Composite powder for magnetic powder core and method for preparing magnetic powder core
Through the composite powder of amorphous rare earth and nanocrystalline alloy powder, combined with specific annealing treatment, the performance limitations and high cost of magnetic powder cores are solved, and low-cost, high-performance magnetic powder core preparation is achieved, which is suitable for wide frequency bands and reduces the cost of magnetic powder cores. high frequency loss.
Patent Information
- Application Number
- CN202111407186.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-11-24
AI Technical Summary
Different types of magnetic powder cores have limited application range due to performance limitations, especially cost issues and high-frequency loss issues caused by the high price of nickel and molybdenum.
The composite powder of amorphous rare earth Fe65+2xAl3Si6P5+xB4Co2+yYb1.5yDyy alloy powder and nanocrystalline Fe73.5Cu1Nb3Si13.5B9 alloy powder is used to prepare a magnetic powder core with low cost and excellent performance through specific proportion mixing and annealing treatment.
A magnetic powder core with low cost, high saturation magnetic induction intensity, effective magnetic permeability, good frequency and temperature stability is realized, which is suitable for wide frequency band and reduces high frequency loss.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of soft magnetic materials, and in particular relates to composite powder for magnetic powder core and a method for preparing the magnetic powder core. Background Art
[0002] Magnetic powder core is a composite functional soft magnetic material made by mixing ferromagnetic powder and insulating medium. It retains the excellent properties of metal soft magnetic materials and ferrite soft magnetic materials and overcomes some defects of the two. Magnetic powder core is a new type of soft magnetic material with excellent comprehensive performance. It has the advantages of high magnetic induction intensity and effective magnetic permeability, good magnetic performance stability, low high-frequency loss, etc. It is widely used in various inductors, power transformers and many other fields.
[0003] The magnetic properties of magnetic powder cores are closely related to the type, content, and proportion of elements in the ferromagnetic powder used. The iron powder cores, iron silicon magnetic powder cores, sendust magnetic powder cores, high magnetic flux powder cores, and iron-nickel-molybdenum alloy powder cores prepared by existing processes use different magnetic metal / alloy powders, and the properties of the magnetic powder cores are also very different. Different types of magnetic powder cores have different applications in different technical fields due to their respective performance advantages, but their application scope is also limited due to their shortcomings in performance and other aspects. Summary of the invention
[0004] In view of the limitations of different magnetic powder cores due to their performance, the present invention comprehensively considers factors such as saturation magnetic induction intensity, loss, stability, cost, etc., and provides a composite powder for magnetic powder cores and a method for preparing the magnetic powder cores.
[0005] The first object of the present invention is to provide a composite powder for magnetic powder core; another object of the present invention is to provide a method for preparing a magnetic powder core using the composite powder. The present invention is specifically achieved through the following technical solutions:
[0006] A composite powder for magnetic powder core, comprising the following preparation raw materials:
[0007] Amorphous rare earth Fe 65+2x Al3Si6P 5+x B4Co 2+y Yb 1.5y Dy y Alloy powder, accounting for 60%-85% of the total mass of the raw materials; wherein 1.5≤x≤4, 1≤y≤3.5;
[0008] Also includes nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder accounts for 15%-40% of the total mass of raw materials.
[0009] Furthermore, the composite powder is composed of amorphous rare earth Fe68 Al3Si6P 6.5 BxF 4.5 Dy3 alloy powder and nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder.
[0010] Furthermore, the amorphous rare earth Fe 68 Al3Si6P 6.5 BxF 4.5 Dy3 alloy powder accounts for 68%-82% of the total mass of the raw materials, and the nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 The B9 alloy powder accounts for 18%-34% of the total mass of the raw materials.
[0011] Iron-nickel-molybdenum magnetic powder cores have extremely high saturation magnetic induction intensity and magnetic permeability, but the rapid increase in the price of nickel and molybdenum has led to high raw material costs for iron-nickel-molybdenum magnetic powder cores. Therefore, the composite powder raw material of the present invention uses amorphous Fe-Al-Si-PB-Co-Yb-Dy magnetic materials, which are mainly composed of aluminum, silicon, phosphorus, boron and iron, greatly reducing its own preparation cost; in addition, the present invention adds a certain proportion of cobalt, ytterbium and dysprosium to the Fe-Al-Si-PB material, which significantly reduces the loss of the material at high frequencies on the one hand, and ensures the magnetic stability of the material on the other hand. It can be used in a wide band from tens of hertz to several megahertz, and the temperature coefficient is also lower than 90ppm. The nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder has high saturation magnetic induction intensity and magnetic permeability, its magnetic anisotropy is very small, magnetostriction tends to zero, and its resistivity is also high. 65+2x Al3Si6P 5+x B4Co 2+y Yb 1.5y Dy y (1.5≤x≤4, 1≤y≤3.5) alloy powder as the main component, with a certain proportion of nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 The composite powder of the present invention is prepared by mixing B9 alloy powder, and the composite powder can be used to prepare a magnetic powder core with low cost and excellent comprehensive performance.
[0012] The method for preparing a magnetic powder core using the composite powder as a raw material comprises the following steps:
[0013] 1) Weigh amorphous rare earth Fe according to the formula ratio 65+2x Al3Si6P 5+x B4Co 2+y Yb 1.5y Dyy Alloy powder and nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder and sieving;
[0014] 2) mixing the two alloy powders to obtain a composite powder, mixing the composite powder with a binder, an insulating agent, and a release agent, stirring the mixture evenly, and vacuum drying the mixture;
[0015] 3) Pressing the dried powder obtained in step 2) into a shape, and then subjecting the powder to high temperature annealing treatment and low temperature annealing treatment in an inert atmosphere, and obtaining the magnetic powder core after cooling.
[0016] The magnetic powder core prepared by the present invention has excellent comprehensive performance: it has high saturation magnetic induction intensity and high effective magnetic permeability. In addition, the frequency stability and temperature stability of the magnetic powder core are better than those of soft magnetic materials such as iron powder core, iron silicon magnetic powder core, and sendust magnetic powder core prepared by existing processes.
[0017] Furthermore, in step 1), the two alloy powders must pass through a 100-mesh sieve to account for more than 99% of the total mass, and must pass through a 230-mesh sieve to account for 65%-72% of the total mass.
[0018] Furthermore, in step 2), the added amounts of the binder, insulating agent and release agent are 0.8%-3.0%, 1.5%-3.5% and 0.4%-1.2% of the mass of the composite powder respectively.
[0019] Furthermore, the adhesive is obtained by mixing alkyd resin and epoxy resin in equal amounts.
[0020] Furthermore, the insulating agent is aluminum oxide powder.
[0021] Furthermore, the release agent is calcium stearate.
[0022] Furthermore, in step 3), after the high temperature annealing treatment, the material is cooled in the furnace to 420-450° C., air-cooled to room temperature, and then heated to perform low temperature annealing.
[0023] Furthermore, in step 3), the temperature of the high temperature annealing is 550-650° C., and the annealing time is 20-35 min; the temperature of the low temperature annealing is 300-320° C., and the annealing time is 1-1.5 h.
[0024] The magnetic powder core of the present invention is subjected to two annealing heat treatments after being pressed and formed: first, the magnetic powder core is heated to 550-650°C for short-time high-temperature annealing for 20-35 minutes, and then heated to 300-320°C for low-temperature annealing after furnace cooling and air cooling, which can effectively eliminate residual stress in the magnetic powder core and improve the magnetic properties of the magnetic powder core.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. The present invention uses amorphous rare earth Fe 65+2x Al3Si6P 5+x B4Co 2+y Yb 1.5y Dy y (1.5≤x≤4, 1≤y≤3.5) alloy powder as the main component, with a certain proportion of nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 A composite powder is prepared by mixing B9 alloy powder, and a magnetic powder core with low cost and excellent comprehensive performance can be prepared by using the composite powder.
[0027] 2. The magnetic powder core prepared by the present invention has excellent comprehensive performance: it has high saturation magnetic induction intensity and high effective magnetic permeability. In addition, the frequency stability and temperature stability of the magnetic powder core are better than those of soft magnetic materials such as iron powder core, iron silicon magnetic powder core, and sendust magnetic powder core prepared by existing processes. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0029] Example 1
[0030] A composite powder for a magnetic powder core, comprising:
[0031] 1) Amorphous rare earth Fe 68 Al3Si6P 6.5 BxF 4.5 Dy3 alloy powder, accounting for 72% of the total raw material mass;
[0032] 2) Nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder accounts for 28% of the total mass of raw materials.
[0033] Example 2
[0034] A composite powder for a magnetic powder core, comprising:
[0035] 1) Amorphous rare earth Fe 68 Al3Si6P 6.5 BxF 4.5 Dy3 alloy powder, accounting for 82% of the total raw material mass;
[0036] 2) Nanocrystalline Fe 73.5 Cu1Nb3Si13.5 B9 alloy powder, accounting for 18% of the total mass of raw materials.
[0037] Example 3
[0038] A composite powder for a magnetic powder core, comprising:
[0039] 1) Amorphous rare earth Fe 72.7 Al3Si6P 8.8 B4CO3 1.5 Dy1 alloy powder, accounting for 72% of the total raw material mass;
[0040] 2) Nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder accounts for 28% of the total mass of raw materials.
[0041] Example 4
[0042] A magnetic powder core:
[0043] 1. According to Example 1 of the present invention, weigh amorphous rare earth Fe 68 Al3Si6P 6.5 BxF 4.5 Dy3 alloy powder and nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder and sieve (the two alloy powders must account for more than 99% of the total mass when passing through a 100-mesh sieve, and must account for 65%-72% of the total mass when passing through a 230-mesh sieve; the same below);
[0044] 2. The two alloy powders are mixed to obtain a composite powder, and the composite powder is mixed with a binder (mixed by an alkyd resin and an epoxy resin of equal mass), an insulating agent (alumina powder), and a release agent (calcium stearate) (the mixed addition amounts are 2.2%, 1.8%, and 0.8% of the mass of the composite powder, respectively), stirred evenly, and vacuum dried;
[0045] 3. The dried powder is pressed into a shape, and then heated to 590°C for high temperature annealing for 25 minutes in an inert atmosphere, cooled to 440°C in the furnace, taken out and air-cooled to room temperature, and then heated to 320°C for low temperature annealing for 1.2 hours. After cooling, the magnetic powder core is obtained.
[0046] The performance of the magnetic powder core sample prepared in this embodiment was tested: the saturation magnetic induction intensity was 1280mT, the effective magnetic permeability was 166H / m, the applicable frequency was 50Hz-10MHz, and the temperature was stable at 88ppm / °C.
[0047] Example 5
[0048] A magnetic powder core:
[0049] 1. According to Example 2 of the present invention, weigh amorphous rare earth Fe 68 Al3Si6P 6.5 BxF 4.5 Dy3 alloy powder and nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder and sieving;
[0050] 2. The two alloy powders are mixed to obtain a composite powder, and the composite powder is mixed with a binder (mixed by an alkyd resin and an epoxy resin of equal mass), an insulating agent (alumina powder), and a release agent (calcium stearate) (the mixed addition amounts are 2.2%, 1.8%, and 0.8% of the mass of the composite powder, respectively), stirred evenly, and vacuum dried;
[0051] 3. The dried powder is pressed into a shape, and then heated to 600°C for high temperature annealing for 20 minutes in an inert atmosphere, cooled to 440°C in the furnace, air-cooled to room temperature, and then heated to 320°C for low temperature annealing for 1.2 hours. After cooling, the magnetic powder core is obtained.
[0052] The performance of the magnetic powder core sample prepared in this embodiment was tested: the saturation magnetic induction intensity was 1210mT, the effective magnetic permeability was 154H / m, the applicable frequency was 50Hz-8MHz, and the temperature was stable at 90ppm / °C.
[0053] Example 6
[0054] A magnetic powder core:
[0055] 1. According to Example 3 of the present invention, weigh amorphous rare earth Fe 72.7 Al3Si6P 8.8 B4CO3 1.5 Dy1 alloy powder and nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder and sieving;
[0056] 2. The two alloy powders are mixed to obtain a composite powder, and the composite powder is mixed with a binder (mixed by an alkyd resin and an epoxy resin of equal mass), an insulating agent (alumina powder), and a release agent (calcium stearate) (the mixed addition amounts are 2.2%, 1.8%, and 0.8% of the mass of the composite powder, respectively), stirred evenly, and vacuum dried;
[0057] 3. The dried powder is pressed into a shape, and then heated to 590°C for high temperature annealing for 25 minutes in an inert atmosphere, cooled to 440°C in the furnace, taken out and air-cooled to room temperature, and then heated to 320°C for low temperature annealing for 1.2 hours. After cooling, the magnetic powder core is obtained.
[0058] The performance of the magnetic powder core sample prepared in this embodiment was tested: the saturation magnetic induction intensity was 1170mT, the effective magnetic permeability was 149H / m, the applicable frequency was 70Hz-8MHz, and the temperature stability was 91ppm / °C.
[0059] Comparative Example 1
[0060] 1. Composite powder: amorphous rare earth Fe 75 Al3Si6P 10 B4Co2 alloy powder, accounting for 72% of the total mass of raw materials; nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder, accounting for 28% of the total raw material mass;
[0061] 2. Weigh amorphous rare earth Fe according to the ratio 75 Al3Si6P 10 B4Co2 alloy powder and nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder and sieving;
[0062] 3. The two alloy powders are mixed to obtain a composite powder, and the composite powder is mixed with a binder (mixed by an alkyd resin and an epoxy resin of equal mass), an insulating agent (alumina powder), and a release agent (calcium stearate) (the mixed addition amounts are 2.2%, 1.8%, and 0.8% of the mass of the composite powder, respectively), stirred evenly, and vacuum dried;
[0063] 4. The dried powder is pressed into a shape, and then heated to 590°C for high-temperature annealing for 25 minutes in an inert atmosphere, cooled to 440°C in the furnace, air-cooled to room temperature, and then heated to 320°C for low-temperature annealing for 1.2 hours. After cooling, the magnetic powder core is obtained.
[0064] The performance of the magnetic powder core sample prepared in this comparative example was tested: the saturation magnetic induction intensity was 670mT, the effective magnetic permeability was 82H / m, the applicable frequency was 0.12kHz-2MHz, and the temperature stability was 134ppm / ℃.
[0065] Comparative Example 2
[0066] 1. According to Example 1 of the present invention, weigh amorphous rare earth Fe 68 Al3Si6P 6.5 BxF 4.5 Dy3 alloy powder and nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder and sieving;
[0067] 2. The two alloy powders are mixed to obtain a composite powder, and the composite powder is mixed with a binder (mixed by an alkyd resin and an epoxy resin of equal mass), an insulating agent (alumina powder), and a release agent (calcium stearate) (the mixed addition amounts are 2.2%, 1.8%, and 0.8% of the mass of the composite powder, respectively), stirred evenly, and vacuum dried;
[0068] 3. The dried powder is pressed into a shape, and then heated to 590° C. for high temperature annealing for 25 min in an inert atmosphere, and the magnetic powder core is obtained after cooling.
[0069] The performance of the magnetic powder core sample prepared in this comparative example was tested: the saturation magnetic induction intensity was 778mT, the effective magnetic permeability was 101H / m, the applicable frequency was 0.09kHz-4MHz, and the temperature stability was 115ppm / ℃.
[0070] It can be seen from the test data of the magnetic powder core samples of Examples 4-6 and Comparative Examples 1 and 2 that the magnetic powder cores prepared using the composite powder of the present invention have high saturation magnetic induction intensity and effective magnetic permeability, and good frequency stability and temperature stability; Comparative Example 1 changes the types and proportions of elements in the amorphous rare earth alloy powder, and the performance of the magnetic powder core samples obtained is greatly reduced except for their suitability for low frequency; Comparative Example 2 only performs high-temperature annealing treatment on the molding powder, and the internal stress after stirring and compression is not completely removed, so the performance of the magnetic powder core samples obtained is also slightly reduced.
[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application and not to limit it. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present application can still be modified or some technical features can be replaced by equivalents, which should all be included in the scope of the technical solution requested for protection in this application.
Claims
1. A method for preparing a magnetic powder core, characterized in that: The following steps are involved: 1) Weigh amorphous rare earth Fe 65+2x Al3Si6P 5+x B4Co 2+y Yb 1.5y Dy y Alloy powder and nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder and sieving; Among them, amorphous rare earth Fe 65+2x Al3Si6P 5+x B4Co 2+y Yb 1.5y Dy y Alloy powder, accounting for 60%-85% of the total mass of raw materials; among which, 1.5≤x≤4, 1≤y≤3.5; nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder, accounting for 15%-40% of the total mass of raw materials; 2) Mixing the two alloy powders to obtain composite powder, mixing the composite powder with a binder, an insulating agent, and a release agent, stirring the mixture evenly, and vacuum drying the mixture; 3) Pressing the powder obtained after drying in step 2) into a shape, and then subjecting the powder to high temperature annealing treatment and low temperature annealing treatment in an inert atmosphere, and cooling the powder core to obtain the magnetic powder core; Among them, after high-temperature annealing treatment, the steel is cooled to 420-450°C in the furnace and then taken out and air-cooled to room temperature, and then the temperature is increased for low-temperature annealing; the temperature of high-temperature annealing is 550-650°C, and the annealing time is 20-35 min; the temperature of low-temperature annealing is 300-320°C, and the annealing time is 1-1.5 h.
2. The method for preparing a magnetic powder core according to claim 1, characterized in that: Step 1) Powder combination is amorphous rare earth Fe 68 Al3Si6P 6.5 BxF 4.5 Dy3 alloy powder and nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder.
3. The method for preparing a magnetic powder core according to claim 2, characterized in that: The amorphous rare earth Fe 68 Al3Si6P 6.5 BxF 4.5 Dy3 alloy powder accounts for 68%-82% of the total mass of the raw materials, and the nanocrystalline Fe 73.5 Cu1Nb3Si 13.5 B9 alloy powder accounts for 18%-34% of the total mass of raw materials.
4. The method for preparing a magnetic powder core according to claim 1, characterized in that: Step 1) The two alloy powders must pass through a 100-mesh sieve to account for more than 99% of the total mass, and pass through a 230-mesh sieve to account for 65%-72% of the total mass.
5. The method for preparing a magnetic powder core according to claim 1, characterized in that: Step 2) The amounts of the binder, insulating agent and release agent added are 0.8%-3.0%, 1.5%-3.5% and 0.4%-1.2% of the mass of the composite powder respectively.
6. The method for preparing a magnetic powder core according to claim 5, characterized in that: The binder is obtained by mixing alkyd resin and epoxy resin in equal quantities.