A kind of thermoplastic medium voltage cable insulation material and preparation method thereof

Through the combination of ethylene propylene copolymerization modified polypropylene material and antioxidant, the catalytic synthesis is carried out using a gas-phase reactor and an extruder to solve the performance instability and environmental pollution problems of cross-linked polyethylene in cable insulating materials, and realizes the The production of green and environmentally friendly cable insulation materials has high efficiency, low consumption and excellent performance.

CN114106504BActive Publication Date: 2024-11-26CHINA ELECTRIC POWER RESEARCH INSTITUTE CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111039674.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-06
Publication Date
2024-11-26
Estimated Expiration
2041-09-06

AI Technical Summary

Technical Problem

The insulating materials used in extruded cables have problems such as unstable insulation performance, high production energy consumption, low efficiency and environmental pollution, which are difficult to meet the energy conservation, environmental protection and dual carbon goals.

Method used

Using thermoplastic medium voltage cable insulating material, modified polypropylene material through ethylene propylene copolymerization, combined with antioxidant and anti-copper agent, and catalytic synthesis-copolymerization-extrusion granulation using gas-phase reactor and extruder to avoid cross-section Coupling and degassing treatment simplifies process steps.

Benefits of technology

It realizes the production of green and friendly cable insulation materials, reduces energy losses and carbon emissions, shortens supply cycles, has excellent mechanical and electrical properties, avoids pollution, and is suitable for use in medium-voltage power cables.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114106504B_ABST
    Figure CN114106504B_ABST
Patent Text Reader

Abstract

The present application discloses a thermoplastic medium-voltage cable insulation material and a preparation method thereof. The thermoplastic medium-voltage cable insulation material comprises the following components in parts by weight: 100 parts of copolymer modified polypropylene, 0.5 to 1 part of antioxidant, and 0.5 to 1 part of anti-copper agent. The present application adopts copolymer modified polypropylene, which is a thermoplastic environmentally friendly material, green and friendly, and does not require cross-linking and degassing treatment during the cable extrusion process, which greatly simplifies the process steps, reduces energy loss and carbon emissions, and shortens the cable supply cycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of novel power transmission and distribution equipment, and in particular to a thermoplastic medium-voltage cable insulation material and a preparation method thereof. Background Art

[0002] Cross-linked polyethylene (XLPE) has excellent mechanical and electrical properties and is currently the main insulation material for extruded cables. However, since XLPE is a heat-fixed material, it needs to be cross-linked by a cross-linking agent or chemical action. The by-products produced during the cross-linking process, such as acetophenone, cumyl alcohol methane and water, are small molecules with low boiling points, which can cause unstable cable insulation and affect the performance of the cable. At the same time, the cross-linking and degassing processes consume a lot of energy and have low production efficiency. The retired insulation materials are difficult to recycle, and incineration or landfilling causes environmental pollution, which is not in line with the current concept of "energy conservation and environmental protection" and the "dual carbon" goal.

[0003] Application Contents

[0004] The present application provides a thermoplastic medium-voltage cable insulation material and a preparation method thereof, which can eliminate the need for cross-linking and degassing treatment during the cable extrusion process, simplify the production process steps, and promote the transformation of power cable insulation materials to green and environmentally friendly types.

[0005] This application adopts the following technical solutions:

[0006] The present application provides a thermoplastic medium-voltage cable insulation material, comprising the following components in parts by weight: 100 parts of copolymer modified polypropylene, 0.5 to 1 part of antioxidant, and 0.5 to 1 part of anti-copper agent.

[0007] Furthermore, the copolymer-modified polypropylene includes ethylene-propylene copolymer-modified polypropylene.

[0008] Furthermore, the polypropylene in the ethylene-propylene copolymer modified polypropylene is one of isotactic polypropylene and atactic polypropylene.

[0009] Furthermore, the content of ethylene and propylene in the ethylene and propylene copolymer modified polypropylene is 10% to 20%.

[0010] Furthermore, the melt index of the ethylene-propylene copolymer modified polypropylene is 2±0.5 g / 10 min.

[0011] Furthermore, the antioxidant includes a primary antioxidant, and the primary antioxidant includes 1,2-bis(3,5-di-tert-butyl-4-hydroxy-phenylpropionic acid)hydrazine.

[0012] Furthermore, the content of the main antioxidant in the antioxidant is greater than or equal to 50%.

[0013] Furthermore, the antioxidant also includes an auxiliary antioxidant, which includes one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol ester, tris(2,4-di-tert-butylphenyl)phosphite, and 4,4′-thiobis(6-tert-butyl-3-methylphenol).

[0014] Furthermore, the content of various auxiliary antioxidants in the antioxidant is 10% to 20%.

[0015] Further, the anti-copper agent includes N-salicylicyl phthalimide.

[0016] The present application also provides a method for preparing a thermoplastic medium-voltage cable insulation material, comprising the following steps: generating polypropylene in a first reactor, and feeding the polypropylene into a second reactor to copolymerize with ethylene and propylene to generate ethylene-propylene copolymer-modified polypropylene. Feeding the ethylene-propylene copolymer-modified polypropylene into an extruder for mixing and granulation, and feeding an antioxidant and an anti-copper agent into the extruder to obtain a thermoplastic medium-voltage cable insulation material.

[0017] Furthermore, the first reactor and the second reactor are both gas phase reactors.

[0018] Furthermore, before the ethylene-propylene copolymer-modified polypropylene is fed into the extruder, the ethylene-propylene copolymer-modified polypropylene is fed into a bag filter to be separated from the gas.

[0019] Furthermore, after the ethylene-propylene copolymer modified polypropylene is sent to a bag filter to be separated from the gas, the ethylene-propylene copolymer modified polypropylene is sent to a degassing bin to be dried and the activity of the residual catalyst therein is removed.

[0020] Furthermore, the heating temperature of the extruder is 175-185°C.

[0021] The present application also provides a thermoplastic medium-voltage cable, the preparation raw materials of which include the above-mentioned thermoplastic medium-voltage cable insulation material or the thermoplastic medium-voltage cable insulation material prepared by the preparation method of the above-mentioned thermoplastic medium-voltage cable insulation material.

[0022] Compared with the prior art, this application has the following beneficial effects:

[0023] The present application uses ethylene-propylene copolymer modified polypropylene, which is a thermoplastic environmentally friendly material, green and friendly, and does not require cross-linking and degassing treatment during the cable extrusion process, which greatly simplifies the process steps, reduces energy loss and carbon emissions, and shortens the cable supply cycle. The present application uses petrochemical equipment to directly produce thermoplastic medium-voltage cable insulation materials, which can directly enter the cable factory extrusion chain for the cable extrusion process, without the need for secondary modification and additive treatment to prevent pollution. The thermoplastic medium-voltage cable insulation material of the present application has excellent mechanical properties and electrical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0025] Figure 1 Schematic diagram of the process of preparing a thermoplastic medium-voltage cable insulation material in an embodiment of the present application.

[0026] Implementation Method

[0027] The technical methods in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0028] Based on the existing technology, it is extremely important to develop an environmentally friendly cable insulation material that meets mechanical and electrical properties. After modification, the thermoplastic polypropylene material has good electrical properties, mechanical properties and heat resistance stability, and consumes less energy during the production process and has a short delivery cycle. It can be used as an insulation material for medium-voltage power cables.

[0029] The present application provides a thermoplastic medium voltage cable insulation material, comprising the following components in parts by weight: 100 parts of ethylene-propylene copolymer modified polypropylene, 0.5-1 parts of antioxidant, and 0.5-1 parts of anti-copper agent. For ethylene-propylene copolymer modified polypropylene, a random copolymerization modification method is adopted to insert ethylene and propylene segments into the polypropylene segment.

[0030] The polypropylene in the ethylene-propylene copolymer modified polypropylene is one of isotactic polypropylene and atactic polypropylene, the content of ethylene-propylene in the ethylene-propylene copolymer modified polypropylene is 10% to 20%, and the melt index of the ethylene-propylene copolymer modified polypropylene is 2±0.5 g / 10 min. The melt index of the ethylene-propylene copolymer modified polypropylene is 2±0.5 g / 10 min, which is obtained by testing at 230° C. with a force of 2.16 kg.

[0031] The antioxidant comprises a primary antioxidant, the primary antioxidant comprises 1,2-bis(3,5-di-tert-butyl-4-hydroxy-phenylpropionic acid)hydrazine, and the content of the primary antioxidant in the antioxidant is greater than or equal to 50%.

[0032] The antioxidant also includes an auxiliary antioxidant, which includes one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol, tris(2,4-di-tert-butylphenyl) phosphite, and 4,4′-thiobis(6-tert-butyl-3-methylphenol), and the content of various auxiliary antioxidants in the antioxidant is 10% to 20%. The auxiliary antioxidant may not be added.

[0033] The anti-copper agent includes N-salicylic amide phthalimide. The anti-copper agent is used to prevent the polypropylene material from contacting with the cable copper core to produce copper degradation.

[0034] See also Figure 1 The present application also provides a method for preparing a thermoplastic medium-voltage cable insulation material, comprising the following steps:

[0035] Step 1: Produce polypropylene in the first reactor, and send the polypropylene into the second reactor to copolymerize with ethylene and propylene to generate ethylene-propylene copolymer modified polypropylene.

[0036] In step 1, in the first reactor, polypropylene is produced using the gas phase Innovene process.

[0037] The first reactor is fed with a catalyst, a modifier, ethylene and propylene. The catalyst includes a main catalyst and a co-catalyst. The main catalyst may be a Ziegler-Natta catalyst, including TiCl4 and di-n-butyl titanate supported on MgCl2, and may be selected from one of the CD / CDI catalyst of Amoco, the NG / NA catalyst of Beijing Chemical Research Institute, and the SAL catalyst of Beijing Aoda Catalyst Company. The co-catalyst may be triethylaluminum. The modifier may be diisobutyldimethoxysilane. In addition, hydrogen is also fed into the first reactor as a molecular weight regulator.

[0038] In the first reactor, the propylene feed rate is 25 kg / h, and the flow ratio of ethylene to propylene is 1:10. The flow ratio of the main catalyst to propylene is 1:5000. The amounts of the main catalyst, co-catalyst and modifier meet the following conditions: Al / Mg (mol / mol) = 12:1, Al / Si (mol / mol) = 6:1. The flow ratio of hydrogen to propylene is 1:50000. The polymerization temperature is 70°C, the polymerization pressure is 3.20 MPa, and the residence time of the material in the first reactor is 1.2 h. The flow unit is kg / h.

[0039] In step 1, in the second reactor, the polymer powder in the first reactor is copolymerized with ethylene and propylene to generate ethylene-propylene copolymer modified polypropylene.

[0040] The polymer powder, ethylene and propylene in the first reactor are introduced into the second reactor. In addition, hydrogen is also introduced into the second reactor as a molecular weight regulator.

[0041] In the second reactor, the mass ratio of propylene:ethylene was 1:4, the mass concentration of hydrogen was 0.25%, the copolymerization temperature was 65° C., the copolymerization pressure was 2.4 MPa, and the copolymerization time was 1.3 hours.

[0042] In step 1, both the first reactor and the second reactor are gas phase reactors, specifically, both are horizontal stirred bed gas phase reactors.

[0043] See also Figure 1 In step 1, the catalyst and the modifier are both located in the catalyst feeding system and are fed from the catalyst feeding system to the first reactor of the first polymerization reaction unit. Ethylene and propylene are both located in the raw material refining unit and are fed from the raw material refining unit to the first reactor of the first polymerization reaction unit and the second reactor of the second polymerization reaction unit.

[0044] Step 2: feeding the ethylene-propylene copolymer modified polypropylene into an extruder for mixing and granulation, and feeding an antioxidant and an anti-copper agent into the extruder to obtain a thermoplastic medium-voltage cable insulation material.

[0045] In step 2, before the ethylene-propylene copolymer modified polypropylene is fed into the extruder, the ethylene-propylene copolymer modified polypropylene is fed into a bag filter to be separated from the gas.

[0046] In step 2, the ethylene-propylene copolymer modified polypropylene is sent to a bag filter to be separated from the gas, and then sent to a degassing bin to be dried and the activity of the residual catalyst is removed.

[0047] In step 2, the extruder is a twin-screw extruder, and the heating temperature of the extruder is 175-185°C.

[0048] In step 2, after granulation, the formed pellets are sent to be evenly mixed with pellets produced in the same batch to ensure the uniformity of the pellets before being sent to storage tanks for packaging.

[0049] See also Figure 1 In step 2, the copolymer powder in the second reactor is sent to the bag filter and degassing bin of the powder deactivation and drying unit. The deactivated and dried copolymer powder in the degassing bin is sent to the extruder of the granulation unit. The pellets extruded by the extruder are blended and homogenized and then sent to the storage tank of the pellet storage unit. The pellets in the storage tank are sent for packaging.

[0050] In summary, the thermoplastic medium-voltage cable insulation material of the present application is directly produced by catalytic synthesis-copolymerization modification-extrusion granulation using a petrochemical device. At the same time, antioxidants and anti-copper agents are also added to the petrochemical device in the above process, which avoids pollution caused by secondary processing and ensures the purity of the insulation material. At the same time, the petrochemical device can ensure the uniformity and stability of the output.

[0051] The present application also provides a thermoplastic medium-voltage cable, the preparation raw materials of which include the above-mentioned thermoplastic medium-voltage cable insulation material or the thermoplastic medium-voltage cable insulation material prepared by the preparation method of the above-mentioned thermoplastic medium-voltage cable insulation material.

[0052] The technical solution and beneficial effects of the present application are further explained below in conjunction with embodiments.

[0053] In the following embodiments, a catalyst, a modifier, ethylene and propylene are introduced into the first reactor. The catalyst includes a main catalyst and a co-catalyst. The main catalyst is a Ziegler-Natta catalyst selected from the CD / CDI catalyst of Amoco. The co-catalyst is triethylaluminum. The modifier is diisobutyldimethoxysilane. In addition, hydrogen is also introduced into the first reactor as a molecular weight regulator.

[0054] In the first reactor, the propylene feed rate is 25 kg / h, and the flow ratio of ethylene to propylene is 1:10. The flow ratio of the main catalyst to propylene is 1:5000. The amounts of the main catalyst, co-catalyst and modifier meet the following conditions: Al / Mg (mol / mol) = 12:1, Al / Si (mol / mol) = 6:1. The flow ratio of hydrogen to propylene is 1:50000. The polymerization temperature is 70°C, the polymerization pressure is 3.20 MPa, and the residence time of the material in the first reactor is 1.2 h. The flow unit is kg / h.

[0055] The polymer powder, ethylene and propylene in the first reactor are introduced into the second reactor. In addition, hydrogen is also introduced into the first reactor as a molecular weight regulator.

[0056] In the second reactor, the mass ratio of propylene:ethylene was 1:4, the mass concentration of hydrogen was 0.25%, the copolymerization temperature was 65° C., the copolymerization pressure was 2.4 MPa, and the copolymerization time was 1.3 hours.

[0057] Example 1

[0058] Polypropylene is generated in the first reactor, and the polypropylene is sent to the second reactor to copolymerize with ethylene and propylene to generate ethylene-propylene copolymer-modified polypropylene, wherein the content of ethylene-propylene in the ethylene-propylene copolymer-modified polypropylene is 17%, and the melt index of the ethylene-propylene copolymer-modified polypropylene is 2.2 g / 10 min.

[0059] The ethylene-propylene copolymer modified polypropylene is sent to a bag filter to be separated from the gas, and the ethylene-propylene copolymer modified polypropylene is sent to a degassing bin to be dried and the activity of the residual catalyst is removed therefrom. 100 parts of the ethylene-propylene copolymer modified polypropylene are sent to a twin-screw extruder for mixing and granulation, and 0.6 parts of 1,2-bis(3,5-di-tert-butyl-4-hydroxy-phenylpropionic acid)hydrazine, 0.1 parts of tetra[β-(3,5-di-tert-butyl)-4-hydroxy-phenylpropionic acid)hydrazine, The invention relates to a novel thermoplastic medium voltage cable insulation material, wherein the thermoplastic medium voltage cable insulation material is prepared by feeding 0.1 parts of tris(2,4-di-tert-butylphenyl)propionate, 0.1 parts of tris(2,4-di-tert-butylphenyl)phosphite, 0.1 parts of 4,4′-thiobis(6-tert-butyl-3-methylphenol) and 0.5 parts of N-salicylicylamidophthalimide into a twin-screw extruder. The heating temperature of the twin-screw extruder is 175°C. The formed pellets are sent for blending, homogenization treatment and then sent to a storage tank for packaging to obtain a thermoplastic medium voltage cable insulation material.

[0060] Example 2

[0061] Polypropylene is generated in the first reactor, and the polypropylene is sent to the second reactor to copolymerize with ethylene and propylene to generate ethylene-propylene copolymer-modified polypropylene, wherein the content of ethylene-propylene in the ethylene-propylene copolymer-modified polypropylene is 10%, and the melt index of the ethylene-propylene copolymer-modified polypropylene is 1.5 g / 10 min.

[0062] The ethylene-propylene copolymer modified polypropylene is sent to a bag filter to be separated from the gas, and the ethylene-propylene copolymer modified polypropylene is sent to a degassing bin to be dried and the activity of the residual catalyst is removed therein. 100 parts of the ethylene-propylene copolymer modified polypropylene are sent to a twin-screw extruder for mixing and granulation, and 0.5 parts of 1,2-bis(3,5-di-tert-butyl-4-hydroxy-phenylpropionic acid)hydrazine, 0.2 parts of tetra[β-(3,5-di-tert-butyl)-4-hydroxy-phenylpropionic acid)hydrazine, The invention relates to a novel thermoplastic medium voltage cable insulation material, wherein the thermoplastic medium voltage cable insulation material is prepared by feeding 0.1 parts of 4,4′-thiobis(6-tert-butyl-3-methylphenol) and 0.7 parts of N-salicylicyl amide phthalimide into a twin-screw extruder. The heating temperature of the twin-screw extruder is 180°C. The formed pellets are sent for blending, homogenization treatment and then sent to a storage tank for packaging to obtain a thermoplastic medium voltage cable insulation material.

[0063] Example 3

[0064] Polypropylene is generated in the first reactor, and the polypropylene is sent to the second reactor to copolymerize with ethylene and propylene to generate ethylene-propylene copolymer-modified polypropylene, wherein the content of ethylene-propylene in the ethylene-propylene copolymer-modified polypropylene is 20%, and the melt index of the ethylene-propylene copolymer-modified polypropylene is 2.5 g / 10 min.

[0065] The ethylene-propylene copolymer modified polypropylene is sent to a bag filter to separate from the gas, and the ethylene-propylene copolymer modified polypropylene is sent to a degassing bin to dry and remove the activity of the residual catalyst therein, and 100 parts of ethylene-propylene copolymer modified polypropylene are sent to a twin-screw extruder for mixing and granulation, and 0.25 parts of 1,2-bis(3,5-di-tert-butyl-4-hydroxy-phenylpropionic acid)hydrazine, 0.05 parts of tetrakis[β-(3,5-di- tert-butyl-4-hydroxyphenyl) propionic acid pentaerythritol ester, 0.1 part of tris(2,4-di-tert-butylphenyl) phosphite, 0.1 part of 4,4′-thiobis(6-tert-butyl-3-methylphenol) and 1 part of N-salicylicylamide phthalimide are fed into a twin-screw extruder, the heating temperature of the twin-screw extruder is 185°C, the formed pellets are sent for blending, homogenization treatment and then sent to a storage tank for packaging to obtain a thermoplastic medium-voltage cable insulation material.

[0066] Example 4

[0067] Polypropylene is generated in the first reactor, and the polypropylene is sent to the second reactor to copolymerize with ethylene and propylene to generate ethylene-propylene copolymer-modified polypropylene, wherein the content of ethylene-propylene in the ethylene-propylene copolymer-modified polypropylene is 18%, and the melt index of the ethylene-propylene copolymer-modified polypropylene is 2.4 g / 10 min.

[0068] The ethylene-propylene copolymer modified polypropylene is sent to a bag filter to be separated from the gas, and the ethylene-propylene copolymer modified polypropylene is sent to a degassing bin to be dried and the activity of the residual catalyst is removed therefrom. 100 parts of the ethylene-propylene copolymer modified polypropylene are sent to a twin-screw extruder for mixing and granulation, and 0.25 parts of 1,2-bis(3,5-di-tert-butyl-4-hydroxy-phenylpropionic acid)hydrazine, 0.1 parts of tetra[β-(3,5-di-tert-butyl)-4-hydroxy-phenylpropionic acid)hydrazine, The invention relates to a novel thermoplastic medium voltage cable insulation material, wherein the thermoplastic medium voltage cable insulation material is prepared by feeding 0.1 parts of 4,4′-thiobis(6-tert-butyl-3-methylphenol) and 0.8 parts of N-salicylicyl amide phthalimide into a twin-screw extruder. The heating temperature of the twin-screw extruder is 180°C. The formed pellets are sent for blending, homogenization treatment and then sent to a storage tank for packaging to obtain a thermoplastic medium voltage cable insulation material.

[0069] Example 5

[0070] Polypropylene is generated in the first reactor, and the polypropylene is sent to the second reactor to copolymerize with ethylene and propylene to generate ethylene-propylene copolymer-modified polypropylene, wherein the content of ethylene-propylene in the ethylene-propylene copolymer-modified polypropylene is 17%, and the melt index of the ethylene-propylene copolymer-modified polypropylene is 2.1 g / 10 min.

[0071] The ethylene-propylene copolymer modified polypropylene is sent to a bag filter to be separated from the gas, and the ethylene-propylene copolymer modified polypropylene is sent to a degassing bin to be dried and the activity of the residual catalyst is removed. 100 parts of the ethylene-propylene copolymer modified polypropylene are sent to a twin-screw extruder for mixing and granulation at 100 g per part, and 0.5 parts of 1,2-bis(3,5-di-tert-butyl-4-hydroxy-phenylpropionic acid)hydrazine and 0.5 parts of N-salicylicylamide phthalimide are sent to the twin-screw extruder. The heating temperature of the twin-screw extruder is 180° C. The formed pellets are sent for blending, homogenization treatment, and then sent to a storage tank for packaging to obtain a thermoplastic medium-voltage cable insulation material.

[0072] Example 6

[0073] Polypropylene is generated in the first reactor, and the polypropylene is sent to the second reactor to copolymerize with ethylene and propylene to generate ethylene-propylene copolymer-modified polypropylene, wherein the content of ethylene-propylene in the ethylene-propylene copolymer-modified polypropylene is 20%, and the melt index of the ethylene-propylene copolymer-modified polypropylene is 2.5 g / 10 min.

[0074] The ethylene-propylene copolymer modified polypropylene is sent to a bag filter to be separated from the gas, and the ethylene-propylene copolymer modified polypropylene is sent to a degassing bin to be dried and the activity of the residual catalyst is removed therefrom. 100 parts of the ethylene-propylene copolymer modified polypropylene are sent to a twin-screw extruder at 100 g per part for mixing and granulation, and 0.8 parts of 1,2-bis(3,5-di-tert-butyl-4-hydroxy-phenylpropionic acid)hydrazine, 0.2 parts of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid]pentaerythritol ester and 1 part of N-salicylicylamide phthalimide are sent to the twin-screw extruder. The heating temperature of the twin-screw extruder is 185° C. The formed pellets are sent for blending, homogenization treatment and then sent to a storage tank for packaging to obtain a thermoplastic medium-voltage cable insulation material.

[0075] Example 7

[0076] Polypropylene is generated in the first reactor, and the polypropylene is sent to the second reactor to copolymerize with ethylene and propylene to generate ethylene-propylene copolymer-modified polypropylene, wherein the content of ethylene-propylene in the ethylene-propylene copolymer-modified polypropylene is 15%, and the melt index of the ethylene-propylene copolymer-modified polypropylene is 1.6 g / 10 min.

[0077] The ethylene-propylene copolymer modified polypropylene is sent to a bag filter to be separated from the gas, and the ethylene-propylene copolymer modified polypropylene is sent to a degassing bin to be dried and the activity of the residual catalyst is removed therefrom. 100 parts of the ethylene-propylene copolymer modified polypropylene are sent to a twin-screw extruder for mixing and granulation at 100 g per part, and 0.7 parts of 1,2-bis(3,5-di-tert-butyl-4-hydroxy-phenylpropionic acid)hydrazine, 0.1 parts of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid]pentaerythritol ester, 0.1 parts of 4,4′-thiobis(6-tert-butyl-3-methylphenol) and 0.8 parts of N-salicylicylamidophthalimide are sent to the twin-screw extruder. The heating temperature of the twin-screw extruder is 175° C. The formed pellets are sent for blending, homogenization treatment and then sent to a storage tank for packaging to obtain a thermoplastic medium-voltage cable insulation material.

[0078] The comprehensive properties of the cross-linked polyethylene used in the commercial medium-voltage cross-linked polyethylene insulated cable and the ethylene-propylene copolymer modified polypropylene used in the thermoplastic medium-voltage cable insulation material of Examples 1-6 were tested, and the results are shown in the following table:

[0079]

[0080] Semi-crystalline polymers are interpenetrating network structures composed of entangled amorphous and crystalline phase structures. Under large deformation, the molecular chains of the amorphous regions connecting the basic morphological units rotate parallel to the stretching direction. In the ethylene-propylene copolymer modified polypropylene of the present application, by introducing ethylene segments with strong segment mobility into the polypropylene, the position adjustment of the crystal morphological primitives during the stretching process can be promoted, thereby improving the tensile properties of the polypropylene. It can be seen from the data in the above table that the elongation at break of the ethylene-propylene copolymer modified polypropylene of Example 1 reached 680%, the elongation at break of the ethylene-propylene copolymer modified polypropylene of Example 2 reached 650%, the elongation at break of the ethylene-propylene copolymer modified polypropylene of Example 3 reached 712%, the elongation at break of the ethylene-propylene copolymer modified polypropylene of Example 4 reached 682%, the elongation at break of the ethylene-propylene copolymer modified polypropylene of Example 5 reached 682%, the elongation at break of the ethylene-propylene copolymer modified polypropylene of Example 6 reached 710%, and the elongation at break of the ethylene-propylene copolymer modified polypropylene of Example 7 reached 679%, which are all higher than the elongation at break of 564% of cross-linked polyethylene. That is to say, the ethylene-propylene copolymer modified polypropylene of the present application has a higher elongation at break, which is beneficial to reducing the construction difficulty of the medium voltage polypropylene cable during installation.

[0081] As can be seen from the data in the above table, the shape parameters of the ethylene-propylene copolymer modified polypropylene of the present application in the AC breakdown test are overall greater than those of cross-linked polyethylene, and the dispersion of the data is smaller, which is related to the uniform size distribution of the crystals in the ethylene-propylene copolymer modified polypropylene. At room temperature, the breakdown strength of the ethylene-propylene copolymer modified polypropylene of Example 1 reached 138.7kV / mm, the breakdown strength of the ethylene-propylene copolymer modified polypropylene of Example 2 reached 142.4kV / mm, the breakdown strength of the ethylene-propylene copolymer modified polypropylene of Example 3 reached 130.3kV / mm, the breakdown strength of the ethylene-propylene copolymer modified polypropylene of Example 4 reached 139.2kV / mm, the breakdown strength of the ethylene-propylene copolymer modified polypropylene of Example 5 reached 138.5kV / mm, the breakdown strength of the ethylene-propylene copolymer modified polypropylene of Example 6 reached 130.5kV / mm, and the breakdown strength of the ethylene-propylene copolymer modified polypropylene of Example 7 reached 134.8kV / mm, which are all substantially equivalent to cross-linked polyethylene. When the temperature rises to 90°C, the breakdown strength of the cross-linked polyethylene is 74.5 kV / mm, which is 49.4% lower than that at room temperature, while the breakdown strength of the ethylene-propylene copolymer modified polypropylene in Example 1 is 95.8 kV / mm, which is 42.9% lower than that at room temperature, and the breakdown strength of the ethylene-propylene copolymer modified polypropylene in Example 2 is 100.3 kV / mm, which is 42.1% lower than that at room temperature, and the breakdown strength of the ethylene-propylene copolymer modified polypropylene in Example 3 is 91.5 kV / mm, which is 29.8% lower than that at room temperature, and the breakdown strength of the ethylene-propylene copolymer modified polypropylene in Example 4 is 100.3 kV / mm, which is 42.1% lower than that at room temperature, and the breakdown strength of the ethylene-propylene copolymer modified polypropylene in Example 5 is 101.5 kV / mm, which is 29.8% lower than that at room temperature, and the breakdown strength of the ethylene-propylene copolymer modified polypropylene in Example 6 is 101.5 kV / mm, which is 29.8% lower than that at room temperature, and the breakdown strength of the ethylene-propylene copolymer modified polypropylene in Example 7 is 101.5 kV / mm, which is 10 The breakdown strength of copolymer modified polypropylene is 95.4kV / mm, which is 43.8% lower than that at room temperature. The breakdown strength of ethylene propylene copolymer modified polypropylene in Example 5 is 95.9kV / mm, which is 42.9% lower than that at room temperature. The breakdown strength of ethylene propylene copolymer modified polypropylene in Example 6 is 91.6kV / mm, which is 38.9% lower than that at room temperature. The breakdown strength of ethylene propylene copolymer modified polypropylene in Example 7 is 90.1kV / mm, which is 44.7% lower than that at room temperature, all of which are higher than the breakdown strength of cross-linked polyethylene at 90°C. This is because the distribution size of the crystals in ethylene propylene copolymer modified polypropylene is more uniform, the melting point is higher, and it has better stability to temperature. Under normal operating temperature, higher breakdown strength is conducive to ensuring the normal operation of the cable.

[0082] In summary, the elongation at break of the ethylene-propylene copolymer modified polypropylene of the present application has been greatly improved, and has exceeded the elongation at break of cross-linked polyethylene, and its elastic modulus has been greatly reduced, the material has better flexibility, which is conducive to the laying of cables, and the ethylene-propylene copolymer modified polypropylene has excellent mechanical properties. At the same time, the ethylene-propylene copolymer modified polypropylene has higher breakdown strength and changes less with temperature.

[0083] The above shows and describes the basic principles, main features and advantages of the present application. Those skilled in the art should understand that the present application is not limited by the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present application. Without departing from the spirit and scope of the present application, the present application may have various changes and improvements, and the scope of protection required by the present application is defined by the attached claims, description and their equivalents.

[0084] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.

Claims

1. A method for preparing a thermoplastic medium voltage cable insulation material, characterized in that: Thermoplastic medium voltage cable insulation material includes the following components in parts by weight: 100 parts of copolymer modified polypropylene, 0.5-1 parts of antioxidant, 0.5-1 parts of anti-copper agent; The copolymer modified polypropylene includes ethylene propylene copolymer modified polypropylene; The content of ethylene and propylene in the ethylene and propylene copolymer modified polypropylene is 10% to 20%; The anti-copper agent includes N-salicylicyl phthalimide; The polypropylene in the ethylene-propylene copolymer modified polypropylene is one of isotactic polypropylene and atactic polypropylene; The melt index of the ethylene-propylene copolymer modified polypropylene is 2±0.5 g / 10 min; The antioxidant includes a primary antioxidant, and the primary antioxidant includes 1,2-bis(3,5-di-tert-butyl-4-hydroxy-phenylpropionic acid)hydrazine; The content of the main antioxidant in the antioxidant is greater than or equal to 50%; The antioxidant further comprises an auxiliary antioxidant, and the auxiliary antioxidant comprises one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate]pentaerythritol ester, tris(2,4-di-tert-butylphenyl)phosphite, and 4,4'-thiobis(6-tert-butyl-3-methylphenol); The content of each auxiliary antioxidant in the antioxidant is 10% to 20%; The preparation method comprises the following steps: Producing polypropylene in the first reactor, and sending the polypropylene into the second reactor to copolymerize with ethylene and propylene to generate ethylene-propylene copolymer modified polypropylene; The ethylene-propylene copolymer modified polypropylene is fed into an extruder for mixing and granulation, and an antioxidant and an anti-copper agent are fed into the extruder to obtain a thermoplastic medium-voltage cable insulation material; The first reactor and the second reactor are both gas phase reactors; Before feeding the ethylene-propylene copolymer modified polypropylene into the extruder, feeding the ethylene-propylene copolymer modified polypropylene into a bag filter to separate it from the gas; After the ethylene-propylene copolymer modified polypropylene is sent to a bag filter to be separated from the gas, the ethylene-propylene copolymer modified polypropylene is sent to a degassing bin to be dried and the activity of the residual catalyst therein is removed; The heating temperature of the extruder is 175-185°C.

2. A thermoplastic medium voltage cable, characterized in that: The preparation raw materials include the thermoplastic medium-voltage cable insulation material prepared by the preparation method of the thermoplastic medium-voltage cable insulation material described in claim 1.

Citation Information

Patent Citations

  • Modified polypropylene insulation material and manufacturing method thereof

    CN103589105A

  • Environment-friendly insulating material for medium voltage power cables, and preparation method of environment-friendly insulating material

    CN108912492A

  • Thermoplastic insulating material for medium and high voltage and preparation method of thermoplastic insulating material

    CN110330727A

  • Polypropylene-based high-voltage direct-current cable material and preparation method thereof

    CN110498997A

  • High-voltage direct-current polypropylene cable material

    CN113248832A