A mold and method for preparing resin sand high temperature compressive strength test specimen

By designing the combination of mold base plate, molding outer mold and molding core, hollow specimens are formed, which solves the problem of the core not being heated and the cross-sectional area of ​​the sample being too small, and the sample being too small at high temperature Full heat permeability in compressive strength test and stability of test results.

CN114136748BActive Publication Date: 2024-12-06HUAZHONG UNIV OF SCI & TECH
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202111425812.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-26
Publication Date
2024-12-06
Estimated Expiration
2041-11-26

AI Technical Summary

Technical Problem

During the high-temperature compressive strength test of resin sand, the core of the sample is prone to not be heated through, and the test results are unstable due to the small cross-sectional area of ​​the sample.

Method used

Design a mold including a mold base plate, a molded outer mold and a molded core. Through the combination of the cavity of the molded outer mold and a molded core, a hollow sample is formed to ensure that the core is completely heated, and through the optimization of the molded core and the molded outer mold Size, increase the cross-sectional area of ​​the sample to improve the stability of the test results.

Benefits of technology

The sample is fully thermally permeable during high-temperature compressive strength testing, and by increasing the cross-sectional area, the stability of the test results is improved, while reducing the mold release resistance, which is convenient to operate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114136748B_ABST
    Figure CN114136748B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of casting molds, and specifically discloses a mold and method for preparing a resin sand high-temperature compressive strength test specimen. The mold includes a mold bottom plate, a molding outer mold and a molding core; the molding outer mold is connected to the top of the mold bottom plate and spliced ​​in pairs; each two adjacent molding outer molds are spliced ​​with a vertically penetrating cylindrical cavity; a molding core is arranged at each cavity, which includes a molding part and a connecting part; the molding part is in the shape of a round rod, placed in the cavity and coaxial with the cavity; the connecting part is cylindrical, coaxially connected to the molding part, and embedded in the mold bottom plate, and its top surface is flush with the top surface of the mold bottom plate; the present invention uses the cavity of the molding outer mold and the molding core arranged inside it to make a hollow specimen. On the one hand, the hollow structure solves the problem that the core of the specimen is not heated through when heated in the high-temperature compressive strength test; on the other hand, the hollow structure increases the cross-sectional area of ​​the specimen and improves the stability of the test results.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of casting molds, and more specifically, relates to a mold and a method for preparing a resin sand high-temperature compressive strength test sample. Background Art

[0002] In recent years, with the continuous development of casting technology, resin sand casting has been widely used in casting due to its outstanding advantages such as high production efficiency and high dimensional accuracy. As the research continues to deepen, more and more researchers of casting defects have begun to pay attention to the high temperature performance of resin sand, especially the high temperature compressive strength.

[0003] However, when testing the high temperature compressive strength of resin sand, the sample often fails to be fully heated, that is, the outer layer of the sample is fully heated, but the core is not fully heated. This kind of sample is thin, so it can avoid the above-mentioned problem of not being heated through, but because its cross-sectional area is too small (113.1mm 2 ), the test results of this type of sample are unstable and have relatively high fluctuations.

[0004] Based on the above defects and shortcomings, this field urgently needs to make further improvements to the design of existing resin sand high temperature compressive strength test specimens to solve the problem that the existing resin sand high temperature compressive strength test specimens are not heated through, and at the same time solve the problem of unstable test results due to the small cross-sectional area of ​​the specimens. Summary of the invention

[0005] In view of the above defects or improvement needs of the prior art, the present invention provides a mold and method for preparing resin sand high-temperature compressive strength test specimens, so as to solve the problem that the core of the specimen is not heated through during the high-temperature compressive strength test, and at the same time solve the problem of unstable test results due to the small cross-sectional area of ​​the specimen, and provide a resin sand high-temperature compressive strength test specimen mold and a test specimen production method that can be fully heated through, has a large cross-sectional area, and has stable test results.

[0006] To achieve the above object, according to one aspect of the present invention, the present invention provides a mold for preparing a resin sand high temperature compressive strength test specimen, characterized in that it includes a mold bottom plate, a molding outer mold and a molding core;

[0007] The mold bottom plate is used to fix the molding outer mold and the molding core;

[0008] The outer molding molds are provided with multiple pieces, which can be detachably connected to the top of the mold bottom plate and spliced ​​in pairs; each outer molding mold is provided with a row of semi-cylindrical grooves at its splicing position, and the grooves of each two adjacent outer molding molds are spliced ​​in pairs to form a vertically penetrating cylindrical cavity;

[0009] A forming core is arranged at each cavity where the forming outer molds are spliced, and is detachably connected to the mold bottom plate; the forming core includes a forming part and a connecting part; the forming part is in the shape of a round rod, whose diameter is smaller than the diameter of the cavity, and whose height is equal to the height of the cavity, and is used to be coaxially placed in the cavity; the connecting part is cylindrical and is coaxially connected to the forming part; the connecting part is embedded in the mold bottom plate and is detachably connected to the mold bottom plate to realize the detachable connection between the forming core and the mold bottom plate, and the top surface of the connecting part is flush with the top surface of the mold bottom plate.

[0010] Through the above conception, a hollow specimen is made by utilizing the cavity of the outer molding mold and the molding core arranged inside the cavity. On the one hand, the hollow structure can avoid the problem of the core not being heated through during the high-temperature compressive strength test of the specimen; on the other hand, the hollow structure increases the cross-sectional area of ​​the specimen, thereby improving the stability of the high-temperature compressive strength test results of the resin sand.

[0011] As a further preference, the molding part of the molding core is large at one end and small at the other end, and the large end is connected to the connecting part; the molding part is set to be large at one end and small at the other end to reduce its demolding resistance, so that the resistance encountered by the sample when it is separated from the molding part is extremely low, which not only realizes the complex hollow structure, but also protects the sample during demolding.

[0012] As a further preference, the detachable connection between the connecting portion of the forming core and the mold bottom plate is a threaded connection, which facilitates the installation and removal of the forming core.

[0013] As a further preference, the forming core is further provided with a base below the connecting portion, and a slot or a cross slot is provided at the bottom of the base to further facilitate the installation and removal of the forming core.

[0014] As a further preferred embodiment, the molding outer mold is detachably connected to the mold base plate by means of plug screws, and each molding outer mold is connected to multiple plug screws; by using the plug screws, on the one hand, it is convenient to install and disassemble the molding outer mold; on the other hand, because the top of the plug screw has a certain thickness and protrudes from the top surface of the molding outer mold, when the mold is inverted, the top surface of the molding outer mold and the molding core will not directly contact the operating platform, which can protect the molding outer mold and the molding core.

[0015] As a further preference, each outer molding mold is connected to two plug screws.

[0016] As a further preference, the molding outer molds are also provided with slots and protrusions at their splicing points, and the protrusion of each molding outer mold is embedded in the slot of the molding outer mold to which it is connected to achieve splicing of the molding outer molds in pairs; by providing the slots and protrusions, the molding outer molds are facilitated to be spliced.

[0017] As a further preference, one clamping groove and one protruding portion are respectively provided at each joint of the outer molding die, and are respectively located at two ends of a row of semi-cylindrical grooves provided at the joint.

[0018] As a further preference, the height of the molding outer mold is 20 mm, and the diameter of the spliced ​​cavity is 20 mm; the size of the molding outer mold is optimized based on the stress and thermal properties of the resin sand high-temperature compressive strength test sample to further optimize the sample testing effect.

[0019] As a further preference, the height of the molding part of the molding core is 20 mm, the diameter of one end is 4 mm, and the diameter of the other end is 5 mm; the size of the molding core is optimized based on the stress and thermal properties of the resin sand high temperature compressive strength test specimen to further optimize the specimen testing effect.

[0020] According to another aspect of the present invention, the present invention provides a method for preparing a resin sand high temperature compressive strength test specimen, which comprises the following steps:

[0021] S1, placing the outer molding dies on the mold bottom plate in sequence and connecting them in pairs, so that the grooves of each two adjacent outer molding dies are spliced ​​into a vertically penetrating cylindrical cavity; and fixing the outer molding dies to the mold bottom plate;

[0022] S2, placing a forming core in each cylindrical cavity assembled in step S1, so that the connecting portion of the forming core is embedded in the mold bottom plate and connected to the mold bottom plate, and the forming portion of the forming core is located in the cavity, completing the assembly of the mold;

[0023] S3, placing the assembled mold on the operating platform for sample preparation;

[0024] S4, injecting the resin sand mixed according to the production ratio into the cavity where the molding core is placed, and pounding and smoothing the resin sand;

[0025] S5, waiting for the resin sand to solidify to form a resin sand high temperature compressive strength test specimen;

[0026] S6, after the resin sand is solidified, the molding core is taken out;

[0027] S7, remove the outer molding mold, take out the resin sand high temperature compressive strength test specimen and save it, and the preparation of the resin sand high temperature compressive strength test specimen is completed.

[0028] In general, the above technical solution conceived by the present invention has the following technical advantages compared with the prior art:

[0029] 1. A hollow specimen is made by using the cavity of the outer molding mold and the molding core arranged inside it. On the one hand, the hollow structure solves the problem that the core of the specimen is not heated through during the high-temperature compressive strength test; on the other hand, the hollow structure increases the cross-sectional area of ​​the specimen and improves the stability of the high-temperature compressive strength test results of the resin sand.

[0030] 2. As an improvement to the above solution, by setting the molding part of the molding core to be large at one end and small at the other end, the resistance encountered by the sample during demoulding is extremely low, thereby achieving a hollow structure and protecting the sample during demoulding.

[0031] 3. As another improvement of the above scheme, the molding core is connected to the mold bottom plate through a threaded connection, and a base with a groove is provided on the molding core to facilitate the installation and removal of the molding core; and the molding outer mold is facilitated by providing a slot and a protrusion on the molding outer mold.

[0032] 4. As another improvement of the above solution, by using plug screws to connect the molding outer mold and the mold base plate, on the one hand, it is convenient for installing and disassembling the molding outer mold, and on the other hand, it can play a role in protecting the molding outer mold and the molding core.

[0033] 5. As another improvement of the above solution, by optimizing the sizes of the molding core and the molding outer mold, the test effect of the sample can be further optimized. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 is a schematic diagram of the arrangement of an embodiment of the present invention;

[0035] Figure 2 is a top view of an embodiment of the present invention;

[0036] Figure 3 Schematic diagram of a molded core according to an embodiment of the present invention.

[0037] Throughout the drawings, the same reference numerals are used to denote the same elements or structures, wherein:

[0038] Mold bottom plate 1; molding outer mold 2; molding core 3; plug screw 4; molding part 31; connecting part 32; bottom support 33. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0040] When preparing resin sand high-temperature compressive strength test specimens, the core of the specimen is often not fully heated through. The use of thin cylindrical specimens can avoid the problem of incomplete heating, but it also brings about the problem of unstable test results. Based on this, the present invention provides a mold and method for preparing resin sand high-temperature compressive strength test specimens to solve the problem that the core of the resin sand high-temperature compressive strength test specimen is not fully heated through when performing a high-temperature compressive strength test, and at the same time solves the problem that the test results are unstable due to the small cross-sectional area of ​​the specimen.

[0041] like Figure 1 As shown, the mold for preparing a resin sand high temperature compressive strength test specimen provided in an embodiment of the present invention comprises a mold bottom plate 1, a molding outer mold 2 and a molding core 3;

[0042] The mold bottom plate 1 is used to fix the molding outer mold 2 and the molding core 3;

[0043] The outer molding mold 2 is provided with multiple pieces, which can be detachably connected to the top of the mold bottom plate 1 and spliced ​​in pairs; each outer molding mold 2 is provided with a row of semi-cylindrical grooves at its splicing position, and the grooves of each two adjacent outer molding molds 2 are spliced ​​in pairs to form a vertically penetrating cylindrical cavity;

[0044] A molding core 3 is provided at each cavity where the molding outer mold 2 is spliced, and is detachably connected to the mold bottom plate 1; the molding core 3 includes a molding portion 31 and a connecting portion 32; the molding portion 31 is in the shape of a round rod, and its diameter is smaller than the diameter of the cavity, so that it can be coaxially placed in the cavity; the connecting portion 32 is cylindrical and is coaxially connected to the molding portion 31; the connecting portion 32 is embedded in the mold bottom plate 1 and is detachably connected to the mold bottom plate 1 to realize the detachable connection between the molding core 3 and the mold bottom plate 1, and the top surface of the connecting portion 32 is flush with the top surface of the mold bottom plate 1.

[0045] Through the mutual cooperation of the above-mentioned components, a hollow specimen is made by utilizing the cavity of the outer molding die 2 and the molding core 3 arranged therein. On the one hand, the hollow structure solves the problem that the core of the specimen is not heated through during the high-temperature compressive strength test; on the other hand, the hollow structure increases the cross-sectional area of ​​the specimen to improve the stability of the experimental results; compared with the prior art, the method is more advanced and practical.

[0046] Each component will be described in more detail below.

[0047] In this embodiment, if Figure 1 and Figure 2 As shown in , four outer molding molds 2 are provided; in some embodiments, two or more outer molding molds 2 are provided as needed; in this embodiment, the height of the outer molding mold 2 is 20 mm, and the diameter of the cavity formed by splicing thereof is 20 mm. The size of the outer molding mold 2 is optimized based on the stress and heat performance of the resin sand high temperature compressive strength test specimen;

[0048] In this embodiment, if Figure 1 and Figure 2 As shown in , the molding outer mold 2 is also provided with a card slot and a protrusion at its splicing, and the protrusion of each molding outer mold 2 is embedded in the card slot of the molding outer mold 2 to which it is connected, so as to realize the splicing of the molding outer molds 2 in pairs; by providing the card slot and the protrusion, it is convenient to splice the molding outer mold 2; in this embodiment, a card slot and a protrusion are respectively provided at each splicing of the molding outer mold 2, and are respectively located at the two ends of a row of grooves provided at the splicing; in some embodiments, a plurality of card slots and protrusions are provided at each splicing of the molding outer mold 2;

[0049] In this embodiment, if Figure 1 and Figure 2 As shown in the figure, the molding outer mold 2 is detachably connected to the mold base plate 1 by means of plug screws 4, and each molding outer mold 2 is connected to two plug screws 4; in some embodiments, depending on the shape and size of the molding outer mold 2, the number of plug screws 4 connected to each molding outer mold 2 may exceed two; in this embodiment, positioning holes are provided on the molding outer mold 2 and the mold base plate 1 for installing the plug screws 4; by using the plug screws 4, on the one hand, it is convenient to install and disassemble the molding outer mold 2, and on the other hand, because the top of the plug screw 4 has a certain thickness and protrudes from the top surface of the molding outer mold 2, when the mold is inverted, the top surfaces of the molding outer mold 2 and the molding core 3 will not be in direct contact with the operating platform, which can protect the molding outer mold 2 and the molding core 3.

[0050] like Figure 3 As shown in , in this embodiment, the molding part 31 of the molding core 3 is large at one end and small at the other end, and the large end is connected to the connecting part 32; in this embodiment, the height of the molding part 31 of the molding core 3 is 20 mm, the diameter of one end is 4 mm, and the diameter of the other end is 5 mm; the size of the molding core 3 is optimized based on the stress and heat performance of the resin sand high temperature compressive strength test sample; the molding part 31 is set to be large at one end and small at the other end to reduce its low demoulding resistance, so that the resistance encountered when the sample is separated from the molding part 31 is extremely low, which not only realizes the complex structure of the hollow, but also prevents the sample from being damaged due to demoulding;

[0051] like Figure 3 As shown in , in this embodiment, the detachable connection between the connection portion 32 of the molding core 3 and the mold base plate 1 is a threaded connection, which is convenient for installing and removing the molding core 3; the mold base plate 1 is provided with a threaded hole at the connection with the molding core 3, which is used to screw the molding core 3; in some embodiments, the detachable connection between the connection portion 32 of the molding core 3 and the mold base plate 1 can also be an interference connection;

[0052] like Figure 3As shown in , in this embodiment, the molding core 3 is further provided with a base 33 below the connecting portion 32, and a slot is provided at the bottom of the base 33, and the molding core 3 can be rotated by a flat-blade screwdriver, further facilitating the installation and disassembly of the molding core 3; in some embodiments, a cross slot is provided at the bottom of the base 33.

[0053] The above examples are used to illustrate the accessories adapted to the application program and do not constitute a limitation on the protection scope of the present invention.

[0054] A method for preparing a resin sand high temperature compressive strength test specimen provided by an embodiment of the present invention is described in detail below. The method comprises the following steps:

[0055] S1, place the molding outer molds 2 on the mold bottom plate 1 in sequence and connect them in pairs, so that the grooves of each two adjacent molding outer molds 2 are spliced ​​into a vertically penetrating cylindrical cavity; and fix the molding outer mold 2 to the mold bottom plate 1; the specific operations in this embodiment are: first place the mold bottom plate 1 on the sample preparation operation platform, and place four molding outer molds 2 on the mold bottom plate 1 in sequence, so that the protrusion of each molding outer mold 2 is embedded in the groove of the molding outer mold 2 to which it is connected, so as to realize the splicing of the molding outer molds 2 in pairs; place the plug screws 4 in the positioning holes of the molding outer mold 2 and the mold bottom plate 1, and tighten the plug screws 4 to complete the connection between the molding outer mold 2 and the mold bottom plate 1;

[0056] S2, place a forming core 3 in each cylindrical cavity spliced ​​in step S1, so that the connecting part 32 of the forming core 3 is embedded in the mold bottom plate 1 and connected to the mold bottom plate 1, and the forming part 31 of the forming core 3 is located in the cavity, and the assembly of the mold is completed; the specific operation in this embodiment is: first turn over the mold bottom plate 1 and the forming outer mold 2 connected in step S1 and place them upside down on the operating platform, place the forming core 3 in the threaded hole of the mold bottom plate 1, tighten the forming core 3, and complete the connection between the forming core 3 and the mold bottom plate 1; in this step, since the top of the plug screw 4 has a certain thickness and protrudes from the top surface of the forming outer mold 2, when the mold is inverted, the forming outer mold 2 and the top of the tightened forming core 3 will not directly contact the operating platform, which can protect the forming outer mold 2 and the forming core 3;

[0057] S3, placing the assembled mold on the sample preparation operation platform; the specific operation of this embodiment is: turning over the mold that has completed step S2 again, placing it on the operation platform, checking each connection, and completing the assembly of the mold;

[0058] S4, injecting the resin sand mixed according to the production ratio into the cavity where the molding core 3 is placed, and pounding and smoothing the resin sand;

[0059] S5, waiting for the resin sand to solidify to form a resin sand high temperature compressive strength test specimen; waiting for the resin to solidify until the specimen can be demoulded according to factors such as the type of resin, local climate, temperature and humidity;

[0060] S6, after the resin sand is solidified, the molding core 3 is taken out; the specific operation in this embodiment is: the mold is turned over again as a whole and placed upside down on the operating platform, and the molding core 3 is screwed out from the mold bottom plate 1 with a flat screwdriver;

[0061] S7, remove the molding outer mold 2, take out the resin sand high temperature compressive strength test sample and save it, and the preparation of the resin sand high temperature compressive strength test sample is completed; the specific operations in this embodiment are: turn the mold over again as a whole, place the front side on the operating platform, unscrew the plug screws 4 to remove the molding outer mold 2, and separate the molding outer molds 2 from each other; remove the resin sand compressive hollow sample, place it in a sealed bag and save it for testing.

[0062] In summary, the mold and method for preparing resin sand high temperature compressive strength test specimens according to the present invention not only solve the problem that the resin sand high temperature compressive strength test specimens are not heated through during the high temperature compressive strength test, but also solve the problem that the test results are unstable due to the small cross-sectional area of ​​the specimen. The mold and method are easy to operate, and are therefore particularly suitable for applications in which resin sand high temperature compressive strength test specimens are prepared.

[0063] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a resin sand high temperature compressive strength test specimen using a mold for preparing a resin sand high temperature compressive strength test specimen, It is characterized in that The mold for preparing the resin sand high temperature compressive strength test specimen is as follows: The mold is used to prepare a hollow specimen, and comprises a mold base (1), a molding outer mold (2), and a molding core (3); the mold base (1) is used to fix the molding outer mold (2) and the molding core (3); the molding outer mold (2) is provided with a plurality of pieces, which are all detachably connected to the top of the mold base (1) and spliced ​​in pairs; each of the molding outer molds (2) is provided with a row of semi-cylindrical grooves at the splicing position, and the grooves of each two adjacent molding outer molds (2) are spliced ​​in pairs to form a vertically through cylindrical cavity; The molding core (3) is provided at each of the cavities spliced ​​together in the molding outer mold (2), and is detachably connected to the mold bottom plate (1); the molding core (3) comprises a molding portion (31) and a connecting portion (32); the molding portion (31) is in the shape of a round rod, the diameter of which is smaller than the diameter of the cavity, and the height of which is equal to the height of the cavity, and is used to be coaxially placed in the cavity; the connecting portion (32) is in the shape of a cylinder, and is coaxially connected to the molding portion (31); the connecting portion (32) is embedded in the mold bottom plate (1) and is detachably connected to the mold bottom plate (1), so as to realize the detachable connection between the molding core (3) and the mold bottom plate (1), and the top surface of the connecting portion (32) is flush with the top surface of the mold bottom plate (1). The molding part (31) of the molding core (3) has one end that is large and the other end that is small, and the large end is connected to the connecting part (32). The connecting part (32) of the molding core (3) is detachably connected to the mold bottom plate (1) by a threaded connection. The molding core (3) is further provided with a base (33) below the connecting part (32). The bottom of the base (33) is provided with a straight groove or a cross groove. The height of the molding outer mold (2) is 20 mm, and the diameter of the spliced ​​cavity is 20 mm. The molding part (31) of the molding core (3) is 20 mm in height, and the diameter of one end is 4 mm, and the diameter of the other end is 5 mm. The hollow specimen is made by using the cavity of the outer molding mold and the molding core arranged inside it. On the one hand, the hollow structure can avoid the problem that the core of the specimen is not heated through during the high-temperature compressive strength test; on the other hand, the hollow structure increases the cross-sectional area of ​​the specimen and improves the stability of the test results of the high-temperature compressive strength of the resin sand. The outer molding die (2) is detachably connected to the mold base plate (1) via plug screws (4), and each of the outer molding die (2) is connected to a plurality of plug screws (4). The outer molding dies (2) are also provided with a slot and a protrusion at their joints, and the protrusion of each outer molding dies (2) is embedded in the slot of the outer molding dies (2) to which it is connected, so as to realize the splicing of the outer molding dies (2) in pairs. The clamping groove and the protruding portion are each provided at each joint of the outer molding die (2), and are respectively located at the two ends of the row of semi-cylindrical grooves at the joint. The preparation method comprises the following steps: S1, placing the molding outer molds (2) on the mold bottom plate (1) in sequence and connecting them in pairs, so that the grooves of each two adjacent molding outer molds (2) are spliced ​​in pairs to form a vertically penetrating cylindrical cavity; and fixing the molding outer molds (2) to the mold bottom plate (1); S2, placing one of the molding cores (3) at each cylindrical cavity in step S1, so that the connecting portion (32) of the molding core (3) is embedded in the mold bottom plate (1) and connected to the mold bottom plate (1), and the molding portion (31) of the molding core (3) is located in the cavity, and the mold assembly is completed, specifically: The mold base plate (1) and the molding outer mold (2) connected in step S1 are turned upside down on the operating platform, the molding core (3) is placed in the threaded hole of the mold base plate (1), and the molding core (3) is screwed in to complete the connection between the molding core (3) and the mold base plate (1). In this step, the top of the plug screw (4) has a certain thickness and protrudes from the top surface of the outer molding die (2). When the die is inverted, the top of the outer molding die (2) and the screwed molding core (3) will not directly contact the operating platform, which can protect the outer molding die (2) and the molding core (3). S3, placing the assembled mold on the operating platform for sample preparation; S4, injecting the mixed resin sand into the cavity where the molding core (3) is placed, and pounding and smoothing the resin sand; S5, waiting for the resin sand to solidify to form a resin sand high temperature compressive strength test specimen; S6, after the resin sand is solidified, taking out the molding core (3); S7, dismantling the outer molding mold (2), taking out the resin sand high temperature compressive strength test specimen and preserving it, and the preparation of the resin sand high temperature compressive strength test specimen is completed.

Citation Information

Patent Citations

  • Mold of wire drawing mold

    CN107008762A

  • Slag-resistant sample processing mould

    CN108562474A

  • Assembled hollow torsion shear instrument sample preparation tool and use method thereof

    CN110082185A

  • Hollow cylinder sample compaction device and method

    CN112747982A

  • Die in use for molding component of concrete filled double thin wall

    CN1727152A