Resin composition, modifier and composition containing the modifier

By using resin compositions of ethylene-vinyl acetate copolymers with different vinyl acetate contents and ethylene-acrylic acid or ethylene-methacrylic acid copolymers, the problem of insufficient mechanical properties of various resin laminates is solved, and the resistance of resin is improved Impactivity and elongation of breaking achieve efficient reuse of a variety of resins.

CN114075357BActive Publication Date: 2024-12-03TOSOH CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110935189.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-17
Filing Date
2021-08-16
Publication Date
2024-12-03
Estimated Expiration
2041-08-16

AI Technical Summary

Technical Problem

In the reuse of plastics, the mechanical properties of various resin laminates are insufficient, resulting in insufficient impact resistance and elongation of break, and problems of increasing viscosity, yellowing and odor, limiting the use of recycled resins.

Method used

The resin composition containing ethylene-vinyl acetate copolymers with different vinyl acetate content and ethylene-acrylic acid or ethylene-methacrylic acid copolymers as modifiers is used to improve the resin composition by adjusting the proportion and mixing ratio of the copolymer. Compatibility and physical properties.

Benefits of technology

It significantly improves the impact resistance and elongation of breaking resin molded products, effectively reuses plastic waste from various resins, and improves the use performance of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004982570820000131
    Figure GDA0004982570820000131
  • Figure GDA0004982570820000171
    Figure GDA0004982570820000171
  • Figure GDA0004982570820000201
    Figure GDA0004982570820000201
Patent Text Reader

Abstract

The technical problem and purpose of the present invention is to provide a resin composition that can be used as a modifier, wherein the modifier can be used to overcome the brittleness of plastic materials containing multiple resins, such as a laminate of different types of materials that are recycled, and can improve impact resistance and elongation at break. The means for solving the above technical problems of the present invention is a resin composition (A) containing the following components (1) and (2): (1) a composition (a1) containing at least two ethylene-vinyl acetate copolymers with different vinyl acetate contents; (2) a copolymer (a2) of at least one selected from ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition and a molded article comprising the same. Background Art

[0002] In recent years, concerns about environmental pollution caused by plastics have increased, promoting the material recycling of plastic products. In the material recycling of plastics, most of the recycled plastic waste is melted and restored to raw material pellets, or recycled into consumables such as pallets. At this time, if the recycled plastic waste is reused in a state where different types of plastics are mixed, there is a problem that the physical properties of the recycled plastic deteriorate due to poor compatibility between them. Therefore, the current procedure is to sort the recycled plastic waste according to each raw material and recycle it into products.

[0003] However, in multilayer films and multilayer containers, etc., in which different types of plastics are laminated, it is difficult to separate each raw material, and therefore they cannot be reused and are currently disposed of in landfills or incinerated.

[0004] In such a background, as a means of recycling the composite resin in a stacked state, the addition of a compatibilizer has been studied. For example, the use of an ionomer resin as a compatibilizer has been studied to composite and reuse PE-PET and PP-ABS (Patent Document 1). In addition, the use of an oxazoline-based compatibilizer has been studied to composite and reuse PE-PET, etc. (Patent Document 2). Further, the composite recycling of PE-EVOH has also been studied (Patent Document 3). According to these documents, it is shown that by adding a compatibilizer, the physical properties of the composite of PE and PET, EVOH, etc. can be improved.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2001-220473

[0008] Patent Document 2: Japanese Patent Application Publication No. 2004-182957

[0009] Patent Document 3: Japanese Patent Application No. 2009-535452 Summary of the invention

[0010] Technical problem to be solved by the invention

[0011] However, the mechanical properties of the recycled resins obtained by these methods are not sufficient, so it is necessary to develop a technology that can further improve the mechanical properties. In addition, due to problems such as increased viscosity, yellowing and odor, there are problems such as poor recyclability and restrictions on the use of recycled resins.

[0012] The present invention is made in view of the above-mentioned technical problems, and its purpose is to provide a resin composition that can be used as a modifier, wherein the modifier is used to overcome the brittleness of plastic materials containing multiple resins such as laminates of different types of materials for recycling and reuse, and to improve impact resistance and elongation at break.

[0013] Means for solving technical problems

[0014] The present inventors have conducted intensive studies to solve the above-mentioned technical problems, and as a result, have found that a resin composition comprising two ethylene-vinyl acetate copolymers having different vinyl acetate contents and either an ethylene-acrylic acid copolymer or an ethylene-methacrylic acid copolymer can be suitably used as a resin modifier capable of improving the impact resistance and elongation at break of a brittle material comprising a plurality of resin components, thereby completing the present invention.

[0015] That is, the present invention is a resin composition (A) comprising the following components (1) and (2).

[0016] (1) Composition (a1) comprising at least two ethylene-vinyl acetate copolymers having different vinyl acetate contents

[0017] (2) a copolymer (a2) of at least one selected from ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers

[0018] Effects of the Invention

[0019] According to the present invention, a resin composition that is excellent in the effect of improving impact resistance and elongation at break and is useful as a modifier for resin molded products requiring these physical properties can be provided. In particular, by using the resin composition, plastic waste containing a variety of resins can be effectively recycled. DETAILED DESCRIPTION

[0020] Hereinafter, the resin composition (A) which is one aspect of the present invention will be described in detail.

[0021] The resin composition (A) of the present invention contains a composition (a1) comprising at least two ethylene-vinyl acetate copolymers having different vinyl acetate contents (hereinafter referred to as “EVA composition (a1)”).

[0022] The vinyl acetate content of each ethylene-vinyl acetate copolymer in the EVA composition (a1) is preferably 5% by weight or more and 85% by weight or less. The vinyl acetate content can be measured by the method of JIS K6924-1.

[0023] As the production method of ethylene-vinyl acetate copolymer, known production methods such as high pressure free radical polymerization, solution polymerization and emulsion polymerization can be cited. In addition, such resin can be easily selected from commercially available products. As ethylene-vinyl acetate copolymer, it is sold by Tosoh Corporation under the trade name of ULTRASEN, and by LANXESS Co., Ltd. under the trade name of Levapren and Levamelt.

[0024] In the EVA composition (a1), the differences in the vinyl acetate content of the various copolymers are all preferably 1% by weight or more, more preferably 5% by weight or more. Thus, when the resin composition (A) is added as a modifier to the thermoplastic resin (B), the compatibility is further improved, and the impact resistance and elongation at break of the obtained composition are improved.

[0025] In addition, in the EVA composition (a1), when the difference in the vinyl acetate content of various copolymers is taken, it is preferred that the difference in the vinyl acetate content of at least one group of copolymers is 40% by weight or less. Thus, the compatibility between the ethylene-vinyl acetate copolymers constituting the resin composition (A) is further improved, and when the ethylene-vinyl acetate copolymers are added to the thermoplastic resin (B) as a modifier, the impact resistance and elongation at break of the resin are further improved. The difference in the vinyl acetate content of at least one group of copolymers is preferably 30% by weight or less, more preferably 20% by weight or less, and most preferably 15% by weight or less.

[0026] Here, the difference in vinyl acetate content of various copolymers in the EVA composition (a1), for example, in a composition containing three types of ethylene-vinyl acetate copolymers having vinyl acetate contents of 25 wt%, 50 wt%, and 80 wt% (hereinafter, the vinyl acetate contents are expressed as VAc25, VAc50, and VAc80, respectively), can be calculated as follows.

[0027] VAc50-VAc25=25 wt%

[0028] VAc80-VAc50=30 wt%

[0029] VAc80-VAc25=55 wt%

[0030] The EVA composition (a1) preferably comprises at least three ethylene-vinyl acetate copolymers having different vinyl acetate contents.

[0031] In order to satisfy the above conditions, the ethylene-vinyl acetate copolymer constituting the EVA composition (a1) can be adjusted by mixing two or more, preferably three or more. If an ethylene-vinyl acetate copolymer having a vinyl acetate content of N wt% (N is a positive number less than 100) is denoted as VAcN, and the composition of the components is represented by (+), for example, (VAc15+VAc25), (VAc25+VAc40), (VAc25+VAc50), (VAc50+VAc80), (VAc15+VAc25+VAc50), (VAc25+VAc50+VAc80), (VAc15+VAc25+VAc50+VAc70), (VAc15+VAc25+VAc50+VAc80), (VAc15+VAc25+VAc50+VAc70+VAc80), etc. can be exemplified.

[0032] The resin composition (A) of the present invention comprises a copolymer (a2) (hereinafter referred to as "copolymer (a2)") of at least one selected from ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers. In one aspect, copolymer (a2) is any one of ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers.

[0033] The acrylic acid content or methacrylic acid content of copolymer (a2) is preferably 3 mol% or more and 15 mol% or less. In the case where copolymer (a2) contains both ethylene-acrylic acid copolymer and ethylene-methacrylic acid copolymer, the total amount of acrylic acid content and methacrylic acid content is preferably 3 mol% or more and 15 mol% or less.

[0034] Copolymer (a2) may be one type of copolymer or two or more types of copolymers. Here, "copolymer (a2) contains two or more types of copolymers" means (i) the copolymer (a2) is an ethylene-acrylic acid copolymer, and two or more types of ethylene-acrylic acid copolymers are used; (ii) the copolymer (a2) is an ethylene-methacrylic acid copolymer, and two or more types of ethylene-methacrylic acid copolymers are used; and (iii) the copolymer (a2) is an ethylene-acrylic acid copolymer and an ethylene-methacrylic acid copolymer. Both ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers may be used. Further, in the case of (iii), the ethylene-acrylic acid copolymer and the ethylene-methacrylic acid copolymer may be one type, or two or more types may be used.

[0035] In the resin composition (A) of the present invention, the absolute value of the difference between the solubility parameter (hereinafter referred to as "SP value") calculated by the Fedors method (Polym. Eng. Sci., 14, 147 (1974)) of at least one ethylene-vinyl acetate copolymer constituting the EVA composition (a1) and the copolymer (a2) is preferably 0.3 (MPa).1 / 2 As a result, the compatibility between the ethylene-vinyl acetate copolymer composition (a1) and the copolymer (a2) in the resin composition (A) is improved, and the impact resistance and elongation at break of the obtained composition are improved.

[0036] In addition, when the copolymer (a2) contains two or more types, it is sufficient that the above conditions are satisfied in terms of the relationship with any one of the copolymers (a2). In addition, it is more preferable that the above conditions are satisfied in terms of the relationship with any one of the copolymers (a2).

[0037] Here, if the SP value of each component is calculated by the Fedors method, for example, the SP values ​​of four ethylene-vinyl acetate copolymers having vinyl acetate contents of 15 wt%, 25 wt%, 50 wt%, and 80 wt%, an ethylene-acrylic acid copolymer having an acrylic acid content of 20 wt% (= 9 mol%), and an ethylene-methacrylic acid copolymer having a methacrylic acid content of 11 wt% (= 4 mol%) can be calculated as follows.

[0038] Ethylene-vinyl acetate copolymer with a vinyl acetate content of 15% by weight = 18.0 (MPa) 1 / 2 Ethylene-vinyl acetate copolymer with a vinyl acetate content of 25% by weight = 18.3 (MPa) 1 / 2 Ethylene-vinyl acetate copolymer with a vinyl acetate content of 50% by weight = 19.3 (MPa) 1 / 2 Ethylene-vinyl acetate copolymer with a vinyl acetate content of 80% by weight = 20.6 (MPa) 1 / 2 Ethylene-methacrylic acid copolymer with methacrylic acid content of 4 mol% = 18.2 (MPa) 1 / 2

[0039] Ethylene-acrylic acid copolymer with an acrylic acid content of 9 mol% = 19.2 (MPa) 1 / 2

[0040] For example, in the case where the resin composition (A) contains an ethylene-methacrylic acid copolymer (SP value = 18.2 (MPa)) having a methacrylic acid content of 4 mol % 1 / 2 ) as the copolymer (a2), by using at least an ethylene-vinyl acetate copolymer having a vinyl acetate content of 25% by weight (18.3 (MPa) 1 / 2 ), the absolute value of the difference between the SP value of copolymer (a2) and that of copolymer (a2) is 0.3 (MPa) 1 / 2 Similarly, in an ethylene-acrylic acid copolymer (19.2 (MPa) containing 9 mol% of acrylic acid, 1 / 2) as the copolymer (a2), by using at least an ethylene-vinyl acetate copolymer having a vinyl acetate content of 50% by weight (19.3 (MPa) 1 / 2 ), the absolute value of the difference between the SP value of copolymer (a2) and that of copolymer (a2) is 0.3 (MPa) 1 / 2 the following.

[0041] In the resin composition (A) of this aspect, the mixing ratio of EVA composition (a1) and copolymer (a2) preferably includes 50% by weight or more and 99% by weight or less of EVA composition (a1), 1% by weight or more and 50% by weight or less of copolymer (a2) (herein, the total amount of (a1) and (a2) is calculated as 100% by weight), preferably includes 70% by weight or more and 90% by weight or less of EVA composition (a1), 10% by weight or more and 30% by weight or less of copolymer (a2) (herein, the total amount of (a1) and (a2) is calculated as 100% by weight). By including 50% by weight or more and 99% by weight or less of EVA composition (a1), the compatibility and impact resistance of the resin to be matched are further improved. On the other hand, by including 1% by weight or more and 50% by weight or less of copolymer (a2), the compatibility of the resin to be matched is further improved.

[0042] Hereinafter, the modifying agent which is one aspect of the present invention will be described in detail.

[0043] The present invention provides a modifier comprising a resin composition (A) (hereinafter referred to as “the modifier of the present invention”).

[0044] By adding the resin composition (A) of the present invention as a modifier to a resin as a masterbatch, the impact resistance of the resin can be improved. In addition, when the masterbatch to be mixed is composed of resins of multiple components, the compatibility between the components can be improved.

[0045] The modifier of the present invention can be used in any form such as pellets or powder.

[0046] The masterbatch (hereinafter referred to as "thermoplastic resin (B)") used for the modifier of the present invention is preferably selected from at least one of polyolefin resins, acrylic resins, polyamide resins, polyester resins, polycarbonate resins, polystyrene resins and styrene-acrylonitrile copolymers, and more preferably a composition containing at least two of them, from the viewpoint of excellent compatibility with the modifier. Here, the composition of the thermoplastic resin (B) does not include the components of the EVA composition (a1) and the copolymer (a2).

[0047] Examples of the polyolefin resin include high-density polyethylene, low-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-propylene copolymers, ethylene-vinyl alcohol copolymers, ethylene-acrylate copolymers, ethylene-methacrylate copolymers, polybutadiene, and polyisoprene.

[0048] Examples of the acrylic resin include polyacrylic acid, polymethyl acrylate, polyethyl acrylate, polybutyl acrylate, polyoctyl acrylate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, and polyoctyl methacrylate.

[0049] Examples of the polyamide-based resin include nylon 6, nylon 6,6, nylon 11, and nylon 12.

[0050] Examples of the polyester resin include polyethylene terephthalate, glycol-modified polyethylene terephthalate resin (PETG resin), polybutylene terephthalate, polylactic acid (including poly-L-lactic acid, poly-D-lactic acid, a copolymer of L-lactic acid and D-lactic acid, and a stereocomplex of poly-L-lactic acid and poly-D-lactic acid), polybutylene succinate, poly(butylene succinate / adipate), polyethylene succinate, poly(butylene succinate / terephthalate), poly(adipate / terephthalate), poly(hydroxybutyrate / hydroxycaproate), polyglycolic acid, poly-3-hydroxybutyrate, and polycaprolactone.

[0051] Among them, from the viewpoint of large improvement in impact resistance and elongation at break when blended with the resin composition (A), the thermoplastic resin constituting the thermoplastic resin (B) is preferably at least one selected from high-density polyethylene, low-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl alcohol copolymer, nylon 6, nylon 6,6, nylon 11, nylon 12, polyethylene terephthalate, glycol-modified polyethylene terephthalate resin (PETG resin), polybutylene terephthalate, polylactic acid (including poly-L-lactic acid, poly-D-lactic acid, a copolymer of L-lactic acid and D-lactic acid, and a stereocomplex of poly-L-lactic acid and poly-D-lactic acid) and polybutylene succinate.

[0052] As the thermoplastic resin constituting the thermoplastic resin (B), it is more preferable to be at least one selected from high-density polyethylene, low-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl alcohol copolymer, nylon 6, nylon 6,6, nylon 11, nylon 12, polyethylene terephthalate, glycol-modified polyethylene terephthalate resin (PETG resin) and polybutylene terephthalate.

[0053] The thermoplastic resin (B) may be an unused virgin resin or a resin obtained by recycling a used molded article. That is, it includes a form in which all of one or more resins are virgin resins, a form in which at least one of one or more resins is a used resin, and a form in which all of one or more resins are used resins.

[0054] When the thermoplastic resin (B) is a resin obtained by recycling a used molded body, it may contain a plurality of resins. In this case, it may contain organic impurities such as vinyl chloride resin, wax, adhesive, plasticizer and antioxidant. On the other hand, it may also contain inorganic impurities such as fillers.

[0055] Regarding the mixing ratio of the resin composition (A) and the thermoplastic resin (B), it is preferred to include a thermoplastic resin (B) of more than 50% by weight and less than 99% by weight, and a resin composition (A) of more than 1% by weight and less than 50% by weight. The impact resistance of the resin composition obtained by including less than 99% by weight of the thermoplastic resin (B) is excellent. On the other hand, the rigidity of the resin composition obtained by including more than 50% by weight of the thermoplastic resin (B) is excellent. It is further preferred to include a thermoplastic resin (B) of more than 60% by weight and less than 95% by weight, and a resin composition (A) of more than 5% by weight and less than 40% by weight, and it is further preferred to include a thermoplastic resin (B) of more than 70% by weight and less than 95% by weight, and a resin composition (A) of more than 5% by weight and less than 30% by weight.

[0056] When the modifier of the present invention is blended into a thermoplastic resin (B), a resin composition (C) in which the modifier is blended into a thermoplastic resin (B) can be produced by a production method having a kneading step of kneading the modifier and the thermoplastic resin (B).

[0057] As the kneading method, there can be mentioned a method of kneading the modifier and various materials constituting the thermoplastic resin (B) simultaneously using a kneading device; and a method of kneading only the modifier in advance, then blending the kneaded modifier into the thermoplastic resin (B), and further kneading. In the latter method, the modifier is more uniformly mixed, and the desired physical properties can be stably obtained, so it is preferred.

[0058] As a mixing device, there is no particular limitation as long as each component can be uniformly dispersed, and a mixing device of a commonly used resin can be used. For example, mixing devices such as a single screw extruder, a twin screw extruder, a multi-screw extruder, a Banbury mixer, a pressure kneader, a rotating roller, and an internal mixer can be cited. Among them, from the viewpoint of excellent dispersibility and continuous productivity, a twin screw extruder is more preferably used.

[0059] The screw speed when mixing with a twin-screw extruder is not particularly limited, preferably mixing with more than 50rpm and less than 3000rpm, more preferably more than 300rpm and less than 3000rpm. If the screw speed is more than 50rpm, the dispersibility of each component mixed is improved, and the physical property of the obtained resin is excellent, so it is preferred. In addition, if the screw speed is less than 3000rpm, the deterioration of the resin caused by excessive shearing heat will not occur, so the physical property of the obtained resin is excellent, so it is preferred.

[0060] When using a forcing machine in the mixing step, the resin composition after the mixing with the forcing machine, preferably the resin composition after the mixing with the high-speed shearing condition of more than the aforementioned 50rpm and below 3000rpm can be used as raw material. In addition, the molded body obtained by directly extruding the forcing machine can be used as a molded product.

[0061] The kneading temperature is preferably from the melting point of the component with the lowest melting point in the thermoplastic resin (B) to about 300° C. If the thermoplastic resin (B) is an amorphous resin, it is preferably from the glass transition temperature to about 300° C.

[0062] Hereinafter, the resin composition (C) comprising the resin composition (A) and the thermoplastic resin (B) which is one aspect of the present invention will be described in detail.

[0063] The resin composition (C) of the present invention comprises the resin composition (A) and the thermoplastic resin (B). That is, it has the same meaning as what is obtained by blending the modifier of the present invention into the thermoplastic resin (B).

[0064] The composition of this aspect may contain antistatic agents, light stabilizers, ultraviolet absorbers, nucleating agents, lubricants, antioxidants, anti-blocking agents, fluidity improvers, release agents, flame retardants, colorants, inorganic neutralizers, hydrochloric acid absorbers, fillers, conductive agents, chain extenders and anti-hydrolysis agents, etc. without impairing the effects of the present invention.

[0065] When the resin composition (C) of the present invention contains components other than the resin composition (A) and the thermoplastic resin (B), the total of (A) and (B) can be taken as 100 parts by weight, and the content of the component can be expressed as the amount added relative to the above 100 parts by weight. In other words, the expression "to % by weight" of (A) and (B) indicates the ratio of (A) to (B), and the ratio of the other components can be defined separately.

[0066] Furthermore, the resin composition (C) of the present aspect can be used in any form such as pellets or powder.

[0067] The resin composition (C) of the present invention may be molded by any method, and examples thereof include random extrusion, film, sheet, blow molding, injection, foaming, extrusion coating, and rotational molding.

[0068] The molded articles comprising the resin composition (C) of the present invention can be used in various applications such as automobile parts, housings of electric and electronic parts, building materials, civil engineering members, agricultural materials, containers, packaging materials, adhesives, and daily necessities.

[0069] Example

[0070] Hereinafter, the present invention will be described by way of Examples and Comparative Examples, but the present invention is not limited thereto.

[0071] (1) Melt flow rate (MFR)

[0072] The MFR of the ethylene-vinyl acetate copolymer, the ethylene-acrylic acid copolymer, the ethylene-methacrylic acid copolymer and the thermoplastic resin (B) was measured using a melt indexer (manufactured by Takara Industries) at 190°C and a load of 2.16 kg.

[0073] (2) Vinyl acetate content

[0074] The vinyl acetate content is measured in accordance with JIS K6924-1.

[0075] (3) SP value

[0076] The SP values ​​of the ethylene-vinyl acetate copolymer, the ethylene-acrylic acid copolymer, and the ethylene-methacrylic acid copolymer were calculated by the Fedors method.

[0077] (4) Impact strength

[0078] The impact strength was measured in accordance with JIS P 8134. The press-formed sheet with a thickness of 0.1 mm was tested using a film impact tester (manufactured by Toyo Seiki; FT-M model) at a test capacity of 3 J and a hemispherical hammer at the puncture tip.

[0079] (5) Tensile test

[0080] The sheet with a thickness of 0.1 mm after press forming is punched into a dumbbell-shaped test piece of ASTM D-1822-L. The dimensions of the test piece are 63.5 mm in total length, 9.53 mm in parallel length, 3.18 mm in parallel width, 0.1 mm in thickness, and 9.53 mm in clamp width. The test piece is measured using a TENSILON tensile tester (ORIENTEC; RTE-1210) under the conditions of a distance between the clamps of 30 mm and a tensile speed of 200 mm / min. The point at which the sample breaks is recorded as the elongation at break (elongation at break [%] = tensile length required for break [mm] / distance between the clamps of 30 mm), and the stress at the time of break is recorded as the breaking stress.

[0081] Example 1

[0082] As the resin composition (A), a resin composition having the following composition was used.

[0083] [Resin composition (A)]

[0084] 65 wt% of ethylene-vinyl acetate copolymer (a1-25) having a vinyl acetate content of 25 wt% and a melt mass flow rate of 3 g / 10 min (manufactured by Tosoh Corporation; trade name ULTRASEN 640)

[0085] 10% by weight of an ethylene-vinyl acetate copolymer (a1-50) having a vinyl acetate content of 50% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by LANXESS Co., Ltd.; trade name: Levapren 500)

[0086] · Ethylene-acrylic acid copolymer (a2-9) having an acrylic acid content of 9 mol% and a melt mass flow rate of 300 g / 10 min (SK Sogo Chemical; trade name SK Primacor 5980I) 25 wt%

[0087] The above resin composition was dry-blended and melt-kneaded using a twin-screw extruder with a screw diameter of 25 mm (manufactured by TECHNOVEL; trade name ULTnano25TW) at a resin temperature of 160° C. and a screw rotation speed of 150 rpm to obtain pellets of a resin composition (A).

[0088] As the thermoplastic resin (B), a thermoplastic resin composition having the following composition was used.

[0089] [Composition of thermoplastic resin (B)]

[0090] · Low-density polyethylene (B-1) having a melt mass flow rate of 3 g / 10 min and a melting point of 111° C. (manufactured by Tosoh Corporation; trade name: PETROSEN 205) 70% by weight

[0091] Ethylene-vinyl alcohol copolymer (B-4) having an ethylene content of 35 mol% and a melting point of 177°C (manufactured by KURARAY CO., LTD.; trade name EVAL C109B) 30 wt%

[0092] 80 wt% of the thermoplastic resin (B) composition and 20 wt% of the resin composition (A) were dry-blended and melt-kneaded using a twin-screw extruder with a screw diameter of 25 mm (manufactured by TECHNOVEL; trade name ULTnano25TW) at a resin temperature of 200°C and a screw speed of 300 rpm to obtain a composition.

[0093] The obtained composition was press-molded using a press-molding machine (manufactured by Shinto Metal Industry; AWFA-50 model) under the conditions of a pressure of 10 MPa, a heating temperature of 200°C (first pressurization × 3 minutes, second pressurization × 3 minutes), and a cooling temperature of 25°C (4 minutes) to obtain a pressurized sheet with a thickness of 0.1 mm.

[0094] The obtained pressurized sheet was used to carry out an impact test and a tensile test. The evaluation results are shown in Table 1.

[0095] Example 2

[0096] As the thermoplastic resin (B), a thermoplastic resin composition having the following composition was used.

[0097] [Composition of thermoplastic resin (B)]

[0098] · Low-density polyethylene (B-1) having a melt mass flow rate of 3 g / 10 min and a melting point of 111° C. (manufactured by Tosoh Corporation, trade name PETROSEN 205) 70% by weight

[0099] Nylon 6 (B-5) with a melting point of 220°C (manufactured by Ube Industries, Ltd.; trade name: UBE NYLON 1022D) 30% by weight

[0100] 80 wt% of the composition of the thermoplastic resin (B) and 20 wt% of the resin composition (A) described in Example 1 are dry-blended and melt-kneaded using a twin-screw extruder with a screw diameter of 25 mm (manufactured by TECHNOVEL; trade name ULTnano25TW) at a resin temperature of 230°C and a screw speed of 300 rpm to obtain a composition.

[0101] The obtained composition was press-molded using a press-molding machine (AWFA-50 model manufactured by Shinto Metal Industries, Ltd.) under the conditions of a pressure of 10 MPa, a heating temperature of 230°C (first pressurization × 3 minutes, second pressurization × 3 minutes), and a cooling temperature of 25°C (4 minutes) to obtain a pressurized sheet with a thickness of 0.1 mm.

[0102] The obtained pressurized sheet was used to carry out an impact test and a tensile test. The evaluation results are shown in Table 1.

[0103] Example 3

[0104] As the thermoplastic resin (B), a thermoplastic resin composition having the following composition was used.

[0105] [Composition of thermoplastic resin (B)]

[0106] · Low-density polyethylene (B-1) having a melt mass flow rate of 3 g / 10 min and a melting point of 111° C. (manufactured by Tosoh Corporation, trade name PETROSEN 205) 70% by weight

[0107] · Polyethylene terephthalate (B-6) with a melting point of 255°C (manufactured by UNITIKA Corporation; MA-2103) 30% by weight

[0108] The thermoplastic resin (B) composition was dry-blended and melt-kneaded using a twin-screw extruder with a screw diameter of 25 mm (manufactured by TECHNOVEL; trade name ULTnano25TW) at a resin temperature of 270°C and a screw speed of 150 rpm to obtain pellets of the thermoplastic resin (B).

[0109] 80 wt% of the obtained thermoplastic resin (B) is dry-blended with 20 wt% of the resin composition (A) described in Example 1, and melt-kneaded using a twin-screw extruder with a screw diameter of 25 mm (manufactured by TECHNOVEL; trade name ULTnano25TW) at a resin temperature of 230°C and a screw speed of 300 rpm to obtain a composition.

[0110] The obtained composition was press-molded using a press-molding machine (manufactured by Shinto Metal Industry; AWFA-50 model) under the conditions of a pressure of 10 MPa, a heating temperature of 230°C (first pressurization × 3 minutes, second pressurization × 3 minutes), and a cooling temperature of 25°C (4 minutes) to obtain a pressurized sheet with a thickness of 0.1 mm.

[0111] The obtained pressurized sheet was used to carry out an impact test and a tensile test. The evaluation results are shown in Table 1.

[0112] Example 4

[0113] A pressed sheet was obtained in the same manner as in Example 3 except that a thermoplastic resin composition having the following composition was used as the thermoplastic resin (B).

[0114] [Composition of thermoplastic resin (B)]

[0115] · Low-density polyethylene (B-1) having a melt mass flow rate of 3 g / 10 min and a melting point of 111° C. (manufactured by Tosoh Corporation; trade name: PETROSEN 205) 70% by weight

[0116] 10 wt% of ethylene-vinyl alcohol copolymer (B-4) having an ethylene content of 35 mol% and a melting point of 177°C (manufactured by KURARAY CO., LTD.; trade name EVAL C109B)

[0117] Nylon 6 (B-5) with a melting point of 220°C (manufactured by Ube Industries, Ltd.; trade name: UBE NYLON 1022D) 10% by weight

[0118] · Polyethylene terephthalate (B-6) with a melting point of 255°C (manufactured by UNITIKA Corporation; MA-2103) 10% by weight

[0119] The obtained pressurized sheet was used to carry out an impact test and a tensile test. The evaluation results are shown in Table 1.

[0120] Example 5

[0121] A pressed sheet was obtained in the same manner as in Example 1 except that a resin composition having the following composition was used as the resin composition (A).

[0122] [Resin composition (A)]

[0123] · Ethylene-vinyl acetate copolymer (a1-15) having a vinyl acetate content of 15% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by Tosoh Corporation; trade name ULTRASEN 626) 33% by weight

[0124] · Ethylene-vinyl acetate copolymer (a1-25) having a vinyl acetate content of 25% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by Tosoh Corporation; trade name ULTRASEN 640) 32% by weight

[0125] 10% by weight of an ethylene-vinyl acetate copolymer (a1-50) having a vinyl acetate content of 50% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by LANXESS Co., Ltd.; trade name: Levapren 500)

[0126] · Ethylene-acrylic acid copolymer (a2-9) having an acrylic acid content of 9 mol% and a melt mass flow rate of 300 g / 10 min (SK Sogo Chemical; trade name SK Primacor 5980I) 25 wt%

[0127] The obtained pressurized sheet was used to carry out an impact test and a tensile test. The evaluation results are shown in Table 1.

[0128] Example 6

[0129] A pressed sheet was obtained by the same procedure as in Example 2 except that the resin composition described in Example 5 was used as the resin composition (A).

[0130] The obtained pressurized sheet was used to carry out an impact test and a tensile test. The evaluation results are shown in Table 1.

[0131] Example 7

[0132] A pressed sheet was obtained by the same procedure as in Example 3 except that the resin composition described in Example 5 was used as the resin composition (A).

[0133] The obtained pressurized sheet was used to carry out an impact test and a tensile test. The evaluation results are shown in Table 1.

[0134] Example 8

[0135] A pressed sheet was obtained by the same procedure as in Example 4 except that the resin composition described in Example 5 was used as the resin composition (A).

[0136] The obtained pressurized sheet was used to carry out an impact test and a tensile test. The evaluation results are shown in Table 1.

[0137]

Table 1

[0138]

[0139] Example 9

[0140] A pressed sheet was obtained in the same manner as in Example 8 except that the thermoplastic resin (B) was changed to 90% by weight and the resin composition (A) was changed to 10% by weight.

[0141] The obtained pressurized sheet was used to carry out an impact test and a tensile test.

[0142] Example 10

[0143] A pressed sheet was obtained in the same manner as in Example 8 except that the thermoplastic resin (B) was changed to 95% by weight and the resin composition (A) was changed to 5% by weight.

[0144] The obtained pressurized sheet was used to carry out an impact test and a tensile test.

[0145] Embodiment 11

[0146] A pressed sheet was obtained in the same manner as in Example 4 except that a resin composition having the following composition was used as the resin composition (A).

[0147] [Resin composition (A)]

[0148] · Ethylene-vinyl acetate copolymer (a1-15) having a vinyl acetate content of 15% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by Tosoh Corporation; trade name ULTRASEN 626) 25% by weight

[0149] · Ethylene-vinyl acetate copolymer (a1-25) having a vinyl acetate content of 25% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by Tosoh Corporation; trade name ULTRASEN 640) 25% by weight

[0150] 10% by weight of an ethylene-vinyl acetate copolymer (a1-50) having a vinyl acetate content of 50% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by LANXESS Co., Ltd.; trade name: Levapren 500)

[0151] · Ethylene-acrylic acid copolymer (a2-9) having an acrylic acid content of 9 mol% and a melt mass flow rate of 300 g / 10 min (SK Sogye Chemical Co., Ltd.; trade name SK Primacor 5980I) 40 wt%

[0152] The obtained pressurized sheet was used to carry out an impact test and a tensile test.

[0153] Example 12

[0154] A pressed sheet was obtained in the same manner as in Example 4 except that a resin composition having the following composition was used as the resin composition (A).

[0155] [Resin composition (A)]

[0156] · Ethylene-vinyl acetate copolymer (a1-15) having a vinyl acetate content of 15% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by Tosoh Corporation; trade name ULTRASEN 626) 33% by weight

[0157] · Ethylene-vinyl acetate copolymer (a1-25) having a vinyl acetate content of 25% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by Tosoh Corporation; trade name ULTRASEN 640) 32% by weight

[0158] 10% by weight of an ethylene-vinyl acetate copolymer (a1-50) having a vinyl acetate content of 50% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by LANXESS Co., Ltd.; trade name: Levapren 500)

[0159] · Ethylene-methacrylic acid copolymer (a2-4) having a methacrylic acid content of 4 mol% and a melt mass flow rate of 10 g / 10 min (manufactured by DOW-MITSUI CHEMICAL; trade name NUCREL 1108C) 25 wt%

[0160] The obtained pressurized sheet was used to carry out an impact test and a tensile test.

[0161] Embodiment 13

[0162] A pressed sheet was obtained in the same manner as in Example 4 except that a resin composition having the following composition was used as the resin composition (A).

[0163] [Resin composition (A)]

[0164] · Ethylene-vinyl acetate copolymer (a1-15) having a vinyl acetate content of 15% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by Tosoh Corporation; trade name ULTRASEN 626) 23% by weight

[0165] · Ethylene-vinyl acetate copolymer (a1-25) having a vinyl acetate content of 25% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by Tosoh Corporation; trade name ULTRASEN 640) 22% by weight

[0166] 10% by weight of an ethylene-vinyl acetate copolymer (a1-50) having a vinyl acetate content of 50% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by LANXESS Co., Ltd.; trade name: Levapren 500)

[0167] · Ethylene-vinyl acetate copolymer (a1-80) having a vinyl acetate content of 80% by weight and a melt mass flow rate of 5 g / 10 min (manufactured by LANXESS Co., Ltd.; trade name: Levapren 800) 20% by weight

[0168] · Ethylene-acrylic acid copolymer (a2-9) having an acrylic acid content of 9 mol% and a melt mass flow rate of 300 g / 10 min (SK Sogo Chemical; trade name SK Primacor 5980I) 25 wt%

[0169] The obtained pressurized sheet was used to carry out an impact test and a tensile test.

[0170] Embodiment 14

[0171] A pressed sheet was obtained in the same manner as in Example 8 except that a thermoplastic resin composition having the following composition was used as the thermoplastic resin (B).

[0172] [Composition of thermoplastic resin (B)]

[0173] · Linear low-density polyethylene (B-2) having a melt mass flow rate of 0.8 g / 10 min and a melting point of 122° C. (manufactured by Tosoh Corporation; trade name: NIPOLON-L F15R) 70% by weight

[0174] · Ethylene-vinyl alcohol copolymer (B-4) having an ethylene content of 35 mol% and a melting point of 177°C (manufactured by KURARAY CO., LTD.; trade name EVAL C109B) 10 wt%··

[0175] ·Nylon 6 (B-5) with a melting point of 220°C (manufactured by Ube Industries, Ltd.; trade name: UBE NYLON 1022D) 10 wt%·

[0176] · Polyethylene terephthalate (B-6) with a melting point of 255°C (manufactured by UNITIKA Co., Ltd.; MA-2103) 10 wt%·

[0177] The obtained pressurized sheet was used to carry out an impact test and a tensile test.

[0178] Embodiment 15

[0179] A pressed sheet was obtained in the same manner as in Example 8 except that a thermoplastic resin composition having the following composition was used as the thermoplastic resin (B).

[0180] [Composition of thermoplastic resin (B)]

[0181] High-density polyethylene (B-3) having a melt mass flow rate of 5.5 g / 10 min and a melting point of 133° C. (manufactured by Tosoh Corporation; trade name: NIPOLONHARD 4020) 70% by weight

[0182] 10 wt% of ethylene-vinyl alcohol copolymer (B-4) having an ethylene content of 35 mol% and a melting point of 177°C (manufactured by KURARAY CO., LTD.; trade name EVAL C109B)

[0183] Nylon 6 (B-5) with a melting point of 220°C (manufactured by Ube Industries, Ltd.; trade name: UBE NYLON 1022D) 10% by weight

[0184] · Polyethylene terephthalate (B-6) with a melting point of 255°C (manufactured by UNITIKA Co., Ltd.; MA-2103) 10 wt%·

[0185] The obtained pressurized sheet was used to carry out an impact test and a tensile test.

[0186]

Table 2

[0187]

[0188] Comparative Example 1

[0189] A pressed sheet was obtained in the same manner as in Example 1 except that the resin composition (A) was not blended and only the following thermoplastic resin (B) composition was used.

[0190] [Composition of thermoplastic resin (B)]

[0191] · Low-density polyethylene (B-1) having a melt mass flow rate of 3 g / 10 min and a melting point of 111° C. (manufactured by Tosoh Corporation; trade name: PETROSEN 205) 70% by weight

[0192] Ethylene-vinyl alcohol copolymer (B-4) having an ethylene content of 35 mol% and a melting point of 177°C (manufactured by KURARAY CO., LTD.; trade name EVAL C109B) 30 wt%

[0193] The obtained pressurized sheet was used to carry out an impact test and a tensile test. The evaluation results are shown in Table 3.

[0194] Comparative Example 2

[0195] A pressed sheet was obtained in the same manner as in Example 2 except that the resin composition (A) was not blended and only the following thermoplastic resin (B) composition was used.

[0196] [Composition of thermoplastic resin (B)]

[0197] · Low-density polyethylene (B-1) having a melt mass flow rate of 3 g / 10 min and a melting point of 111° C. (manufactured by Tosoh Corporation; trade name: PETROSEN 205) 70% by weight

[0198] Nylon 6 (B-5) with a melting point of 220°C (manufactured by Ube Industries, Ltd.; trade name: UBE NYLON 1022D) 30% by weight

[0199] The obtained pressurized sheet was used to carry out an impact test and a tensile test. The evaluation results are shown in Table 3.

[0200] Comparative Example 3

[0201] A pressed sheet was obtained in the same manner as in Example 3 except that the resin composition (A) was not blended and only the following thermoplastic resin (B) composition was used.

[0202] [Composition of thermoplastic resin (B)]

[0203] · Low-density polyethylene (B-1) having a melt mass flow rate of 3 g / 10 min and a melting point of 111° C. (manufactured by Tosoh Corporation; trade name: PETROSEN 205) 70% by weight

[0204] · Polyethylene terephthalate (B-6) with a melting point of 255°C (manufactured by UNITIKA Corporation; MA-2103) 30% by weight·

[0205] The obtained pressurized sheet was used to carry out an impact test and a tensile test. The evaluation results are shown in Table 3.

[0206] Comparative Example 4

[0207] A pressed sheet was obtained in the same manner as in Example 4 except that the resin composition (A) was not blended and only the following thermoplastic resin (B) composition was used.

[0208] [Composition of thermoplastic resin (B)]

[0209] · Low-density polyethylene (B-1) having a melt mass flow rate of 3 g / 10 min and a melting point of 111° C. (manufactured by Tosoh Corporation; trade name: PETROSEN 205) 70% by weight

[0210] 10 wt% of ethylene-vinyl alcohol copolymer (B-4) having an ethylene content of 35 mol% and a melting point of 177°C (manufactured by KURARAY CO., LTD.; trade name EVAL C109B)

[0211] Nylon 6 (B-5) with a melting point of 220°C (manufactured by Ube Industries, Ltd.; trade name: UBE NYLON 1022D) 10% by weight

[0212] · Polyethylene terephthalate (B-6) with a melting point of 255°C (manufactured by UNITIKA Corporation; MA-2103) 10% by weight

[0213] The obtained pressurized sheet was used to carry out an impact test and a tensile test. The evaluation results are shown in Table 3.

[0214] Comparative Example 5

[0215] A pressed sheet was obtained in the same manner as in Example 4 except that a resin composition having the following composition was used as the resin composition (A).

[0216] [Resin composition (A)]

[0217] 65% by weight of an ethylene-vinyl acetate copolymer (a1-15) having a vinyl acetate content of 15% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by Tosoh Corporation; trade name ULTRASEN 626)

[0218] · 35 wt% of ethylene-vinyl acetate copolymer (a1-80) (Lavapren 800, manufactured by LANXESS Co., Ltd.) having a vinyl acetate content of 80 wt% and a melt mass flow rate of 5 g / 10 min. The obtained pressed sheet was used to perform an impact test and a tensile test. The evaluation results are shown in Table 3.

[0219] Comparative Example 6

[0220] A pressed sheet was obtained in the same manner as in Example 4 except that a resin composition having the following composition was used as the resin composition (A).

[0221] [Resin composition (A)]

[0222] · Ethylene-vinyl acetate copolymer (a1-15) having a vinyl acetate content of 15% by weight and a melt mass flow rate of 3 g / 10 min (manufactured by Tosoh Corporation; trade name ULTRASEN 626) 75% by weight

[0223] · Ethylene-acrylic acid copolymer (a2-9) having an acrylic acid content of 9 mol% and a melt mass flow rate of 300 g / 10 min (SK Sogo Chemical; trade name SK Primacor 5980I) 25 wt%

[0224] The obtained pressurized sheet was used to carry out an impact test and a tensile test. The evaluation results are shown in Table 3.

[0225]

Table 3

[0226]

Claims

1. A resin composition (A) comprising the following components (1) and (2): (1) a composition (a1) comprising at least two ethylene-vinyl acetate copolymers having different vinyl acetate contents; (2) a copolymer (a2) of at least one selected from ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers, in, The total content of acrylic acid and methacrylic acid is 3 mol% or more and 15 mol% or less, When the total amount of the composition (a1) and the copolymer (a2) is 100 wt %, the content of the composition (a1) is 50 wt % or more and 99 wt % or less, and the content of the copolymer (a2) is 1 wt % or more and 50 wt % or less, The absolute value of the difference between the solubility parameter, i.e., the SP value, calculated by the Fedors method of at least one ethylene-vinyl acetate copolymer constituting the composition (a1) and the SP value calculated by the Fedors method of at least one of the ethylene-acrylic acid copolymer and the ethylene-methacrylic acid copolymer in the copolymer (a2) is 0.3 (MPa) 1 / 2 the following.

2. The resin composition (A) according to claim 1, in, The composition (a1) contains three or more ethylene-vinyl acetate copolymers having different vinyl acetate contents.

3. The resin composition (A) according to claim 1 or 2, in, In the composition (a1), when the difference in vinyl acetate content of various copolymers is taken, the difference in vinyl acetate content of at least one set of copolymers is 40% by weight or less.

4. Use of the resin composition (A) according to any one of claims 1 to 3 as a modifier for compatibilizing at least two types of resins.

5. A resin composition (C) comprising 1% by weight or more and 50% by weight or less of the resin composition (A) according to any one of claims 1 to 3, and 50% by weight or more and 99% by weight or less of a thermoplastic resin (B), in, The total amount of (B) and (A) is 100% by weight.

6. The resin composition (C) according to claim 5, in, The thermoplastic resin (B) contains at least one selected from the group consisting of polyolefins, polyesters, acrylic resins, polyamides, polycarbonates, polystyrenes, and styrene-acrylonitrile copolymers.

7. The resin composition (C) according to claim 5 or 6, in, The thermoplastic resin (B) is at least one selected from high-density polyethylene, low-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl alcohol copolymer, nylon 6, nylon 6,6, nylon 11, nylon 12, polyethylene terephthalate, glycol-modified polyethylene terephthalate resin, polybutylene terephthalate, polylactic acid and polybutylene succinate.

8. The resin composition (C) according to claim 7, in, The polylactic acid is poly-L-lactic acid, poly-D-lactic acid, a copolymer of L-lactic acid and D-lactic acid, or a stereocomplex of poly-L-lactic acid and poly-D-lactic acid.

9. The resin composition (C) according to claim 7, in, The thermoplastic resin (B) is at least one selected from high-density polyethylene, low-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl alcohol copolymer, nylon 6, nylon 6,6, nylon 11, nylon 12, polyethylene terephthalate, glycol-modified polyethylene terephthalate resin and polybutylene terephthalate.

10. The resin composition (C) according to claim 5 or 6, in, The thermoplastic resin (B) contains two or more types of resins.

11. The resin composition (C) according to claim 5 or 6, in, The thermoplastic resin (B) includes a used molded product.

12. A method for producing a resin composition (C) according to any one of claims 5 to 11, comprising a kneading step of kneading a thermoplastic resin (B) and the resin composition (A) according to any one of claims 1 to 3 using a twin-screw extruder.

13. The method for producing the resin composition (C) according to claim 12, in, The kneading step is performed under the condition that the screw rotation speed of the twin-screw extruder is 50 rpm or more and 3000 rpm or less. 14 . A molded product obtained by molding the resin composition (C) according to claim 5 .