Millimeter-scale nitrogen-doped porous carbon sphere and its preparation and application

Through lignin and chitosan-assisted self-assembly and aqueous solvent treatment, the problem of balancing powdering and adsorption properties in the preparation of biomass-based porous carbon materials was solved, and efficient and economical millimeter-sized nitrogen-doped porous carbon spheres were obtained, which are suitable for Activated carbon balls are prepared using adsorbent materials and activation methods.

CN114146679BActive Publication Date: 2024-10-01CENTRAL SOUTH UNIVERSITY OF FORESTRY AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111530704.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-15
Publication Date
2024-10-01
Estimated Expiration
2041-12-15

AI Technical Summary

Technical Problem

Existing biomass-based porous carbon materials have long preparation cycles, high energy consumption, low heteroatom content and uneven distribution, and lack of performance control, making it difficult to meet the requirements of practical applications and environmental development. Moreover, carbon materials are difficult to separate after adsorption in solution. Affect recycling.

Method used

Lignin and chitosan are used to assist self-assembly to prepare gel beads, which are combined with aqueous solvent treatment and pyrolysis carbonization. Through joint control of parameters, the pulverization phenomenon is avoided, and millimeter-sized large particle size carbon materials are obtained with excellent adsorption properties.

Benefits of technology

It has achieved the preparation of millimeter-sized nitrogen-doped porous carbon spheres with high specific surface area, high heteroatom content and controllable pore distribution, which improves the yield and adsorption performance of carbon materials. It is suitable for the preparation of activated porous carbon spheres by adsorption materials and activation methods. precursor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114146679B_ABST
    Figure CN114146679B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of carbon adsorbent preparation, and specifically provides a method for preparing millimeter-level nitrogen-doped porous carbon spheres, obtains a mixed solution A dissolved with lignin, chitosan and acid, then drops it into an alkaline solution under stirring for self-assembly, solid-liquid separation after standing and curing, and obtains lignin-chitosan gel microbeads; the gel microbeads are treated with an aqueous solvent, followed by solid-liquid separation, and a solid and a solution of pH 7 to 9 are obtained; the solid is subjected to vacuum freeze-drying treatment to obtain a precursor sphere; the aqueous solvent is water, or a mixed solvent of a water-organic solvent, and the organic solvent is a solvent miscible with water; the precursor sphere is pyrolyzed and carbonized at a temperature of 500 to 800 ° C under a protective atmosphere, and the carbonized product is subsequently washed and dried to obtain the nitrogen-doped porous carbon spheres. Millimeter-level carbon spheres with excellent adsorption performance can be prepared by the method described in the present invention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of porous carbon materials, and specifically relates to the preparation of a millimeter-scale nitrogen-doped porous carbon ball adsorption material. Background Art

[0002] In recent years, highly toxic phenolic compounds such as phenol, p-nitrophenol, o-nitrophenol, o-aminophenol, etc. produced in the chemical, pharmaceutical, cosmetic, dye and other industries have harmful effects on organisms even at low concentrations, and need to be removed before being discharged into the water environment. At the same time, in order to meet the national "carbon neutrality" and "carbon peak" requirements, the efficient capture, storage and conversion of CO2 are also of great significance. Green and clean nuclear energy, as a new energy source that has attracted much attention, is also one of the main sources of electricity. However, the radioactive iodine nuclides emitted from nuclear power plants are easily diffused through the atmosphere and enter the water environment, which will pose a huge threat to humans and the environment. Therefore, environmental pollutants including the above three must be strictly treated before being discharged into the environment, and adsorption is one of the simplest and most effective methods. Many adsorbents, such as chitosan, kaolin, montmorillonite, polymer adsorbents and biochar, can be used for the adsorption of phenolic compounds in aqueous solutions, CO2 capture, iodine adsorption, etc. Among them, the use of green and low-cost biomass-based porous carbon materials for adsorption and removal is a good choice. For example, Ma Xiancheng et al. (paper Appl. Surf. Sci. 2018, 459, 657-664.) hydrothermally treated discarded cigarette butts and doped them with nitrogen, and then activated and carbonized them to obtain nitrogen-doped porous carbon. Chen et al. first carbonized and activated coconut shells and then added a nitrogen source for pyrolysis doping (paper ACS Sustainable Chem. Eng. 2016, 4, 1439-1445.), and some researchers first performed nitrogen-doped heat treatment and then activated them to prepare nitrogen-doped porous carbon (paper J. Electroanal. Chem. 2020, 878, 114542.). However, the above biomass-based porous carbons have problems such as long preparation cycle, high energy consumption, low heteroatom content and uneven distribution, and lack of performance regulation.

[0003] As a renewable aromatic macromolecule widely found in nature, lignin has received a lot of attention, especially the waste liquid containing a large amount of lignin sulfonate from the pulp and paper industry, and its high-value utilization is particularly important. For example: lignin / sodium alginate composite materials can be used to extract mannitol and iodine; lignin / cellulose composite materials can be used to make composite films in food packaging and biomedical fields; lignin-derived adsorption materials, etc. On the other hand, it is used as a precursor (carbon source) of carbon materials, such as activated carbon (patent CN 103585956 A), carbon (nano) fiber (patent CN 105350114 A, CN106400206A, CN 104695060 B), carbon nanotubes (patent CN 112028054A, CN 111634902A, CN111170402A, CN 104787747A), carbon particles (patent CN 101910060 B), carbon nanosheets (patent CN106564874 B), etc. Lignin-based carbon fiber materials are a hot topic in the research of high-value utilization of lignin. Chitosan is a nitrogen-rich biosorbent. Because it is environmentally friendly, biocompatible, and has rich amino and hydroxyl groups, it can treat a variety of pollutants, can react with a variety of heavy metal ions, and is easy to be modified, and is widely used in the field of water treatment. Therefore, the efficient assembly of lignin and chitosan to prepare functional biomass materials is regarded as a promising method for utilizing biomass resources, for example, chitosan / lignin blended biodegradable membrane (patent CN 101220176B), lignin-chitosan porous scaffold material (patent CN 111760074 A), sodium alginate-lignin composite beads (patent CN 110947368A), magnetic chitosan lignin sulfonate graphene oxide adsorbent (patent CN 105251466 A), lignin xanthate bentonite composite spheres (patent CN 106582550 A), chitosan / lignin composite organic materials (Int. J. Biol. Macromol. 2019, 132, 1304-1317; Chem. Eng. J. 2014, 254, 491-502.), chitosan / lignin composite sponges (Environ. Sci. Nano 2020, 7(3): 793-802.), but there are few reports on the preparation of lignin / chitosan composite microbeads and their derived porous carbon (spheres) and the adsorption of environmental pollutants, and the carbon materials derived from lignin / chitosan composites are generally carbon powders, which have certain limitations on their use scenarios.

[0004] In summary, the current technical methods still have the following disadvantages: 1) Biomass-based porous carbon (spheres) have the disadvantages of long preparation cycle, high energy consumption, low and uneven heteroatom content, and lack of performance regulation, which cannot meet the dual requirements of practical application and environmental development for material preparation technology; 2) The relevant carbon material preparation process is prone to pulverization, and the particle size of the obtained carbon material is small, which makes it more difficult to separate it after adsorption in the solution, thereby affecting the recycling of carbon materials. Summary of the invention

[0005] The first purpose of the present invention is to provide a method for preparing millimeter-scale nitrogen-doped porous carbon spheres, which has simple process, easy operation, low equipment requirements and economical cost.

[0006] The second purpose of the present invention is to provide a millimeter-scale nitrogen-doped porous carbon sphere material with large specific surface area, high heteroatom content and controllable pore distribution obtained by the preparation method.

[0007] The third object of the present invention is to provide the use of the millimeter-scale nitrogen-doped porous carbon sphere material as an adsorption material, especially a gas adsorption material, and / or as a precursor for preparing active porous carbon spheres by an activation method.

[0008] A method for preparing millimeter-scale nitrogen-doped porous carbon spheres comprises the following steps:

[0009] Step (1): obtaining a mixed solution A containing lignin, chitosan and acid, and dropping the mixed solution into an alkaline solution under stirring to perform self-assembly, followed by standing to solidify and solid-liquid separation to obtain lignin-chitosan gel microbeads;

[0010] In the mixed solution A, the mass ratio of lignin to chitosan is 1:1-3:1; the total concentration of lignin and chitosan is 0.1 g / ml-0.05 g / mL; the concentration of the acid is 0.5-3.0 M; the mass concentration fraction of the alkali in the alkali solution is 6%-10%; the drop height from the surface of the alkali solution is 1.0-4.0 cm; the stirring speed during the drop addition stage is 20-40 r / min;

[0011] Step (2): treating the gel microbeads with an aqueous solvent, then performing solid-liquid separation, and collecting the solid when the pH of the liquid during the solid-liquid separation is 7 to 9; performing vacuum freeze-drying on the solid to obtain the precursor sphere; the aqueous solvent is water, or a mixed solvent of water and an organic solvent, and the organic solvent is a solvent that is miscible with water;

[0012] Step (3): heating the precursor sphere to 500-800°C at a heating rate of 2-8°C / min under a protective atmosphere, maintaining the temperature for pyrolysis and carbonization, and then washing and drying the carbonized product to obtain the nitrogen-doped porous carbon sphere.

[0013] The existing preparation methods of chitosan-based porous carbon materials are prone to pulverization, and it is difficult to prepare materials with original large particles. In addition, the pursuit of original large particles will affect its adsorption performance to a certain extent. In view of the difficulties that pulverization is easy to occur in the preparation process of carbon materials, it is difficult to prepare large particles, and it is difficult to take both large particles and adsorption performance into account, the present invention has found through in-depth research that the innovative use of lignin and chitosan to self-assemble gel microbeads, combined with aqueous solvent treatment and pyrolysis carbonization treatment and joint control of parameters of each treatment process can unexpectedly achieve synergy, effectively solve the problem of pulverization in the preparation process, obtain millimeter-level carbon materials, improve the yield of porous carbon, and more importantly, make the prepared large-particle materials have excellent adsorption performance.

[0014] In the present invention, the combination of the lignin-chitosan coordinated self-assembly, aqueous solvent treatment, pyrolysis and carbonization steps and the joint control of the conditions of each step are the key to synergistically solving the problem of pulverization and achieving good adsorption performance.

[0015] In the present invention, it is innovatively discovered that by using lignin-chitosan combined self-assembly, and coordinating the combined control of parameters such as the lignin-chitosan ratio, acid concentration and alkaline solution concentration, stirring speed, and titration height, synergy can be achieved, which is beneficial to obtaining millimeter-scale gel microbeads with good morphology, and is beneficial to reducing the pulverization behavior during the pyrolysis carbonization process, thereby obtaining a carbon material with large particle size and excellent adsorption performance.

[0016] In the present invention, the lignin is lignin powder with certain water solubility and its water-soluble derivatives.

[0017] Preferably, the lignin is at least one of sodium lignin sulfonate, potassium lignin sulfonate and calcium lignin sulfonate.

[0018] In the present invention, the chitosan has a purity of 80-95% deacetylation and a viscosity of 50-800 mpa.s.

[0019] Preferably, the chitosan has a deacetylation degree of 85-90% and a viscosity of 100-500 mPa.s.

[0020] Preferably, the mass ratio of lignin to chitosan is 2:2;

[0021] Preferably, in the mixed solution A of lignin and chitosan, the total concentration of lignin and chitosan is 0.1 g / ml to 0.05 g / mL.

[0022] Preferably, the acid used in the mixed solution A is at least one of hydrochloric acid, acetic acid, and nitric acid, more preferably hydrochloric acid, with a concentration of 0.5 to 3.0 M;

[0023] Preferably, in the mixed solution A, the solvent is water.

[0024] Preferably, the mixed solution A contains 1.0-3.0 g of lignin, 3.0-1.0 g of chitosan, 0.5-3.0 mol / L of acid concentration, 10-15 mL of acid, and 30-60 mL of water (eg, distilled water).

[0025] In the present invention, the mixed solution A is dropped into an alkaline solution to self-assemble into gel microbeads.

[0026] Preferably, the dropping process is carried out under stirring, and the stirring is, for example, magnetic stirring, and the rotation speed is, for example, 25 to 35 r / min.

[0027] Preferably, the alkali in the alkaline solution is at least one of sodium hydroxide, potassium hydroxide, potassium carbonate and sodium carbonate. In the alkaline solution, the mass concentration of the alkali is 6% to 10%, and the ratio of the solution volume to the volume of the mixed solution A is 1 to 4. It is further preferred that the mass concentration is 7% to 9%, and the volume ratio is 2 to 3.

[0028] In the present invention, the drop height refers to the height of the initial drop from the surface of the alkaline solution (that is, the distance between the dripper and the surface of the alkaline solution). Preferably, the drop height is 1 to 3 cm.

[0029] Preferably, the droplet acceleration rate is 1 to 4 drops / s, and the droplet size is 0.8 to 3.5 mm.

[0030] Preferably, after the dropwise addition is completed, the mixture is allowed to stand and solidify; the standing and solidifying time is 6 to 12 hours, more preferably 8 to 10 hours.

[0031] The present invention has found that the obtained gel microspheres are treated with an aqueous solvent, and the treatment process is, for example: mixing the gel microspheres with the aqueous solvent (the mixing may be slurrying or pouring), followed by single-stage or multi-stage solid-liquid separation, controlling the pH of the liquid of the solid-liquid separation to a desired range, and collecting the treated solid. The study found that further combined control of the pH of the liquid of the solid-liquid separation can unexpectedly solve the pulverization problem in a coordinated manner, which is conducive to the preparation of materials with large particle size and excellent adsorption performance.

[0032] The aqueous solvent is, for example, pure water, or a mixed solvent of water and an organic solvent miscible with water. The organic solvent is, for example, a C1-C4 alcohol. The alcohol is a mono- or polyol.

[0033] The water content in the aqueous solvent is greater than or equal to 50 wt. %; preferably, the aqueous solvent is water.

[0034] Preferably, in step (2), the pH is 7 to 8. Studies have found that within this preferred range, the pulverization problem can be further solved, which is conducive to obtaining a material with large particle size and excellent adsorption performance.

[0035] In the present invention, the wet gel microbeads are freeze-dried to obtain dry gel microbead precursors. The freeze-drying can be achieved based on existing equipment and means.

[0036] In the present invention, the freeze-dried material is subjected to pyrolysis carbonization treatment. Preferably, the carbonization process is carried out under a protective atmosphere. The protective atmosphere is at least one of nitrogen and an inert gas.

[0037] Preferably, the protective gas flow rate in step (3) is preferably 50 to 100 mL / min.

[0038] The study found that the lignin-chitosan combined self-assembly and impregnation with an aqueous solution, combined with the temperature and heating rate of pyrolysis carbonization, can further help solve the pulverization problem and produce a carbon material with large particle size and good adsorption performance.

[0039] Preferably, in step (3), the pyrolysis temperature is 500-600°C, and the heating rate is preferably 2-6°C / min.

[0040] Preferably, the pyrolysis carbonization time is 1 to 4 hours, more preferably 1 to 2 hours.

[0041] In the present invention, the carbonized product is preferably placed in an acid solution for acid treatment, followed by solid-liquid separation, washing, and drying to obtain an acid-treated material. In the present invention, the acid treatment is used to remove residual alkali metal or alkaline earth metal salts and oxides thereof in the pyrolysis product.

[0042] Preferably, the acid solution is an aqueous solution of hydrochloric acid, nitric acid, or sulfuric acid;

[0043] Preferably, the concentration of the acid solution is 0.5 to 3 mol / L;

[0044] Preferably, during the acid treatment, the solid-liquid ratio of the carbonized product to the acid solution is 1 g / 5 to 20 mL;

[0045] Preferably, the acid treatment process can be performed with the assistance of ultrasound.

[0046] Preferably, the temperature of the acid treatment is 25-35°C.

[0047] Preferably, the acid treatment process lasts for 10 to 30 minutes.

[0048] In the present invention, water and ethanol can be used alternately for washing in the acid treatment stage until the filtrate is neutral.

[0049] The preferred preparation process of the present invention comprises the following steps:

[0050] Step (1): dissolving lignin and chitosan in an acidic solution of a certain concentration to obtain a mixed solution A, then dropping the mixed solution into an alkaline solution of a certain concentration under magnetic stirring conditions for self-assembly, and after the dropping is completed, standing and curing for a period of time, filtering and separating, and obtaining lignin-chitosan gel microbeads;

[0051] Step (2): mixing the gel microbeads with a certain amount of water and filtering the mixture until the pH of the filtrate is 7 to 9, collecting the solid and subjecting it to vacuum freeze-drying to obtain the precursor spheres;

[0052] Step (3): pyrolyze and carbonize the precursor spheres under a protective atmosphere, and then sequentially treat the carbonized products with acid, wash with water until the filtrate is neutral, filter, and dry to obtain the nitrogen-doped porous carbon spheres.

[0053] A further preferred preparation method of the present invention comprises the following steps:

[0054] (a) Preparation of lignin-chitosan wet gel microbeads: After a certain mass ratio of lignin and chitosan is fully dissolved in a hydrochloric acid solution of a certain volume and concentration, it is dripped into a certain concentration of NaOH solution under stirring at a rate of 2 to 3 drops / s at 25°C to 35°C to allow it to self-assemble into gel microbeads. The solution is allowed to stand for a period of time and filtered to obtain wet gel microbeads.

[0055] (b) Preparation of dry gel microbead precursor: wet gel beads and a certain amount of water are mixed and filtered until the pH of the filtrate is 7-9, the solid is collected and subjected to vacuum freeze-drying to obtain precursor dry gel spheres, which are then dried and stored for later use.

[0056] (c) Preparation of nitrogen-doped porous carbon spheres: The precursor is pyrolyzed and carbonized in a horizontal tubular reactor under an inert atmosphere, cooled, ultrasonically treated in an acidic solution, filtered, washed, and dried to obtain nitrogen-doped porous carbon spheres.

[0057] The present invention also provides nitrogen-doped porous carbon spheres prepared by the preparation method, which are millimeter-scale spheres with a multi-level pore structure of mesopores and macropores, and are doped with at least one heteroatom selected from N, O, and S. Preferably, the content of mesopores (2 to 50 nm) is 60-80%; the content of macropores (>50 nm) is 20-40%; the specific surface area is 14.0 to 120.0 m 2 / g, pore volume is 0.023~0.060cm 3 / g, average pore diameter of 8.0-50.0nm, nitrogen content (3.0-5.0%), particle size (1.0-5.0mm).

[0058] The present invention also provides the application of nitrogen-doped porous carbon spheres prepared by the preparation method, which are used as adsorption materials and / or as precursors for preparing active porous carbon spheres by activation method.

[0059] Preferably, it is used as a gas adsorbent material;

[0060] Preferably, it is used as a gas adsorbent material for capturing CO2 in flue gases;

[0061] Preferably, it is used as an adsorbent material for pollutants in solution;

[0062] The pollutant is at least one of heavy metals and organic pollutants.

[0063] The organic pollutants are, for example, small molecular pollutants of C3 to C20, for example, phenolic pollutants, and further, for example, p-nitrophenol.

[0064] When it is used as a precursor of activated carbon balls, the millimeter-scale nitrogen-doped porous carbon balls can be mixed with an activator and then activated. The activator is, for example, an acid, a salt or the like. The activation treatment temperature can be, for example, above 500°C.

[0065] Compared with the prior art, the present invention has the following beneficial effects:

[0066] (1) The present invention uses lignin and chitosan to assist in self-assembly to prepare gel microbeads, combined with aqueous solvent impregnation and pyrolysis carbonization treatment and joint control of parameters of each treatment process, which can unexpectedly achieve synergy and effectively solve the problem of pulverization during the preparation process. It can obtain millimeter-sized carbon materials with excellent adsorption properties. In addition, it also helps to improve the yield and mechanical strength of the obtained millimeter-sized carbon spheres.

[0067] The present invention can use waste lignin in industrial pulping and papermaking and biorefining as one of the main raw materials. At the same time, green, environmentally friendly and renewable chitosan is used as the nitrogen source. It has the production advantages of wide raw material sources, simple operation, low equipment requirements, economical costs and high product value-added.

[0068] (2) The material prepared by the present invention has the chemical properties imparted by lignin and chitosan. In addition, it also has the characteristics of controllable porous structure, high specific surface area, rich nitrogen content, good physical and chemical stability, etc., and can be used as a precursor for preparing activated carbon balls.

[0069] (3) The material prepared by the present invention has excellent adsorption performance. For example, it can effectively remove CO2, iodine vapor, etc. in gaseous pollutants, as well as pollutants in water bodies, such as p-nitrophenol, etc., and can be recycled efficiently. It has broad market prospects in the fields of air purification and wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] Figure 1 is a preparation flow chart of the present invention;

[0071] Figure 2 The figures are the physical pictures of wet and dry gel microbeads and carbon spheres prepared in Example 1, wherein a is the physical picture of the lignin-chitosan wet gel microbeads prepared in Example 1; b is the physical picture of the dry gel microbeads; c is the physical picture of the nitrogen-doped porous carbon spheres;

[0072] Figure 3 The electron microscope images of the lignin-chitosan xerogel microspheres and carbon spheres prepared in Example 1, wherein a is the SEM image of the xerogel microspheres, and b is the SEM image of the carbon spheres;

[0073] Figure 4 This is an electron microscope image of the internal pore network of the nitrogen-doped porous carbon sphere prepared in Example 1;

[0074] Figure 5 The nitrogen adsorption-desorption isotherm and pore size distribution of the nitrogen-doped porous carbon spheres prepared in Example 1;

[0075] Figure 6 This is an XPS graph of the surface chemical composition of the nitrogen-doped porous carbon spheres prepared in Example 1;

[0076] Figure 7 Isothermal adsorption measurement of p-nitrophenol in water by the nitrogen-doped porous carbon spheres prepared in Example 1;

[0077] Figure 8 This is the selective adsorption experiment of CO2 and N2 by the nitrogen-doped porous carbon spheres prepared in Example 1;

[0078] Fig. 9 Actual picture of nitrogen-doped porous carbon powder prepared in comparative example 1

[0079] Fig.10 The actual picture of the broken and poorly spherical porous carbon particles prepared in Comparative Example 4

[0080] Fig.11 The actual picture of the non-spherical gel precursor prepared in comparative example 5

[0081] Fig.12 Actual picture of nitrogen-doped porous carbon powder prepared in comparative example 7 DETAILED DESCRIPTION

[0082] The following are specific embodiments of the present invention, and the technical solution of the present invention is further described in conjunction with the accompanying drawings, but the protection scope of the present invention is not limited thereto.

[0083] The lignin used in the following examples is lignin sulfonate purchased from Shanghai Macklin Biochemical Technology Co., Ltd., which is a brown powder. The chitosan used is purchased from Sinopharm Chemical Reagent Co., Ltd., which is a white powder with a deacetylation degree of 85% and a viscosity of 100 mPa.s. Chitosan from other sources such as shrimp shells, crab shells, carboxymethyl chitosan, etc. are also within the scope of the present invention. The other reagents and materials can be obtained from commercial sources or can be prepared by conventional methods.

[0084] Example 1

[0085] (1) Weigh 2.0 g of sodium lignin sulfonate and 2.0 g of chitosan in a beaker, add 30 mL of distilled water to disperse, then add 15 mL of 2 mol / L hydrochloric acid solution, stir in a water bath at room temperature for 1 h to fully dissolve it, and obtain suspension A. Then, under magnetic stirring conditions of 20 r / min, at a rate of 2 drops / s, the droplets are 2 cm above the liquid surface, and added dropwise into 100 mL of 8% potassium hydroxide solution for gel self-assembly. After the addition is completed, the mixture is allowed to stand for 10 h to solidify, and filtered to obtain wet gel microbeads.

[0086] (2) The wet gel beads are mixed with a certain amount of water and then filtered. This process can be repeated multiple times until the pH of the filtrate is 7. The solid is then freeze-dried in a vacuum for 20 hours to obtain precursor dry gel beads, which are then dried and stored for later use.

[0087] (3) Weigh 2.0 g of dry gel spheres and heat them directly from room temperature to 600 °C in a horizontal tubular reactor at a nitrogen gas flow rate of 75 mL / min and a heating rate of 5 °C / min for 2 h. After natural cooling, the solid product was placed in 30 mL of 2 mol / L hydrochloric acid solution and ultrasonicated for 10 min, filtered, and washed alternately with water and ethanol until the filtrate was neutral, and dried in a vacuum oven to obtain nitrogen-doped porous carbon spheres.

[0088] From the attached Figure 2 a It can be seen that there are many orange-yellow wet gel microspheres in the alkali solution after dropping, and the dry gel microspheres (attached) obtained after filtration, water immersion and freeze drying Figure 2 b) Light yellow, with uniform particle size. Figure 2 c It can be seen that the obtained carbon material is spherical particles with a relatively complete structure, a monodispersed state, no adhesion, and a particle size of 1.0 to 3.0 mm. Figure 3 a and 3b are scanning electron micrographs of the xerogel microbead precursor and nitrogen-doped porous carbon spheres, respectively. The particle structure is complete and the sphericity is good. Figure 4 This is an electron microscope image of the internal pore network of carbon sphere particles, which shows that its three-dimensional network structure is well-developed, continuously connected and penetrated, and has a rich pore structure. Figure 5The nitrogen adsorption-desorption test showed that the BET specific surface area of ​​nitrogen-doped porous carbon spheres was 13.4 m 2 / g, average particle size is 1.5mm, pore volume is 0.023cm 3 / g, the average pore size is 42.7nm. From the pore size distribution curve, it can be seen that it is a hierarchical pore structure of mesopores and macropores, in which the content of mesopores (2-50nm) is 57.4%; the content of macropores (>50nm) is 42.6%. Figure 6 It is obvious that its chemical composition contains elements such as carbon, nitrogen, oxygen, and sulfur, and the nitrogen content is higher than 4.0%.

[0089] Example 2

[0090] (1) Weigh 2.0 g of sodium lignin sulfonate and 2.0 g of chitosan in a beaker, add 30 mL of distilled water to disperse, then add 20 mL of 3 mol / L hydrochloric acid solution, stir in a water bath at room temperature for 1 h to fully dissolve it, and obtain suspension A. Then, under magnetic stirring conditions of 20 r / min, at a rate of 2 drops / s, the droplets are 1 cm above the liquid surface, and added dropwise into 100 mL of 9% potassium hydroxide solution for gel self-assembly. After the addition is completed, the mixture is allowed to stand for 10 h to solidify, and filtered to obtain wet gel microbeads.

[0091] (2) The wet gel beads are mixed with water and then filtered, which can be repeated multiple times until the pH of the filtrate is 8. The solid is then subjected to vacuum freeze-drying for 20 hours to obtain precursor dry gel beads, which are then dried and stored for later use.

[0092] (3) Weigh 2.0 g of dry gel spheres and heat them directly from room temperature to 700 °C in a horizontal tubular reactor at a nitrogen gas flow rate of 75 mL / min and a heating rate of 5 °C / min for 2 h. After natural cooling, the solid product was placed in 30 mL of 2 mol / L hydrochloric acid solution and ultrasonicated for 10 min, filtered, washed alternately with water and ethanol until the filtrate was neutral, and dried in a vacuum oven to obtain nitrogen-doped porous carbon (spheres).

[0093] Example 3

[0094] (1) Weigh 1.0 g of sodium lignin sulfonate and 3.0 g of chitosan in a beaker, add 50 mL of distilled water to disperse, then add 20 mL of 3 mol / L hydrochloric acid solution, stir in a water bath at room temperature for 1 h to fully dissolve it, and obtain suspension A. Then, under magnetic stirring conditions of 20 r / min, at a rate of 2 drops / s, the droplets are 3 cm above the liquid surface, and added dropwise into 100 mL of 9% potassium hydroxide solution for gel self-assembly. After the addition is completed, the mixture is allowed to stand for 10 h to solidify, and filtered to obtain wet gel microbeads.

[0095] (2) The wet gel beads and water are mixed and then filtered until the pH of the filtrate is 7. The solid is subjected to vacuum freeze drying for 20 hours to obtain precursor dry gel beads, which are then dried and stored for later use.

[0096] (3) Weigh 2.0 g of dry gel spheres and heat them directly from room temperature to 600°C in a horizontal tubular reactor at a nitrogen gas flow rate of 100 mL / min and a heating rate of 5°C / min for 2 h. After natural cooling, the solid product was placed in 30 mL of 2 mol / L hydrochloric acid solution and ultrasonicated for 10 min, filtered, and washed alternately with water and ethanol until the filtrate was neutral. After drying in a vacuum oven, millimeter-scale nitrogen-doped porous carbon (spheres) was obtained.

[0097] Example 4

[0098] (1) Weigh 2.0 g of sodium lignin sulfonate and 2.0 g of chitosan in a beaker, add 40 mL of distilled water to disperse, then add 20 mL of 1 mol / L hydrochloric acid solution, stir in a water bath at room temperature for 1 h to fully dissolve it, and obtain suspension A. Then, under magnetic stirring conditions of 20 r / min, at a rate of 2 drops / s, the droplets are 2 cm above the liquid surface, and added dropwise into 100 mL of a 7% potassium hydroxide solution to perform gel self-assembly. After the addition is completed, the mixture is allowed to stand for 10 h to solidify, and filtered to obtain wet gel microbeads.

[0099] (2) The wet gel beads are mixed with a certain amount of water and then filtered until the pH of the filtrate is 8. The solid is then subjected to vacuum freeze drying for 20 hours to obtain precursor dry gel beads, which are then dried and stored for later use.

[0100] (3) Weigh 2.0 g of dry gel spheres and heat them directly from room temperature to 600 °C in a horizontal tubular reactor at a nitrogen gas flow rate of 75 mL / min and a heating rate of 5 °C / min for 2 h. After natural cooling, the solid product was placed in 30 mL of 2 mol / L hydrochloric acid solution and ultrasonicated for 10 min, filtered, and washed alternately with water and ethanol until the filtrate was neutral. After drying in a vacuum oven, millimeter-sized nitrogen-doped porous carbon spheres were obtained.

[0101] Example 5

[0102] (1) Weigh 4.0 g of sodium lignin sulfonate and 4.0 g of chitosan in a beaker, add 40 mL of distilled water to disperse, then add 40 mL of 1 mol / L hydrochloric acid solution, stir in a water bath at room temperature for 1 h to fully dissolve it, and obtain suspension A. Then, under magnetic stirring conditions of 20 r / min, at a rate of 2 drops / s, the droplets are 2 cm above the liquid surface, and added dropwise into 100 mL of a 10% potassium hydroxide solution for gel self-assembly. After the addition is completed, the mixture is allowed to stand for 10 h to solidify, and filtered to obtain wet gel microbeads.

[0103] (2) The wet gel beads are mixed with a certain amount of water and then filtered until the pH of the filtrate is 9. The solid is then subjected to vacuum freeze drying for 20 hours to obtain precursor dry gel beads, which are then dried and stored for later use.

[0104] (3) Weigh 2.0 g of dry gel spheres and heat them directly from room temperature to 600 °C in a horizontal tubular reactor at a nitrogen gas flow rate of 75 mL / min and a heating rate of 5 °C / min for 2 h. After natural cooling, the solid product was placed in 30 mL of 2 mol / L hydrochloric acid solution and ultrasonicated for 10 min, filtered, and washed alternately with water and ethanol until the filtrate was neutral. After drying in a vacuum oven, millimeter-sized nitrogen-doped porous carbon spheres were obtained.

[0105] Embodiments 6 to 8

[0106] (1) Same as step (1) of Example 1.

[0107] (2) Same as step (2) in Example 1.

[0108] (3) The pyrolysis carbonization temperature was changed to 500°C, 750°C, and 800°C in sequence, and the rest of the steps were the same as those in Example 1.

[0109] Examples 6 to 8 all obtained millimeter-scale nitrogen-doped porous carbon spheres.

[0110] Examples 9 to 11

[0111] (1) Same as step (1) of Example 1.

[0112] (2) Same as step (2) in Example 1.

[0113] (3) The heating rates of pyrolysis carbonization were changed to 2°C / min, 4°C / min, and 8°C / min, respectively, and the rest of the steps were the same as those in Example 1.

[0114] Examples 9 to 11 all obtained millimeter-scale nitrogen-doped porous carbon spheres.

[0115] Example 12

[0116] (1) The acidic solution type was changed to acetic acid, and the rest was the same as step (1) of Example 1.

[0117] (2) Same as step (2) in Example 1.

[0118] (3) The same as step (3) of Example 1.

[0119] Example 12 obtained millimeter-scale nitrogen-doped porous carbon spheres.

[0120] Example 13

[0121] (1) The acidic solution type was changed to nitric acid, and the rest was the same as step (1) of Example 1.

[0122] (2) Same as step (2) in Example 1.

[0123] (3) The same as step (3) of Example 1.

[0124] Example 13 obtained millimeter-scale nitrogen-doped porous carbon spheres.

[0125] Comparative Example 1

[0126] The difference from Example 1 is that in step (2) of Comparative Example 1, the wet gel microbeads are not treated by water impregnation and filtration, but are directly separated and then freeze-dried in vacuum. The different step (2) is: the wet gel beads are subjected to vacuum freeze-drying for 20 hours to obtain precursor dry gel spheres, which are dried and stored for later use. The other steps and parameters are the same as those in Example 1.

[0127] The substance is porous carbon powder, see attached Fig. 9 , but failed to successfully produce uniform millimeter-sized large-particle carbon spheres.

[0128] Comparative Example 2

[0129] The difference from Example 1 is that in step (1) of Comparative Example 2, the vertical height of the dropwise addition is too large, and the dropwise addition is performed at a height of 10 cm from the liquid surface. The different step (1) is:

[0130] 2.0 g of sodium lignin sulfonate and 2.0 g of chitosan were weighed into a beaker, and 30 mL of distilled water was added to disperse them. Then, 15 mL of 2 mol / L hydrochloric acid solution was added, and the suspension was stirred in a water bath at room temperature for 1 h to fully dissolve it to obtain a suspension A. Subsequently, under the condition of magnetic stirring at 20 r / min, at a rate of 2 drops / s, the droplets were added dropwise to 100 mL of a potassium hydroxide solution with a mass concentration of 8% at a height of 10 cm from the liquid surface to perform gel self-assembly. After the addition was completed, the suspension was allowed to stand for 10 h to solidify, and filtered to obtain wet gel microbeads. Other parameters and steps were the same as those in Example 1.

[0131] It was found that the substance was porous carbon powder, and uniform millimeter-sized carbon sphere particles were not successfully produced.

[0132] Comparative Example 3

[0133] The only difference from Example 1 is that in step (1) of Comparative Example 3, chitosan is not added, and the other steps and parameters are the same as those of Example 1. As a result, it is found that no gel microbeads are formed.

[0134] Comparative Example 4

[0135] The only difference from Example 1 is that no lignin is added in step (1) of Comparative Example 4, and the other steps and parameters are the same as those of Example 1. The results show that the formed gel microbeads are white, and after pyrolysis and carbonization, they are broken carbon balls. It is impossible to obtain uniform millimeter-level porous carbon balls with good sphericity, and the mechanical strength is low. See the attached Fig.10 .

[0136] Comparative Example 5

[0137] The only difference from Example 1 is that the mass ratio of lignin to chitosan in step (1) of Comparative Example 5 is 5 (the total amount added is 4 g), and the other steps and parameters are the same as those of Example 1. As a result, it is found that no gel microbeads are formed. See attached Fig.11 .

[0138] Comparative Example 6

[0139] The only difference from Example 1 is that the stirring rate during the dropwise addition in step (1) of Comparative Example 6 is too fast, i.e., 60 r / min. The other steps and parameters are the same as those of Example 1. As a result, it is found that the formed gel is irregular or broken particles.

[0140] Comparative Example 7

[0141] The only difference from Example 1 is that the pH of the filtrate after the water immersion treatment in step (2) of Comparative Example 7 is 11, and the other steps and parameters are the same as those of Example 1. It is found that the product obtained after pyrolysis and carbonization is carbon powder, see attached Fig.12 .

[0142] Comparative Example 8

[0143] The only difference from Example 1 is that the heating rate in the pyrolysis carbonization of step (3) in Comparative Example 8 is 10° C. / min, and the products obtained after carbonization are carbon powder and broken carbon particles, and uniform millimeter-level particles cannot be obtained.

[0144] Comparative Example 9

[0145] The only difference from Example 1 is that the carbonization temperature in the pyrolysis carbonization in step (3) of Comparative Example 9 is 1000° C., and the products obtained after carbonization are carbon powder and crushed carbon particles.

[0146] Application Example 1

[0147] 100 mg of the product in each embodiment and comparative example was weighed and heated for degassing under high vacuum conditions at a degassing temperature of 120°C for 12 hours to remove moisture, CO2 and other impurities in the product, and then transferred to a 20 mL sample tube and subjected to a CO2 adsorption isotherm test on a Kubo-X1000 gas adsorption instrument of Beijing Biode Electronic Technology Co., Ltd. The test temperature was 0°C and 25°C, and the test pressure range was 0.02 to 1.00 bar.

[0148] Weigh 50 mg of the product in Example 1 and add them to 50 ml of aqueous solutions of p-nitrophenol with different initial concentrations (100-500 mg / L), respectively. Oscillate and adsorb for a period of time at 25°C until equilibrium is reached. Dilute the supernatant by a certain multiple, test the concentration of the iodine solution with a UV-visible spectrophotometer, and calculate the adsorption amount.

[0149] The adsorption data of each material are shown in Table 1

[0150]

[0151]

[0152] As shown in Table 1, the material prepared by the preparation method of the present invention has better adsorption performance.

Claims

1. A method for preparing millimeter-scale nitrogen-doped porous carbon spheres used as adsorption materials, characterized in that: The following steps are involved: Step (1): obtaining a mixed solution A containing lignin, chitosan and acid, and dropping the mixed solution into an alkaline solution under stirring to perform self-assembly, followed by standing to solidify and solid-liquid separation to obtain lignin-chitosan gel microbeads; In the mixed solution A, the mass ratio of lignin to chitosan is 1:1~3:1; the total concentration of lignin and chitosan is 0.1 g / ml~0.05 g / mL; the concentration of acid is 0.5~3.0 M; the mass concentration fraction of alkali in the alkali solution is 6%~10%; the drop height from the surface of the alkali solution is 1.0~4.0 cm; the stirring speed during the drop addition stage is 20~40 r / min; Step (2): treating the gel microbeads with an aqueous solvent, and then performing solid-liquid separation, collecting the solid when the liquid pH is 7 to 9 during the solid-liquid separation; performing vacuum freeze-drying on the solid to obtain the precursor sphere; the aqueous solvent is water, or a mixed solvent of water-organic solvent, and the organic solvent is a solvent miscible with water; Step (3): heating the precursor sphere to 500-800°C at a heating rate of 2-8°C / min under a protective atmosphere, maintaining the temperature for pyrolysis and carbonization, and then washing and drying the carbonized product to obtain the nitrogen-doped porous carbon sphere.

2. The preparation method according to claim 1, characterized in that The lignin is at least one of lignin sulfonate, alkali lignin, enzymatic lignin, sulfate lignin and dealkalized lignin.

3. The preparation method according to claim 2, characterized in that: The lignin sulfonate is one or more of sodium lignin sulfonate, calcium lignin sulfonate and potassium lignin sulfonate.

4. The preparation method according to claim 1, characterized in that: The chitosan has a deacetylation degree of 80-95% and a viscosity of 50-800 mpa.s.

5. The preparation method according to claim 1, characterized in that: The acid is at least one of hydrochloric acid, acetic acid and nitric acid.

6. The preparation method according to claim 1, characterized in that: The alkali in the alkaline solution is at least one of sodium hydroxide, potassium hydroxide, potassium carbonate and sodium carbonate.

7. The preparation method according to claim 1, characterized in that: The volume ratio of the alkaline solution to the mixed solution A is 1-4.

8. The preparation method according to claim 1, characterized in that: The droplet acceleration rate is 1~4 drops / s, and the droplet size is 0.8~3.5 mm.

9. The preparation method according to claim 1, characterized in that: The static curing time is 6 to 12 hours.

10. The preparation method according to claim 1, characterized in that: The vacuum freeze-drying treatment time is 12 to 24 hours.

11. The preparation method according to claim 1, characterized in that: The protective atmosphere is at least one of nitrogen and inert gas.

12. The preparation method according to claim 1, characterized in that: The flow rate of protective gas during the pyrolysis carbonization process is 50~100 mL / min.

13. The preparation method according to claim 1, characterized in that: The pyrolysis carbonization time is 1~4 h.

14. The preparation method according to claim 1, characterized in that: The carbonized product is washed with acid solution and water until the filtrate is neutral, and then separated from the solid and liquid and dried to obtain nitrogen-doped porous carbon spheres.

15. The preparation method according to claim 14, characterized in that: The acid solution is one of the aqueous solutions of hydrochloric acid, nitric acid and sulfuric acid.

16. The preparation method according to claim 15, characterized in that: The concentration of the acid solution is 0.5~3 mol / L.

17. The preparation method according to claim 14, characterized in that: During the acid treatment process, the solid-liquid ratio of the carbonized product to the acid solution is 1g / 5~20mL.

18. The preparation method according to claim 14, characterized in that: The acid treatment process takes 10 to 30 minutes.

19. A millimeter-sized lignin-chitosan based nitrogen-doped porous carbon sphere prepared by the preparation method according to any one of claims 1 to 18, characterized in that: It is a millimeter-scale sphere with a multi-level pore structure of mesopores and macropores, and is doped with at least one heteroatom selected from N, O, and S.

20. The millimeter-sized lignin-chitosan based nitrogen-doped porous carbon sphere according to claim 19, characterized in that: Mesopore content is 60~80%; macropore content is 20~40%; specific surface area is 14.0~120.0 m 2 / g, pore volume is 0.023~0.060 cm 3 / g, average pore size is 8.0~50.0 nm, nitrogen content is 3.0~5.0%, and particle size is 1.0-5.0 mm.

21. An application of lignin-chitosan based nitrogen doped porous carbon spheres prepared by the preparation method according to any one of claims 1 to 18, characterized in that: It is used as an adsorption material and / or as a precursor for preparing active porous carbon spheres by an activation method.

22. The use according to claim 21, characterized in that It is used as a gas adsorbent.

23. The use according to claim 22, characterized in that The gas is at least one of CO2, iodine vapor and volatile organic compounds.

24. The use according to claim 23, characterized in that The gas is CO2 in flue gas.

25. The use according to claim 21, characterized in that It is used as an adsorbent material for pollutants in solution.

26. The use according to claim 25, characterized in that The pollutant is at least one of heavy metals and organic pollutants.