Wave-absorbing glass microspheres and preparation method and application thereof
By filling the absorbing material in the capsule with the resin and curing agent, forming a coating and applying it to hollow glass microbeads, the problem of insufficient absorption performance and uniformity of the foam glue at the joints of the absorbing structural parts is solved. , the strong absorbing performance and material uniformity at the joints are achieved, ensuring the improvement of the absorbing effect.
Patent Information
- Application Number
- CN202010865480.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-08-25
AI Technical Summary
When existing wave absorbing structural parts use foam glue at the joints, uneven foaming leads to the impact of wave absorbing performance, and the foam glue lacks wave absorbing function, resulting in unnecessary miscellaneous peaks.
The absorbent material is filled in the capsule with mixed resin and curing agent to form a coating, applied onto hollow glass microbeads and cured to form absorbent glass microbeads, and the gap is filled through a double-tube glue gun, utilizing its lightweight and Uniformity improves wave absorption performance.
The strong absorbing performance and material uniformity at the joints are achieved, and the miscellaneous peak problems caused by uneven pores are avoided, ensuring lightweight and efficient absorbing effects, especially the flat plate reflectivity in the 8-12GHz frequency band -15.5dB~-16.5dB.
Smart Images

Figure CN114085041B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of aircraft wave-absorbing fillers, and in particular to wave-absorbing glass microbeads and a preparation method and application thereof. Background Art
[0002] When currently manufacturing absorbing structural parts, there are gaps and seams at the absorbing splicing plates. Such seams will affect the absorbing performance. Currently, foam glue is mainly used for filling. However, on the one hand, foam glue has no absorbing function, and on the other hand, the foaming is uneven, which will produce unnecessary peaks and affect the overall absorbing effect.
[0003] Therefore, there is still a need to provide a lightweight absorbing material suitable for filling gaps or joints. Summary of the invention
[0004] The main purpose of the present invention is to provide a wave-absorbing glass microbead and a preparation method and application thereof, so as to solve the problem in the prior art that the foam glue at the joint affects the wave-absorbing effect.
[0005] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a method for preparing absorbing glass microspheres is provided, the preparation method comprising: filling absorbing material into capsules to obtain capsule absorbing material; mixing the capsule absorbing material, resin and curing agent to form a coating; coating the coating on hollow glass microspheres and curing the coating to obtain absorbing glass microspheres.
[0006] Furthermore, the absorbing material, resin, dispersant and curing agent are mixed to form a coating; preferably, in parts by weight, the absorbing material is 40 to 60 parts, the dispersant is 3 to 5 parts, the curing agent is 1 to 2 parts and the resin is 33 to 56 parts; preferably, the absorbing material is selected from any one or more of carbon nanotubes, superconducting carbon black and graphene; preferably, the resin is a modified epoxy resin.
[0007] Furthermore, the diameter of the hollow glass microspheres is 5 to 10 μm. Preferably, the coating is applied to the hollow glass microspheres by spraying and then cured to obtain the absorbing glass microspheres. Preferably, the thickness of the spraying is 20 to 50 μm. Preferably, the curing is thermal curing, more preferably curing at 120 to 150° C., and further preferably the curing time is 1 to 5 hours.
[0008] In order to achieve the above object, according to a second aspect of the present invention, there is provided a wave-absorbing glass micro-bead, which is prepared by any of the above-mentioned preparation methods.
[0009] According to a third aspect of the present invention, there is provided an absorbing filler, which comprises: 60 to 90 parts of any one of the above-mentioned absorbing glass microbeads, 3 to 4 parts of a dispersant, 1 to 2 parts of a curing agent and 6 to 36 parts of a resin.
[0010] Furthermore, the resin is a modified epoxy resin.
[0011] According to a fourth aspect of the present invention, a method for caulking a radar-absorbing splicing material is provided, the method comprising: loading any one of the above-mentioned radar-absorbing fillers into an inner glue gun barrel of a double-tube glue gun; loading structural glue into an outer glue gun barrel of a double-tube glue gun; and caulking the double-tube glue gun by simultaneously extruding.
[0012] Furthermore, the diameter of the spray gun mouth of the inner rubber gun barrel is 100 to 500 μm.
[0013] According to a fifth aspect of the present invention, there is provided an absorbing splicing material, wherein the gaps of the absorbing splicing plate are filled with any of the above-mentioned filling methods.
[0014] Furthermore, the minimum plate reflectivity of the absorbing spliced plate in the frequency band of 8 to 12 GHz is -15.5 dB to -16.5 dB.
[0015] By applying the technical solution of the present invention, a lightweight absorbing material is placed in a capsule, which is then mixed with a resin and a curing agent to form a coating, and the coating is applied to the surface of hollow glass microspheres to form absorbing glass microspheres. When the coating is used to fill gaps in absorbing materials, the absorbing glass microspheres have strong absorbing properties, and the uniformity of the glass microspheres can ensure uniform material at the gaps, avoiding the generation of mixed peaks due to uneven pores, and the inner hollowness ensures lightness. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0017] Figure 1 A schematic diagram showing a packing method according to an embodiment of the present invention; and
[0018] Figure 2 A schematic diagram showing the test materials and methods for the performance of the wave absorbing filler of the present application;
[0019] Figure 3 The absorbing filler of Example 1 of the present application is shown. Figure 2 The absorption performance after the gap is shown. DETAILED DESCRIPTION
[0020] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0021] In order to improve the influence of the existing foam glue on the absorbing performance, in a typical embodiment of the present application, a method for preparing absorbing glass microspheres is provided, and the preparation method comprises: filling absorbing material into capsules to obtain capsule absorbing material; mixing the capsule absorbing material, resin and curing agent to form a coating; coating the coating on hollow glass microspheres and curing them to obtain absorbing glass microspheres.
[0022] The absorbing glass microbeads are formed by placing a lightweight absorbing material in a capsule, then mixing it with a resin and a curing agent to form a coating, and then applying the coating to the surface of the glass microbeads. When the coating is used to fill the gaps in the absorbing material, it has strong absorbing properties. The uniformity of the glass microbeads can ensure the uniformity of the material in the gaps, avoid the generation of mixed peaks due to uneven pores, and the hollow inside ensures lightness.
[0023] In order to further improve the dispersibility and fluidity of the absorbing material in the resin, in a preferred embodiment, the above-mentioned preparation method includes: mixing the absorbing material, the resin, the dispersant and the curing agent to form a coating. Adding the dispersant helps to improve the uniformity of the dispersion of the material in the system. The proportion of each component is preferably, by weight, 40 to 60 parts of the absorbing material, 3 to 5 parts of the dispersant, 1 to 2 parts of the curing agent and 33 to 56 parts of the resin; the coating formed under this proportion has good fluidity and can form a uniformly coated absorbing material layer on the glass microbeads.
[0024] The above-mentioned absorbing material, from the perspective of strong absorbing performance and light weight, is preferably any one or more of carbon nanotubes, superconducting carbon black and graphene, which are light and strong absorbing materials and can ensure absorbing performance. Preferably, the resin is a modified epoxy resin.
[0025] The size of the glass microspheres is not particularly limited, as long as they can be filled evenly and have wave absorbing properties. In a preferred embodiment, the diameter of the hollow glass microspheres is 5 to 10 μm. Glass microspheres of this diameter have the advantages of uniform coating and filling of the absorbing material and light weight.
[0026] The above-mentioned method of coating the absorbing material on the glass beads is not limited, and can be applied by coating or spraying. In the present application, it is preferred to apply the coating on the glass beads by spraying and then solidify to obtain the absorbing glass beads. The thickness of the spraying can be reasonably selected as needed. Preferably, the thickness of the spraying is 0.1 to 1 mm. Depending on the specific resin material used, the curing method may also be different. In a preferred embodiment of the present application, the curing is thermal curing, more preferably curing at 120 to 150°C, and further preferably the curing time is 1 to 5 hours. Under this curing condition, most resins can be cured at different spraying thicknesses.
[0027] In a second typical embodiment of the present application, a wave-absorbing glass microbead is provided, which is prepared by any of the above-mentioned preparation methods. The glass microbead prepared by the above-mentioned method has a wave-absorbing material coating on the surface, so it has strong wave-absorbing performance. Therefore, when used as a caulking material, the gap not only has wave-absorbing performance, but also has relatively uniform wave-absorbing performance at the gap due to the uniform size of the glass microbeads.
[0028] In a third typical embodiment, an absorbing filler is provided, which includes: 60 to 90 parts of the above-mentioned improved absorbing glass microspheres, 3 to 4 parts of dispersants, 1 to 2 parts of curing agents and 6 to 36 parts of resins. The absorbing filler adopts the above-mentioned weight parts of glass microspheres with absorbing material coating as the main filler, and the above-mentioned weight parts of dispersants are used to improve the fluidity and dispersion uniformity of the coating when the absorbing filler is used to fill the gap. Under the action of the above-mentioned weight parts of resin and curing agent, the gap is filled and then cured to complete the filling of the gap. Such absorbing material, as a filling material for the joint, not only plays a filling role, but also has light weight and strong absorbing performance. The above-mentioned resin is a modified epoxy resin.
[0029] In a fourth typical embodiment, a method for caulking a wave-absorbing splicing material is provided, the method comprising: loading the wave-absorbing filler into the inner ring glue gun barrel of a double-tube glue gun; loading the structural glue into the outer ring glue gun barrel of the double-tube glue gun; and simultaneously extruding the double-tube glue gun to perform caulking.
[0030] The above-mentioned caulking method is to load glass microbeads with light wave-absorbing properties into the inner glue barrel of the double-tube glue gun, and load structural glue into the outer glue barrel of the double-tube glue gun, and extrude them at the same time when in use. The inner ring glue gun barrel extrude fillers containing wave-absorbing glass microbeads, which can be as high as possible. For example: if wave-absorbing glass microbeads and adhesive glue are used for bonding, the proportion of glue increases, and the present invention is equivalent to wrapping hollow glass microbeads inside, and there is no adhesive between the hollow glass microbeads, and the outermost glue is used to bond with the periphery of the gap. There is no need to consider the adhesion, and the bonding is guaranteed by the structural glue of the outer glue gun. The outer glue gun barrel extrude structural glue to ensure close bonding with the edge of the gap and strong bonding force.
[0031] In a preferred caulking method, the diameter of the spray gun nozzle of the inner ring glue gun tube is 100-500 μm. The spray gun nozzle of this diameter helps to control the extrusion amount of glass micro beads, thereby facilitating the arrangement of the glass micro beads to be more orderly and more conducive to filling.
[0032] In a fifth typical embodiment, an absorbing splicing material is provided, and the gaps of the absorbing splicing plate are filled with any of the above-mentioned caulking methods. The above-mentioned double-tube glue gun is used, the outer tube structural glue ensures the bonding force, and the inner tube glue gun can extrude the highly filled absorbing material, and the absorbing material with light weight and strong absorbing effect of carbon nanotubes (CNTs), superconducting carbon black, and graphene is coated on the outer surface of glass beads to form absorbing glass beads. The uniformity of the glass beads can ensure the uniformity of the absorbing filler, avoid uneven gaps, and the inner hollow ensures lightness. The problem of uneven foaming of the absorbing foaming material and the influence of the absorbing effect by the mixed peaks is solved.
[0033] Since the above-mentioned absorbing splicing material uses fillers with lightweight absorbing properties at the joints, the flat plate reflectivity of the absorbing splicing plate in the frequency band of 8 to 12 GHz is -8.5 to -16 dB.
[0034] The following will further illustrate the beneficial effects of the present application in conjunction with specific embodiments. Figure 1 Follow the steps shown.
[0035] Example 1
[0036] 1. Take carbon nanotubes (CNTs), superconducting carbon black or graphene as raw materials, mix them with dispersants, curing agents and resins to prepare coatings, and evenly spray them on the surface of hollow glass microspheres, wherein the weight ratio of each component is 40 parts of absorbing materials, 3 parts of dispersants, 1 part of curing agents, and 56 parts of resins (modified epoxy resins). The diameter of the hollow glass microspheres is 5 microns, and the spraying thickness is 20 microns. The sprayed hollow glass microspheres are placed in an oven for curing, the curing temperature is 120°C, and the curing time is 5 hours to obtain absorbing hollow glass microspheres.
[0037] 2. Mix 60 parts of wave-absorbing hollow glass microspheres, 3 parts of dispersant, 1 part of curing agent, and 36 parts of resin evenly and put them into the inner ring glue gun barrel of the double-tube glue gun. The resin is modified epoxy resin, and the diameter of the spray gun nozzle of the inner ring glue gun barrel is 100 microns.
[0038] 3. Load the structural adhesive into the outer ring glue gun barrel.
[0039] 4. When filling the gap, the inner and outer ring glue gun barrels are extruded at the same time. The inner ring glue gun barrel extrudes fillers containing microwave-absorbing hollow glass beads. The filler can be as high as possible without considering bonding. The bonding is guaranteed by the structural glue of the outer ring glue gun. The outer ring glue gun barrel extrudes structural glue, which ensures a close bond with the edge of the gap and has strong bonding force.
[0040] Example 2
[0041] 1. Take carbon nanotubes (CNTs), superconducting carbon black or graphene as raw materials, mix them with dispersants, curing agents and resins to prepare coatings, and evenly spray them on the surface of hollow glass microspheres, wherein the weight ratio of each component is 60 parts of absorbing materials, 5 parts of dispersants, 2 parts of curing agents, and 33 parts of resins (modified epoxy resins). The diameter of the hollow glass microspheres is 10 microns, and the spraying thickness is 50 microns. The sprayed hollow glass microspheres are placed in an oven for curing at a curing temperature of 150°C and a curing time of 1 hour to obtain absorbing hollow glass microspheres.
[0042] 2. Mix 90 parts of wave-absorbing hollow glass microspheres, 4 parts of dispersant, 2 parts of curing agent, and 6 parts of resin evenly and put them into the inner ring glue gun barrel of the double-tube glue gun. The resin is modified epoxy resin, and the diameter of the spray gun nozzle of the inner ring glue gun barrel is 500 microns.
[0043] 3. Load the structural adhesive into the outer ring glue gun barrel.
[0044] 4. When filling the gap, the inner and outer ring glue gun barrels are extruded at the same time. The inner ring glue gun barrel extrudes fillers containing microwave-absorbing hollow glass beads. The filler can be as high as possible without considering bonding. The bonding is guaranteed by the structural glue of the outer ring glue gun. The outer ring glue gun barrel extrudes structural glue, which ensures a close bond with the edge of the gap and has strong bonding force.
[0045] Example 3
[0046] 1. Take carbon nanotubes (CNTs), superconducting carbon black or graphene as raw materials, mix them with dispersants, curing agents and resins to prepare coatings, and evenly spray them on the surface of hollow glass microspheres, wherein the weight ratio of each component is 50 parts of absorbing materials, 4 parts of dispersants, 2 parts of curing agents, and 44 parts of resins (modified epoxy resins). The diameter of the hollow glass microspheres is 8 microns, and the thickness of the spraying is 22 microns. The hollow glass microspheres after spraying are placed in an oven for curing, the curing temperature is 135°C, and the curing time is 3 hours to obtain absorbing hollow glass microspheres.
[0047] 2. Mix 80 parts of microwave-absorbing hollow glass microspheres, 3 parts of dispersant, 1 part of curing agent, and 16 parts of resin evenly and put them into the inner ring glue gun barrel of the double-tube glue gun. The resin is modified epoxy resin, and the diameter of the spray gun nozzle of the inner ring glue gun barrel is 310 microns.
[0048] 3. Load the structural adhesive into the outer ring glue gun barrel.
[0049] 4. When filling the gap, the inner and outer ring glue gun barrels are extruded at the same time. The inner ring glue gun barrel extrudes fillers containing microwave-absorbing hollow glass beads. The filler can be as high as possible without considering bonding. The bonding is guaranteed by the structural glue of the outer ring glue gun. The outer ring glue gun barrel extrudes structural glue, which ensures a close bond with the edge of the gap and has strong bonding force.
[0050] Example 4
[0051] 1. Take carbon nanotubes (CNTs), superconducting carbon black or graphene as raw materials, mix them with dispersants, curing agents and resins to prepare coatings, and evenly spray them on the surface of hollow glass microspheres, wherein the weight ratio of each component is 50 parts of absorbing materials, 4 parts of dispersants, 2 parts of curing agents, and 44 parts of resins (modified epoxy resins). The diameter of the hollow glass microspheres is 10 microns, and the spraying thickness is 40 microns. The sprayed hollow glass microspheres are placed in an oven for curing, the curing temperature is 135°C, and the curing time is 3 hours to obtain absorbing hollow glass microspheres.
[0052] 2. Mix 95 parts of wave-absorbing hollow glass microspheres, 1 part of dispersant, 1 part of curing agent, and 3 parts of resin evenly and put them into the inner ring glue gun barrel of the double-tube glue gun. The resin is modified epoxy resin, and the diameter of the spray gun nozzle of the inner ring glue gun barrel is 500 microns.
[0053] 3. Load the structural adhesive into the outer ring glue gun barrel.
[0054] 4. When filling the gap, the inner and outer ring glue gun barrels are extruded at the same time. The inner ring glue gun barrel extrudes fillers containing microwave-absorbing hollow glass beads. The filler can be as high as possible without considering bonding. The bonding is guaranteed by the structural glue of the outer ring glue gun. The outer ring glue gun barrel extrudes structural glue, which ensures a close bond with the edge of the gap and has strong bonding force.
[0055] Comparative Example 1
[0056] 1. Mix 95 parts of hollow glass microspheres (5 μm in diameter), 1 part of dispersant, 1 part of curing agent, and 3 parts of resin evenly and put them into the inner ring glue gun barrel of a double-tube glue gun. The resin is modified epoxy resin, and the diameter of the spray gun nozzle of the inner ring glue gun barrel is 30 μm.
[0057] 2. Load the structural adhesive into the outer ring glue gun barrel.
[0058] 3. When filling the gap, the inner and outer ring glue gun barrels extrude at the same time. The inner ring glue gun barrel extrude fillers containing microwave-absorbing hollow glass beads. The filler can be as high as possible without considering bonding. The bonding is guaranteed by the structural glue of the outer ring glue gun. The outer ring glue gun barrel extrude structural glue to ensure close bonding with the edge of the gap and strong bonding force.
[0059] test:
[0060] On the 180*180mm*1mm absorbing patch, press Figure 2 As shown, a 1 mm wide gap is cut off in the middle, and then the gap is filled with foam glue and the absorbing filler of Example 1 of the present invention respectively. The test results are compared as shown in the figure below. Figure 3 As shown. Figure 3It can be seen that compared with the absorbing patch without slits, the peak reflectivity of the absorbing patch with the gap filled with foam glue in the frequency range of 8 to 12 GHz increases from nearly -17dB to nearly -14.5dB, and the absorbing effect decreases by 2.5dB. However, with the absorbing filler of the present application, the peak reflectivity of the absorbing patch increases from nearly -17dB to nearly -16.5dB, and the absorbing effect decreases by less than 1dB.
[0061] The test results of Examples 1 to 4 and Comparative Example 1 are shown in Table 1:
[0062] Table 1
[0063] Example Minimum plate reflectivity Uncut Absorbing Patch -17dB Filling foam -14.5dB Example 1 -16.0dB Example 2 -16.3dB Example 3 -16.5dB Example 4 -15.5dB Comparative Example 1 -15.1dB
[0064] From the above description, it can be seen that the above-mentioned embodiments of the present invention achieve the following technical effects: by using carbon nanotubes (CNTs), superconducting carbon black or graphene, which are lightweight and highly absorbing materials, as raw materials, and mixing them with dispersants, curing agents and resins to prepare absorbing coatings, the absorbing coatings are sprayed on the uniform surface of hollow glass microspheres, thereby forming absorbing glass microspheres. The absorbing hollow glass microspheres of the present application are used as raw materials for caulking materials, and are mixed with dispersants, curing agents and resins to prepare absorbing fillers. The absorbing filler has the characteristics of being lightweight and uniform, and it and the structural adhesive are respectively loaded into the inner and outer ring glue gun barrels of the double-tube glue gun barrel, and extruded at the same time when filling the gap, which can not only achieve the function of connecting the gap, but also the gap connection after curing has the same lightweight and uniform strong absorbing performance, avoiding the phenomenon of uneven pores produced by existing foam glue causing the generation of mixed peaks.
[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for filling seams of a wave-absorbing splicing material, characterized in that: The caulking method comprises: Install the wave-absorbing filler into the inner glue gun barrel of the double-tube glue gun; Loading structural adhesive into the outer glue gun barrel of the double-barrel glue gun; The double-tube glue gun is used to extrude and fill the gaps simultaneously; The absorbing filler comprises: 60-90 parts of absorbing glass microspheres, 3-4 parts of dispersant, 1-2 parts of curing agent and 6-36 parts of resin; the preparation method of the absorbing glass microspheres comprises: Filling the absorbing material into the capsule to obtain the capsule absorbing material; Mixing the capsule absorbing material, resin and curing agent to form a coating; The coating is coated on hollow glass microspheres and then cured to obtain the wave-absorbing glass microspheres; The absorbing material is selected from any one or more of carbon nanotubes, superconducting carbon black and graphene; The resin is a modified epoxy resin; The diameter of the spray gun mouth of the inner rubber gun barrel is 100-500 μm.
2. The caulking method according to claim 1, characterized in that: The diameter of the hollow glass microspheres is 5-10 μm.
3. The caulking method according to claim 1, characterized in that: The wave-absorbing glass microspheres are obtained by coating the coating on the hollow glass microspheres in a spraying manner and then curing the coating.
4. The caulking method according to claim 1, characterized in that: The spraying thickness is 20-50 μm.
5. The caulking method according to claim 1, characterized in that: The curing is performed at 120-150° C., and the curing time is 1-5 hours.
6. A wave-absorbing splicing material, characterized in that: The gaps of the wave-absorbing splicing plate are filled with the gap-filling method described in any one of claims 1 to 5.