alumina carrier and hydrodemetallization catalyst

    CN102441437B

  • Preparation method of large pore volume and high strength alumina for ethanol ethylene catalyst

    CN104084182B

  • Quasi-thin empholite composition containing organic reaming agent

    CN1611300A

  • Method for preparing alumina supporter

    CN1768946A

  • Hydrogenation catalyst for desulfurization and removal of heavy metals

    US4448896A