Preparation method of modified conjugated diene polymer

By using a catalyst composition of neodymium compound and alkylating agent in the rubber composition to polymerize conjugated diene monomers and reacting with the modifier, the problem of low modification rate is solved and the tensile strength of the rubber composition is significantly improved. stretchability and viscoelastic properties.

CN114174354BActive Publication Date: 2024-10-01LG CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080053696.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-19
Filing Date
2020-09-18
Publication Date
2024-10-01
Estimated Expiration
2040-09-18

AI Technical Summary

Technical Problem

The modification rate of existing modified conjugated diene polymers in rubber compositions is low, resulting in poor tensile properties and viscoelastic properties, which are difficult to significantly improve.

Method used

A catalyst composition of a neodymium compound, a first alkylating agent, a second alkylating agent and a halide is used in a hydrocarbon solvent to polymerize conjugated diene monomers, followed by reaction or coupling with a modifier to control the neodymium compound The molar ratio to the second alkylating agent is 1:20 to 1:35, and the polymerization temperature is 30°C to 65°C to increase the modification rate.

Benefits of technology

A conjugated diene polymer with a high modification rate is achieved, which significantly improves the processing performance, tensile performance and viscoelastic properties of the rubber composition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0004941010530000021
    Figure FDA0004941010530000021
  • Figure GDA0003488107500000081
    Figure GDA0003488107500000081
  • Figure GDA0003488107500000101
    Figure GDA0003488107500000101
Patent Text Reader

Abstract

The present invention relates to a method for preparing a modified conjugated diene polymer having excellent physical properties such as tensile properties and viscoelastic properties and a high modification rate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0004] The present invention relates to a method for preparing a modified diene polymer with a high modification rate, wherein the modified diene polymer has excellent physical properties such as tensile properties and viscoelastic properties. Background Art

[0005] Recently, according to the increasing concern about energy saving and environmental issues, it is necessary to reduce the fuel consumption rate of automobiles. As a method for achieving this demand, a method for reducing the heat generation performance of tires by using inorganic fillers such as silica and carbon black in rubber compositions for forming tires has been proposed. However, the dispersion of inorganic fillers in rubber compositions is not good, and the overall physical properties of the rubber compositions, including the disadvantages of decreased wear resistance, crack resistance or processing performance, occur.

[0006] In order to solve these problems, a method of modifying the polymerization active part of a conjugated diene polymer obtained by anionic polymerization using organic lithium with a functional group capable of interacting with an inorganic filler has been developed as a method for improving the dispersibility of inorganic fillers such as silica and carbon black in a rubber composition. In particular, a method of modifying the polymerization active terminal of a conjugated diene polymer with a tin compound, a method of introducing an amino group, or a method of modifying with an alkoxysilane derivative has been proposed.

[0007] As another method, a method of improving processability and physical properties by modifying active terminals in a living polymer obtained by coordination polymerization using a catalyst containing a lanthanide rare earth element compound using a specific coupling agent or a modifier has been developed.

[0008] For example, a method of introducing a branched structure by preparing 1,4-cis-polybutadiene using a catalyst composed of a neodymium carboxylate compound, an alkylaluminum compound and a halogen-containing compound in a nonpolar solvent, adding sulfur chloride, and completing the reaction using a reaction quencher and an antioxidant is disclosed.

[0009] However, if the modified conjugated diene polymer is prepared by the above method and used in a rubber composition, the improvement effect on the physical properties of the rubber composition, such as wear resistance and processing performance, is not obvious. Therefore, there is still a need for a method for introducing a large amount of functional groups from a modifier and improving the mixing properties of a rubber composition, such as tensile properties and viscoelastic properties, by increasing the modification rate during the preparation of the modified conjugated diene polymer.

[0010] [Prior art literature]

[0011] [Patent Document]

[0012] Korean Patent Publication No.2017-0077614 Summary of the invention

[0013] Technical issues

[0014] An object of the present invention is to provide a method for preparing a modified conjugated diene polymer, which can prepare a modified conjugated diene polymer with excellent tensile properties and viscoelastic properties at a high modification rate.

[0015] Technical Solution

[0016] In order to solve the above problems, the present invention provides a method for preparing a modified conjugated diene polymer, comprising: polymerizing a conjugated diene monomer in a hydrocarbon solvent in the presence of a catalyst composition comprising a neodymium compound, a first alkylating agent, a second alkylating agent and a halide to prepare a living polymer; and reacting or coupling the living polymer with a modifier, wherein the molar ratio of the neodymium compound to the second alkylating agent is 1:20 to 1:35, and the polymerization is carried out at a temperature of 30° C. to 65° C.

[0017] Beneficial Effects

[0018] The conjugated diene-based polymer can be modified at a high modification rate by using the preparation method of the present invention, and the modified conjugated diene-based polymer thus prepared is used in a rubber composition to exhibit the effects of excellent processability, tensile properties, and viscoelastic properties. DETAILED DESCRIPTION

[0019] Hereinafter, the present invention will be described in more detail to help understanding of the present invention.

[0020] It should be understood that the words or terms used in the specification and claims of the present invention should not be understood as the meanings defined in common dictionaries. It should also be understood that the words or terms should be understood as having the same meanings as they have in the relevant technical background and the technical concept of the present invention, based on the inventors' ability to appropriately define the meanings of the words or terms in order to best illustrate the principles of the present invention.

[0021] Hereinafter, the present invention will be described in detail.

[0022] The preparation method of the modified conjugated diene polymer of the present invention is characterized by comprising: polymerizing a conjugated diene monomer in a hydrocarbon solvent in the presence of a catalyst composition comprising a neodymium compound, a first alkylating agent, a second alkylating agent and a halide to prepare a living polymer (step 1); and reacting or coupling the living polymer with a modifier (step 2), wherein the molar ratio of the neodymium compound to the second alkylating agent is 1:20 to 1:35, and the polymerization is carried out at a temperature of 30° C. to 65° C.

[0023] Step 1

[0024] Step 1 is a step of polymerizing a conjugated diene monomer in a hydrocarbon solvent in the presence of a catalyst composition comprising a neodymium compound, a first alkylating agent, a second alkylating agent and a halide to prepare a living polymer, wherein the living polymer may refer to a conjugated diene polymer containing an organic metal part.

[0025] The organic metal part can be an activated organic metal part at the end of a conjugated diene polymer (an activated organic metal part at the end of a molecular chain), an activated organic metal part in the main chain, or an activated organic metal part in a side chain (branch), wherein, when the activated organic metal part is obtained by anionic polymerization or coordinated anionic polymerization, the organic metal part can represent the activated organic metal part at the end.

[0026] The molar ratio of the neodymium compound and the second alkylating agent included in the catalyst composition is 1:20 to 1:35. Specifically, the second alkylating agent may be 20 mol or more and 35 mol or less, 30 mol or less based on 1 mol of the neodymium compound.

[0027] In the present invention, the neodymium compound and the second alkylating agent are contained and used in the above-mentioned molar ratio, the functional group from the modifier can be effectively bonded to the terminal of the conjugated diene polymer in the modification step, and the modification rate can be improved. In addition, if the modified conjugated diene polymer prepared in this way is used in a rubber composition, it can show excellent processing properties and excellent mixing properties such as tensile properties and viscoelastic properties.

[0028] If the second alkylating agent is less than 20 mol based on 1 mol of the neodymium compound, the molecular weight of the conjugated diene polymer will be too high, and in order to control the molecular weight, there will be a defect that an excessive amount of the catalyst composition is required. In addition, the preparation efficiency of the catalyst composition will be reduced, and the quality of the catalyst composition prepared thereby will deteriorate, and ultimately, it will lead to a reduction in the modification rate and deterioration in the quality of the rubber composition. In addition, if the second alkylating agent is greater than 35 mol based on 1 mol of the neodymium compound, the molecular weight of the conjugated diene polymer will be too low, and in order to control the molecular weight, it is necessary to reduce the amount of the catalyst composition, in which case, there will be the disadvantages that the polymerization reaction itself cannot be fully carried out and the polymerization conversion rate is significantly reduced. In addition, the activity performance of the active polymer will decrease, and the modification rate will decrease, so the quality of the rubber composition including the mixing performance will deteriorate.

[0029] Furthermore, if the molar ratio of the neodymium compound and the second alkylating agent deviates from the above range, the preparation efficiency of the catalyst composition may be reduced, the quality of the catalyst composition prepared thereby may be deteriorated, and the physical properties of the modified conjugated diene polymer and the rubber composition using the same may be deteriorated.

[0030] As described above, in the present invention, by using the second alkylating agent in an amount of 20 mol to 35 mol based on 1 mol of the neodymium compound, the activity performance of the active polymer is improved, the functional group from the modifier can be effectively bonded to the terminal of the polymer in the modification step to improve the modification rate, and a modified conjugated diene polymer showing excellent physical properties is prepared.

[0031] In the catalyst composition, a molar ratio of the neodymium compound, the first alkylating agent, the second alkylating agent, and the halide may be 1:(50 to 200):(20 to 35):(2 to 5).

[0032] More specifically, based on 1 mol of the neodymium compound, the first alkylating agent may be 50 mol or more, 60 mol or more, 80 mol or more, 90 mol or more, and 200 mol or less, 150 mol or less, 120 mol or less, 110 mol or less. In addition, based on 1 mol of the neodymium compound, the second alkylating agent may be 20 mol or more, and 35 mol or less. In addition, based on 1 mol of the neodymium compound, the halide may be 2.0 mol or more, 2.1 mol or more, 2.2 mol or more, 2.3 mol or more, and 5.0 mol or less, 3.0 mol or less, 2.5 mol or less.

[0033] If the molar ratio of the neodymium compound, the first alkylating agent, the second alkylating agent and the halide deviates from the above range, the preparation efficiency of the catalyst composition will be reduced, and the quality of the catalyst composition prepared thereby will be deteriorated. Finally, the physical properties of the modified conjugated diene polymer and the rubber composition using the same will be deteriorated.

[0034] Based on 100g of the conjugated diene monomer for polymerization, the neodymium compound can be 0.01mmol to 0.50mmol, specifically 0.01mmol or more, 0.02mmol or more, 0.04mmol or more, 0.05mmol or more, 0.07mmol or more, 0.08mmol or more, and 0.50mmol or less, 0.30mmol or less, less than 0.20mmol, 0.19mmol or less, 0.18mmol or less, 0.16mmol or less. For example, based on 100g of the conjugated diene monomer, the neodymium compound can be greater than 0.04mmol and less than 0.20mmol, 0.05mmol to 0.19mmol, 0.07mmol to 0.18mmol, 0.08mmol to 0.16mmol.

[0035] By using the neodymium compound in the above amount, there are effects in that an appropriate concentration can be achieved, excellent catalyst activity can be exhibited, economic feasibility can be ensured, and a separate desalting process is not required.

[0036] Furthermore, the catalyst composition of the present invention may satisfy the above amount range of the neodymium compound based on 100 g of the conjugated diene-based monomer, and may simultaneously satisfy the molar ratios of the neodymium compound, the first alkylating agent, the second alkylating agent, and the halide.

[0037] In addition, the preparation method of the present invention may further include the step of mixing the neodymium compound, the first alkylating agent, the second alkylating agent and the halide at -30°C to -20°C and leaving the mixture at -30°C to -20°C for 24 to 36 hours to prepare a catalyst composition before preparing the active polymer.

[0038] That is, the catalyst composition can be prepared by sequentially injecting a neodymium compound, a first alkylating agent, a second alkylating agent, a halide, and selectively injecting a conjugated diene monomer, and then mixing. Specifically, the catalyst composition can be prepared by sequentially injecting a neodymium compound, a first alkylating agent, a second alkylating agent, a halide, and selectively injecting a conjugated diene monomer in a hydrocarbon solvent, and then mixing. In this case, the hydrocarbon solvent can be a non-polar solvent that is not reactive with the components of the catalyst composition. In particular, the hydrocarbon solvent can use one or more selected from the following: aliphatic hydrocarbon solvents such as pentane, hexane, isopentane, heptane, octane and isooctane; alicyclic hydrocarbon solvents such as cyclopentane, methylcyclopentane, cyclohexane, methylcyclohexane and ethylcyclohexane; and aromatic hydrocarbon solvents such as benzene, toluene, ethylbenzene and xylene. As a specific example, the hydrocarbon solvent can be an aliphatic hydrocarbon solvent such as hexane.

[0039] In this case, in order to promote the generation of the catalyst active species, the mixing process may be performed at -30°C to -20°C, and after the mixing, the mixture thus obtained may be left to stand for 24 hours to 36 hours.

[0040] By preparing the above composition by the above method, the catalyst composition can be applied to the preparation method of the present invention to effectively prepare a modified conjugated diene polymer showing excellent physical properties.

[0041] In the present invention, there is no specific restriction on the conjugated diene monomer for preparing the active polymer, as long as it can be used to prepare the conventional conjugated diene polymer. The conjugated diene monomer can be specifically 1,3-butadiene, isoprene, 1,3-pentadiene, 1,3-hexadiene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 2-methyl-1,3-pentadiene, 3-methyl-1,3-pentadiene, 4-methyl-1,3-pentadiene or 2,4-hexadiene, and any one of them, or a mixture of two or more thereof can be used. More specifically, the conjugated diene monomer can be 1,3-butadiene.

[0042] In addition, considering the physical properties of the active polymer finally prepared in the polymerization reaction, other monomers copolymerizable with the conjugated diene monomers can be used, and the other monomers can be specifically aromatic vinyl monomers, such as styrene, p-methylstyrene, α-methylstyrene, 1-vinylnaphthalene, 3-vinyltoluene, ethylvinylbenzene, divinylbenzene, 4-cyclohexylstyrene and 2,4,6-trimethylstyrene, and any one of them or a mixture of two or more of them can be used. The amount of the other monomers used can be 20% by weight or less relative to the total weight of the monomers used in the polymerization reaction.

[0043] In this case, the entire amount of the conjugated diene monomer used to prepare the conjugated diene polymer is not dissolved in the non-polar solvent, but a part of the entire amount used is dissolved in the polymerization solvent and polymerized, and the conjugated diene monomer can be injected in batches one or more times, specifically two or more times, and more specifically two to four times, depending on the polymerization conversion rate.

[0044] The hydrocarbon solvent used in step 1 may be a non-polar solvent. Specifically, the hydrocarbon solvent may be one or more selected from the following: aliphatic hydrocarbon solvents such as pentane, hexane, isopentane, heptane, octane and isooctane; alicyclic hydrocarbon solvents such as cyclopentane, methylcyclopentane, cyclohexane, methylcyclohexane and ethylcyclohexane; and aromatic hydrocarbon solvents such as benzene, toluene, ethylbenzene and xylene. As a specific example, the hydrocarbon solvent may be an aliphatic hydrocarbon solvent such as hexane.

[0045] Regarding the polymerization solvent, the concentration of the monomer is not particularly limited, but may be 3 wt % to 80 wt %, more specifically, 10 wt % to 30 wt %.

[0046] The polymerization in step 1 may be performed by radical polymerization, and may be performed by various methods such as bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization, or may be performed by a batch method, a continuous method, or a semi-continuous method.

[0047] Specifically, if prepared by solution polymerization, the living polymer according to one embodiment of the present invention may be obtained by injecting a conjugated diene-based monomer into a catalyst composition and reacting in a polymerization solvent.

[0048] Furthermore, the polymerization may be heating polymerization, isothermal polymerization, or constant temperature polymerization (adiabatic polymerization).

[0049] Here, constant temperature polymerization refers to a polymerization method including a step of performing polymerization by utilizing its own reaction heat without optionally supplying heat after injecting the catalyst composition, heating polymerization refers to a polymerization method in which the temperature is increased by optionally supplying heat after injecting the catalyst composition, and isothermal polymerization refers to a polymerization method in which the temperature of the polymer is kept constant by removing heat or supplying heat after injecting the catalyst composition.

[0050] The polymerization in step 1 can be carried out at a temperature of 30°C to 65°C, particularly above 30°C, above 40°C, above 45°C, above 50°C, and below 65°C, below 60°C, below 55°C.

[0051] In the present invention, by conducting the polymerization reaction at a low temperature below 70° C., the conjugated diene polymer can be effectively prepared under mild conditions, and the present invention is characterized in that the conjugated diene polymer is prepared by fully controlling the polymerization reaction while not reducing the rate and efficiency of the polymerization reaction.

[0052] Specifically, as described above, the activity performance of the living polymer can be improved by lowering the polymerization temperature to 30° C. to 65° C., whereby the functional group from the modifier can be effectively bonded to the terminal of the living polymer in the modification step to increase the modification rate. In addition, by controlling the polymerization temperature within the above range, a modified conjugated diene-based polymer having excellent linearity compared to a higher polymerization temperature can be prepared.

[0053] Through such temperature control, although the same catalyst composition and conjugated diene-based monomers are used as reactants, a modified conjugated diene-based polymer having even better tensile properties and viscoelastic properties and excellent affinity with fillers can be prepared.

[0054] If the polymerization temperature is higher than 65°C, the activity performance of the active polymer is reduced, the modification rate is reduced, and a modified conjugated diene polymer with deteriorated linearity is prepared. In short, it becomes difficult to improve the effect of improving the affinity of the modified conjugated diene polymer with the filler, and thus, the mixing performance of the rubber composition is deteriorated. In addition, if the polymerization temperature is lower than 30°C, the polymerization reaction rate or efficiency is significantly reduced, and the preparation of the conjugated diene polymer becomes difficult.

[0055] As described above, since the neodymium compound and the second alkylating agent are mixed in a molar ratio of 1:20 to 1:35, the activity performance of the active polymer can be improved and the modification rate can be increased despite the use of the catalyst composition using a small amount of the second alkylating agent, and these effects can be maximized by controlling the polymerization temperature within the above range.

[0056] Furthermore, the polymerization can be carried out within the above temperature range for more than 15 minutes, more than 30 minutes, and less than 3 hours, less than 2 hours, for example, 1 hour, until the polymerization conversion rate reaches more than 95%, more than 99%, and at most 100%.

[0057] As described above, the catalyst composition of the present invention may include (a) a neodymium compound, (b) a first alkylating agent, (c) a second alkylating agent, and (d) a halide, and may further include (e) a conjugated diene-based monomer.

[0058] (a) Neodymium compounds

[0059] The neodymium compound is activated by the first alkylating agent and the second alkylating agent, and then forms a catalyst active substance for polymerizing the conjugated diene monomer.

[0060] Neodymium compounds may include carboxylates thereof (e.g., neodymium acetate, neodymium acrylate, neodymium methacrylate, neodymium gluconate, neodymium citrate, neodymium fumarate, neodymium lactate, neodymium maleate, neodymium oxalate, neodymium 2-ethylhexanoate, neodymium neodecanoate (versatate), etc.); organic phosphates thereof (e.g., neodymium dibutyl phosphate, neodymium dipentyl phosphate, neodymium dihexyl phosphate, neodymium diheptyl phosphate, neodymium dioctyl phosphate, neodymium bis(1-methylheptyl) phosphate, neodymium bis(2-ethylhexyl) phosphate, neodymium didecyl phosphate, etc.); organic phosphonates thereof (e.g., neodymium butyl phosphonate, neodymium pentyl phosphonate, neodymium hexyl phosphonate, neodymium heptyl phosphonate, neodymium oct ... Its organic phosphinates (for example, neodymium butylphosphinate, neodymium pentylphosphinate, neodymium hexylphosphinate, neodymium heptylphosphinate, neodymium octylphosphinate, (1-methylheptyl)phosphinate, neodymium (2-ethylhexyl)phosphinate, neodymium decylphosphinate, neodymium dodecylphosphinate, neodymium octadecylphosphinate, etc.); its organic phosphinates (for example, neodymium butylphosphinate, neodymium pentylphosphinate, neodymium hexylphosphinate, neodymium heptylphosphinate, neodymium octylphosphinate, (1-methylheptyl)phosphinate, neodymium (2-ethylhexyl)phosphinate, etc.); its carbamates (for example, neodymium dimethylcarbamate, neodymium diethylcarbamate, neodymium diisopropylcarbamate, dibutylcarbamate, neodymium dibenzylcarbamate, etc.); its dithiocarbamates (for example , neodymium dimethyldithiocarbamate, neodymium diethyldithiocarbamate, neodymium diisopropyldithiocarbamate, neodymium dibutyldithiocarbamate, etc.); xanthates thereof (e.g., neodymium methylxanthate, neodymium ethylxanthate, neodymium isopropylxanthate, neodymium butylxanthate, neodymium benzylxanthate, etc.); β-diketonates thereof (e.g., neodymium acetylacetonate, neodymium trifluoroacetylacetonate, neodymium hexafluoroacetylacetonate, neodymium benzoylacetonate, etc.); alkoxides or aromatic oxides thereof (e.g., neodymium methanolate, neodymium ethoxide, neodymium isopropylate, neodymium phenolate, neodymium nonylphenolate, etc.); halides or quasi-halides thereof (e.g., neodymium fluoride, Neodymium chloride, neodymium bromide, neodymium iodide, neodymium cyanide, neodymium cyanate, neodymium thiocyanate, neodymium azide, etc.); its oxyhalides (for example, neodymium oxyfluoride, neodymium oxychloride, neodymium oxybromide, etc.); or organic neodymium-containing compounds containing one or more neodymium-carbon bonds (for example, Cp3Nd, Cp2NdR, Cp2NdCl, CpNdCl2, CpNd(cyclooctatetraene), (C5Me5)2NdR, NdR3, Nd(allyl)3, Nd(allyl)2Cl, etc., wherein R represents a hydrocarbon group), and may include any one of them or a mixture of two or more of them.

[0061] Specifically, the neodymium compound may be a compound represented by Formula 1 below.

[0062] [Formula 1]

[0063]

[0064] In formula 1,

[0065] R a To R care independently hydrogen or an alkyl group having 1 to 12 carbon atoms, wherein all R a To R c Not at the same time hydrogen.

[0066] Furthermore, the neodymium compound may be R in view of excellent solubility in solvents without worrying about oligomerization, conversion rate to catalytically active species, and subsequent excellent improvement effect of catalyst activity. a is an alkyl group of 4 to 12 carbon atoms, R b and R c Formula 1 wherein each is independently hydrogen or an alkyl group of 1 to 8 carbon atoms.

[0067] In a more specific embodiment, the neodymium compound may be R a is an alkyl group of 6 to 10 carbon atoms, R b and R c Formula 1 wherein each is independently hydrogen or an alkyl group of 1 to 4 carbon atoms.

[0068] In a more specific embodiment, the neodymium compound may be R a is an alkyl group of 8 to 10 carbon atoms, R b and R c Formula 1 wherein each is independently hydrogen or an alkyl group of 1 to 3 carbon atoms.

[0069] As described above, if the neodymium compound of Formula 1 contains a carboxylate ligand containing an alkyl group of different lengths having 2 or more carbon atoms as a substituent at the α (alpha) position, a spatial change is induced around the neodymium central metal to block the flocculation phenomenon between the compounds, and as a result, oligomerization is suppressed. In addition, this neodymium compound has high solubility in a solvent, the ratio of neodymium located in the central part that is difficult to convert into a catalyst active substance is reduced, and the conversion rate to the active substance is high.

[0070] More specifically, the neodymium compound may be selected from Nd(neodecanoic acid)3, Nd(2-ethylhexanoic acid)3, Nd(2,2-dimethyldecanoic acid)3, Nd(2,2-diethyldecanoic acid)3, Nd(2,2-dipropyldecanoic acid)3, Nd(2,2-dibutyldecanoic acid)3, Nd(2,2-dihexyldecanoic acid)3, Nd(2,2-dioctyldecanoic acid)3, Nd(2-ethyl-2-propyldecanoic acid)3, Nd(2-ethyl-2-butyldecanoic acid)3, Nd(2-ethyl-2-hexyldecanoic acid)3, Nd(2-propyl-2-butyldecanoic acid)3, Nd(2-propyl-2-hexyldecanoic acid)3, Nd(2-propyl-2-isopropyldecanoic acid)3, Nd(2- One or more of Nd(2-butyl-2-hexyldecanoic acid)3, Nd(2-hexyl-2-octyldecanoic acid)3, Nd(2,2-diethyl-octanoic acid)3, Nd(2,2-dipropyloctanoic acid)3, Nd(2,2-dibutyloctanoic acid)3, Nd(2,2-dihexyloctanoic acid)3, Nd(2-ethyl-2-propyloctanoic acid)3, Nd(2-ethyl-2-hexyloctanoic acid)3, Nd(2,2-diethylnonanoic acid)3, Nd(2,2-dipropylnonanoic acid)3, Nd(2,2-dibutylnonanoic acid)3, Nd(2,2-dihexylnonanoic acid)3, Nd(2-ethyl-2-propylnonanoic acid)3 and Nd(2-ethyl-2-hexylnonanoic acid)3.

[0071] In addition, the solubility of the neodymium compound at room temperature (23±5°C) per 6g of non-polar solvent can be about 4g or more. The solubility of the neodymium compound refers to the degree of transparent dissolution without turbidity. With this high solubility, excellent catalyst activity can be obtained.

[0072] In addition, the neodymium compound can be used in the form of a reactant with a Lewis base. Due to the Lewis base, the reactant can increase the solubility of the neodymium compound in the solvent and can be stored for a long time in a stable state. For example, per 1 mol of neodymium element, a Lewis base can be used in a ratio of less than 30 mol, or 1 mol to 10 mol. Examples of Lewis bases can be acetylacetone, tetrahydrofuran, pyridine, N,N-dimethylformamide, thiophene, diphenyl ether, triethylamine, an organic phosphorus compound, or a monohydric alcohol or a dihydric alcohol.

[0073] (b) First Alkylating Agent

[0074] The first alkylating agent is aluminoxane, which can be prepared by reacting a trihydrocarbylaluminum compound with water. Specifically, the aluminoxane can be a linear aluminoxane of the following formula 2a or a cyclic aluminoxane of the following formula 2b.

[0075] [Formula 2a]

[0076]

[0077] [Formula 2b]

[0078]

[0079] In Formula 2a and Formula 2b, R is a monovalent organic group bonded to the aluminum atom through a carbon atom and may be a hydrocarbon group, and x and y may each independently be an integer of 1 or more, specifically 1 to 100, more specifically 2 to 50.

[0080] More specifically, the aluminoxane may include methylaluminoxane (MAO), modified methylaluminoxane (MMAO), ethylaluminoxane, n-propylaluminoxane, isopropylaluminoxane, n-butylaluminoxane, isobutylaluminoxane, n-pentylaluminoxane, neopentylaluminoxane, n-hexylaluminoxane, n-octylaluminoxane, 2-ethylhexylaluminoxane, cyclohexylaluminoxane, 1-methylcyclopentylaluminoxane, phenylaluminoxane or 2,6-dimethylphenylaluminoxane.

[0081] Furthermore, the modified methylaluminoxane may be one in which the methyl group of methylaluminoxane is substituted with a molecular formula group (R), specifically a hydrocarbon group having 2 to 20 carbon atoms, and may specifically be a compound represented by Formula 3 below.

[0082] [Formula 3]

[0083]

[0084] In Formula 3, R is the same as defined above, and m and n may each independently be an integer greater than 2. In Formula 3, Me represents a methyl group.

[0085] Specifically, in Formula 3, R can be an alkyl group having 2 to 20 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, a cycloalkenyl group having 3 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an arylalkyl group having 7 to 20 carbon atoms, an alkylaryl group having 7 to 20 carbon atoms, an allyl group, or an alkynyl group having 2 to 20 carbon atoms, and can specifically be an alkyl group having 2 to 20 carbon atoms, such as ethyl, isobutyl, hexyl, and octyl, and can more specifically be an isobutyl group.

[0086] More specifically, the modified methylaluminoxane may be one in which about 50 mol% to 90 mol% of the methyl groups in the methylaluminoxane are substituted with the above-mentioned hydrocarbon groups. If the amount of the substituted hydrocarbon groups in the modified methylaluminoxane is within the above-mentioned range, alkylation may be promoted to improve catalyst activity.

[0087] Modified methylaluminoxane can be prepared by conventional methods, and can specifically use trimethylaluminum and the alkylaluminum preparation except trimethylaluminum. In this case, the alkylaluminum can be triisopropylaluminum, triethylaluminum, trihexylaluminum or trioctylaluminum, and any one thereof or a mixture of two or more thereof can be used.

[0088] Furthermore, according to one embodiment of the present invention, the modified conjugated diene-based polymer prepared thereby may be formed to have a narrow molecular weight distribution, and in terms of improving physical properties of the polymer, preferably, the first alkylating agent may be methylaluminoxane.

[0089] (c) Second Alkylating Agent

[0090] The second alkylating agent according to one embodiment of the present invention may be a dihydrocarbyl aluminum hydride or a hydrocarbyl aluminum dihydride. Specifically, the second alkylating agent may include a dihydrocarbyl aluminum hydride, such as diethyl aluminum hydride, di-n-propyl aluminum hydride, diisopropyl aluminum hydride, di-n-butyl aluminum hydride, diisobutyl aluminum hydride (DIBAH), di-n-octyl aluminum hydride, diphenyl aluminum hydride, di-p-tolyl aluminum hydride, dibenzyl aluminum hydride, phenylethyl aluminum hydride, phenyl-n-propyl aluminum hydride, phenylisopropyl aluminum hydride, phenyl-n-butyl aluminum hydride, phenylisobutyl aluminum hydride, phenyl-n-octyl aluminum hydride, p-Tolylethylaluminum hydride, p-tolyln-propylaluminum hydride, p-tolylisopropylaluminum hydride, p-tolyln-butylaluminum hydride, p-tolylisobutylaluminum hydride, p-tolyln-octylaluminum hydride, benzylethylaluminum hydride, benzyln-propylaluminum hydride, benzylisopropylaluminum hydride, benzyln-butylaluminum hydride, benzylisobutylaluminum hydride, and benzyln-octylaluminum hydride; alkylaluminum hydrides such as ethylaluminum dihydride, n-propylaluminum dihydride, isopropylaluminum dihydride, n-butylaluminum dihydride, isobutylaluminum dihydride, and n-octylaluminum dihydride; or combinations thereof without limitation.

[0091] Meanwhile, in the catalyst composition according to one embodiment of the present invention, the alkylating agent is an organic metal compound capable of transferring a hydrocarbon group to another metal and can be used as a co-catalyst.

[0092] Furthermore, as required, the catalyst composition according to one embodiment of the present invention may further contain, in addition to the first alkylating agent and the second alkylating agent, a conventional alkylating agent used as an alkylating agent in the process of preparing a conventional conjugated diene-based polymer, and such an alkylating agent may include alkylaluminum, such as trimethylaluminum, triethylaluminum, tri-n-propylaluminum, triisopropylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-tert-butylaluminum, tripentylaluminum, trihexylaluminum, tricyclohexylaluminum and trioctylaluminum; and alkylmagnesium compounds, such as diethylmagnesium, di-n-propylmagnesium, diisopropylmagnesium, dibutylmagnesium, dihexylaluminum, diphenylmagnesium and dibenzylmagnesium, and the organic lithium compound may include an alkyllithium compound, such as n-butyllithium.

[0093] (d) Halides

[0094] In addition, the halide is not specifically limited, but may include, for example, elemental halogen, interhalogen compound, hydrogen halide, organic halide, non-metallic halide, metal halide and organic metal halide, and any one thereof or a mixture of two or more thereof may be used. Wherein, in view of the enhanced catalyst activity and the improved reactivity obtained, any one selected from organic halide, metal halide and organic metal halide, or a mixture of two or more thereof may be used as the halide.

[0095] Elemental halogens can include diatomic molecular compounds such as fluorine (F2), chlorine (Cl2), bromine (Br2), and iodine (I2).

[0096] Furthermore, the interhalogen compound may include iodine monochloride, iodine monobromide, iodine trichloride, iodine pentafluoride, iodine monofluoride, or iodine trifluoride.

[0097] Furthermore, the hydrogen halide may include hydrogen fluoride, hydrogen chloride, hydrogen bromide, or hydrogen iodide.

[0098] In addition, the organic halide may include tert-butyl chloride (t-BuCl), tert-butyl bromide, allyl chloride, allyl bromide, benzyl chloride, benzyl bromide, chlorodiphenylmethane, bromodiphenylmethane, triphenylchloromethane, triphenylbromomethane, benzal chloride, benzal bromide, methyltrichlorosilane, phenyltrichlorosilane, dimethyldichlorosilane, diphenyldichlorosilane, trimethylchlorosilane (TMSCl), benzoyl chloride, benzoyl bromide, propionyl chloride, propionyl bromide, methyl chloroformate, methyl bromoformate, iodomethane, diiodomethane, triiodomethane (also known as "iodoform"), Tetraiodomethane, 1-iodopropane, 2-iodopropane, 1,3-diiodopropane, tert-butyl iodide, 2,2-dimethyl-1-iodopropane (also known as "neopentyl iodide"), allyl iodide, iodobenzene, benzyl iodide, diphenylmethane iodide, triphenylmethane iodide, benzaldiiodide (also known as "benzylidene diiodide"), trimethylsilyl iodide, triethylsilyl iodide, triphenylsilyl iodide, dimethyldiiodosilane, diethyldiiodosilane, diphenyldiiodosilane, methyltriiodosilane, ethyltriiodosilane, phenyltriiodosilane, benzoyl iodide, propionyl iodide, and methyl iodoformate.

[0099] In addition, non-metal halides can include phosphorus trichloride, phosphorus tribromide, phosphorus pentachloride, phosphorus oxychloride, phosphorus oxybromide, boron trifluoride, boron trichloride, boron tribromide, silicon tetrafluoride, silicon tetrachloride (SiCl4), silicon tetrabromide, arsenic trichloride, arsenic tribromide, selenium tetrachloride, selenium tetrabromide, tellurium tetrachloride, tellurium tetrabromide, silicon tetraiodide, arsenic triiodide, tellurium tetraiodide, boron triiodide, phosphorus triiodide, phosphorus oxyiodide, or selenium tetraiodide.

[0100] In addition, the metal halide can include tin tetrachloride, tin tetrabromide, aluminum trichloride, aluminum tribromide, antimony trichloride, antimony pentachloride, antimony tribromide, aluminum trifluoride, gallium trichloride, gallium tribromide, gallium trifluoride, indium trichloride, indium tribromide, indium trifluoride, titanium tetrachloride, titanium tetrabromide, zinc dichloride, zinc dibromide, zinc difluoride, aluminum triiodide, gallium triiodide, indium triiodide, titanium tetraiodide, zinc diiodide, germanium tetraiodide, tin tetraiodide, tin diiodide, antimony triiodide, or magnesium diiodide.

[0101] In addition, the organometallic halide may include dimethylaluminum chloride, diethylaluminum chloride, dimethylaluminum bromide, diethylaluminum bromide, dimethylaluminum fluoride, diethylaluminum fluoride, methylaluminum dichloride, ethylaluminum dichloride, methylaluminum dibromide, ethylaluminum dibromide, methylaluminum difluoride, ethylaluminum difluoride, sesquimethylaluminum chloride, sesquiethylaluminum chloride (EASC), sesquiisobutylaluminum chloride, methylmagnesium chloride, methylmagnesium bromide, ethylmagnesium chloride, ethylmagnesium bromide, n-butylmagnesium chloride, n-butylmagnesium bromide, phenylmagnesium chloride, phenylmagnesium bromide, benzylmagnesium chloride, trimethyltin chloride, trimethyltin bromide, triethyltin chloride, triethyltin bromide, di-tert-butyldi Tin chloride, di-tert-butyltin dibromide, di-n-butyltin dichloride, di-n-butyltin dibromide, tri-n-butyltin chloride, tri-n-butyltin bromide, methylmagnesium iodide, dimethylaluminum iodide, diethylaluminum iodide, di-n-butylaluminum iodide, diisobutylaluminum iodide, di-n-octylaluminum iodide, methylaluminum diiodide, ethylaluminum diiodide, n-butylaluminum diiodide, isobutylaluminum diiodide, sesquimethylaluminum iodide, sesquiethylaluminum iodide, sesquiisobutylaluminum iodide, ethylmagnesium iodide, n-butylmagnesium iodide, isobutylmagnesium iodide, phenylmagnesium iodide, benzylmagnesium iodide, trimethyltin iodide, triethyltin iodide, tri-n-butyltin iodide, di-n-butyltin diiodide, or di-tert-butyltin diiodide.

[0102] Furthermore, the catalyst composition according to one embodiment of the present invention may include a compound containing a non-coordinating anion or a non-coordinating anion precursor compound instead of or together with the halide.

[0103] Specifically, in the compound containing a non-coordinating anion, the non-coordinating anion is a bulky anion that cannot form a coordination bond with the active center of the catalyst system due to steric hindrance, wherein the non-coordinating anion can be a tetraarylborate anion or a fluorinated tetraarylborate anion. In addition, in addition to the above-mentioned non-coordinating anions, the compound containing a non-coordinating anion can also contain a counter cation, for example, a carbonium cation such as a triarylcarbonium cation; an ammonium cation such as an N,N-dialkylanilinium cation, or a phosphonium cation.

[0104] More specifically, the compound containing a non-coordinating anion may include triphenylcarbonium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, triphenylcarbonium tetrakis[3,5-bis(trifluoromethyl)phenyl]borate, or N,N-dimethylanilinium tetrakis[3,5-bis(trifluoromethyl)phenyl]borate.

[0105] In addition, the non-coordinating anion precursor as a compound capable of forming a non-coordinating anion under the reaction conditions may include triarylboron compounds (BE3, wherein E is a strongly electron-withdrawing aryl group, such as pentafluorophenyl and 3,5-bis(trifluoromethyl)phenyl).

[0106] (e) Conjugated diene monomers

[0107] In addition, the catalyst composition may also contain a conjugated diene monomer, and since the catalyst composition is used in the form of a preformed or premixed catalyst composition in which a portion of the conjugated diene monomer used in the polymerization reaction is prepolymerized by premixing with the catalyst composition for polymerization, not only the activity of the catalyst composition can be improved, but also the conjugated diene polymer prepared thereby can be stabilized.

[0108] In the present invention, the expression "preformation" may mean that in the case of a catalyst composition comprising a neodymium compound, an alkylating agent and a halide, that is, the catalyst system comprises diisobutylaluminum hydride (DIBAH), a small amount of conjugated diene monomers such as 1,3-butadiene is added to reduce the possibility of generating active substances of various catalyst compositions, and prepolymerization is performed in the catalyst composition system to which 1,3-butadiene is added. In addition, the expression "premixing" may mean a state in which each compound is uniformly mixed in the catalyst composition system but polymerization is not performed.

[0109] In this case, for the conjugated diene monomer used for preparing the catalyst composition, some amount within the total amount of the conjugated diene monomer used in the polymerization reaction can be used, for example, based on 1 mol of the neodymium compound, the conjugated diene monomer can be used in an amount of 1 mol to 100 mol, specifically 10 mol to 50 mol, or 20 mol to 50 mol.

[0110] In addition, in the preparation method of the modified conjugated diene polymer of the present invention, after preparing the active polymer, a step of terminating the polymerization by further using an additive, such as a reaction quencher such as polyoxyethylene glycol phosphate, or an antioxidant such as 2,6-di-tert-butyl-p-cresol, may be included. In addition, together with the reaction quencher, an additive that promotes solution polymerization, for example, an additive such as a chelating agent, a dispersant, a pH control agent, a deoxidizer, and an oxygen scavenger may also be selectively used.

[0111] As a result of this polymerization reaction, a conjugated diene polymer containing an active organometallic portion from a catalyst containing a neodymium compound, more specifically, a neodymium-catalyzed conjugated diene polymer containing 1,3-butadiene monomer units can be prepared. The conjugated diene polymer thus prepared can have active properties or quasi-active properties.

[0112] Step 2

[0113] Step 2 is a step of reacting or coupling the living polymer with a modifying agent, and modification may be performed by reacting the organometallic portion of the living polymer with the modifying agent.

[0114] The modification reaction may be carried out by a solution reaction or a solid phase reaction, specifically by a solution reaction. In another embodiment, the modification reaction may be carried out using a batch reactor or a continuous type by using an apparatus such as a multi-step continuous reactor and an inline mixer.

[0115] In another embodiment, the modification reaction can be carried out under the same temperature and pressure conditions as the conventional polymerization reaction, and in a specific embodiment, can be carried out at a temperature of 30°C to 65°C, specifically, above 30°C, above 40°C, above 45°C, above 50°C, and below 65°C, below 60°C, below 55°C.

[0116] Any compound that can give functional group to at least one end of active polymer or improve molecular weight by coupling can be used as properties-correcting agent, and its type is not limited in the present invention.For example, the compound can include one or more functional groups selected from aziridine base, keto group, carboxyl, thiocarboxyl, carbonate group, carboxylic anhydride, metal carboxylate, oxyhalide, urea group, thiourea group, amide group, thioamide group, isocyanate group, thioisocyanate group, halogenated isocyanate group, epoxy group, thioepoxy group, imino group and MZ key (wherein, M is selected from Sn, Si, Ge and P, and Z is a halogen atom), and does not include active proton and onium salt.

[0117] The modifier may be used at 0.5 mol to 20 mol based on 1 mol of the neodymium compound in the catalyst composition. Specifically, the modifier may be used at 1 mol to 10 mol based on 1 mol of the neodymium compound in the catalyst composition.

[0118] After the above modification reaction is completed, the polymerization reaction can be terminated by adding an isopropanol solution of 2,6-di-tert-butyl-p-cresol (BHT) to the polymerization reaction system. Thereafter, the modified conjugated diene polymer can be obtained by desolvation treatment, such as stripping by supplying water vapor to reduce the partial pressure of the solvent, or vacuum drying treatment. In addition, in addition to the above modified conjugated diene polymer, an unmodified active polymer can also be included in the reaction product obtained as a result of the above modification reaction.

[0119] The preparation method of the modified conjugated diene polymer of the present invention may further include the process of precipitating and isolating the modified conjugated diene polymer prepared thereby. The process of filtering, isolating and drying the precipitated modified conjugated diene polymer may be carried out according to common methods.

[0120] As described above, according to the modified conjugated diene-based polymer according to one embodiment of the present invention, a modified conjugated diene-based polymer having excellent physical properties and a narrow molecular weight distribution, specifically, a neodymium-catalyzed butadiene-based polymer may be prepared.

[0121] In addition, the present invention provides a modified conjugated diene-based polymer prepared by the preparation method.

[0122] The modified conjugated diene polymer according to one embodiment of the present invention is prepared under the conditions of the catalyst composition and polymerization temperature having the above-mentioned characteristics, and the rubber composition containing the modified conjugated diene polymer can have an optimized molecular weight distribution to improve the balance of physical properties including viscoelastic properties, tensile properties and processing properties as well as high linearity.

[0123] The modification rate of the modified conjugated diene polymer may be 5 mol% to 80 mol%, specifically, 10 mol% to 80 mol%, or 20 mol% to 80 mol%. Within this range, the mechanical properties of the rubber composition including the modified conjugated diene polymer, including tensile properties and viscoelastic properties, may be excellent. The modification rate may refer to the ratio of the modified conjugated diene polymer reacted or coupled with the modifier in step 2 in the active polymer prepared in step 1.

[0124] The modified conjugated diene polymer may have a cis-1,4 bond content in the conjugated diene portion measured by Fourier transform infrared spectroscopy (FT-IR) of 95% or more, 96% or more, or 96.5% or more. If the modified conjugated diene polymer is used in a rubber composition, the wear resistance, crack resistance, and ozone resistance of the rubber composition may be improved.

[0125] In addition, the content of vinyl bonds in the conjugated diene part of the modified conjugated diene polymer measured by Fourier transform infrared spectroscopy can be 5% or less, 3% or less, 1% or less, or 0.7% or less. If the vinyl content in the polymer is greater than 5%, the wear resistance, crack resistance, and ozone resistance of the rubber composition containing the polymer will deteriorate.

[0126] Here, the cis-1,4 bond content and the vinyl content in the polymer by FT-IR can be obtained by measuring the FT-IR transmission spectrum of a carbon disulfide solution of a conjugated diene-based polymer prepared at a concentration of 5 mg / ml and using carbon disulfide of the same cell as a blank, and using 1130 cm-1 in the measured spectrum. -1 The maximum peak (a, baseline) at 967 cm-1 shows the trans-1,4 bond. -1 The smallest peak near (b) shows the ethylene bond at 911 cm -1 The smallest peak near (c) and 736 cm showing cis-1,4 bonds -1 The minimum peak value near (d).

[0127] The molecular weight distribution of the conjugated diene polymer may be 1.5 to 3.5, specifically, the molecular weight distribution of the conjugated diene polymer may be 2.0 or more, and 3.0 or less, or 2.8 or less. With such a narrow molecular weight distribution, if used in a rubber composition, the tensile properties and viscoelastic properties may be excellent.

[0128] Molecular weight distribution can be calculated by the ratio (Mw / Mn) of weight average molecular weight (Mw) and number average molecular weight (Mn). Number average molecular weight (Mn) is the common average of the molecular weight of a single polymer, which is calculated by measuring the molecular weight of n polymer molecules, obtaining the sum of molecular weights, and dividing the sum by n, and weight average molecular weight (Mw) represents the molecular weight distribution of polymer composition. All average molecular weights can be expressed as grams per mole (g / mol). In addition, weight average molecular weight and number average molecular weight can refer to the molecular weight converted by polystyrene analyzed by gel permeation chromatography (GPC), respectively.

[0129] The conjugated diene polymer according to one embodiment of the present invention can meet the molecular weight distribution conditions, and the weight average molecular weight (Mw) can be 4x10 5 g / mol to 1.0x10 6 g / mol, specifically, 4.00x10 5 g / mol or above, 4.50x10 5 g / mol or above, 5.00x10 5 g / mol / or above, 6.00x105 g / mol or more, 7.00x10 5 g / mol and above, and 1.00x10 6 g / mol or less, 9.00x10 5 Below g / mol.

[0130] In addition, the number average molecular weight (Mn) can be 2.0x10 5 g / mol to 5.0x10 5 g / mol, 2.00x10 5 g / mol or more, 2.50x10 5 g / mol or more, 2.70x10 5 g / mol / or above, and 5.00x10 5 g / mol or less, 4.00x10 5 g / mol or less, 3.50x10 5 Below g / mol.

[0131] Within these ranges, if used in a rubber composition, the tensile properties are excellent, the processing properties are excellent, the processability of the rubber composition is improved, mixing and kneading are easy, and the rubber composition can achieve an excellent balance of mechanical properties and physical properties.

[0132] More specifically, if the conjugated diene polymer satisfies the weight average molecular weight (Mw) and number average molecular weight conditions and the molecular weight distribution, and if used in a rubber composition, the rubber composition is excellent in tensile properties, viscoelastic properties and processability, and the balance therebetween is excellent.

[0133] In addition, the Mooney viscosity (MV) of the modified conjugated diene polymer at 100° C. may be 20 to 100, specifically, 20 or more, 30 or more, 35 or more, 40 or more, 50 or more, and 100 or less, 80 or less, 75 or less, 70 or less. The modified conjugated diene polymer according to the present invention has a Mooney viscosity within the above range and can have excellent processability.

[0134] The Mooney viscosity can be measured, for example, using MV2000E of Monsanto Co. using a large rotor at a rotor speed of 2±0.02 rpm at 100° C. In this case, the sample used is left at room temperature (23±3° C.) for more than 30 minutes, and 27±3 g of the sample can be collected and put into the mold cavity, then, the press plate is operated, and the Mooney viscosity is measured.

[0135] The modified conjugated diene polymer may have a β value (β-value) of 0.190 or more, specifically, 0.195 or more, 0.200 or more, or 0.210 or more. With such a high β value, if used in a rubber composition, the resistance performance and fuel consumption performance may be excellent.

[0136] Here, the β value refers to the change in the viscoelastic coefficient according to the frequency change in response to the same amount of strain, wherein it is an indicator of the linearity of the polymer. Generally, when the β value decreases, the linearity of the polymer is lower, and if used in a rubber composition, the rolling resistance or rotational resistance increases as the linearity decreases.

[0137] The β value was obtained by performing a frequency sweep under the conditions of 7% strain and 100° C. using a rubber process analyzer (RPA2000, Alphs Technoligies Co.), and calculating the slope of Log(1 / tanδ) versus Log(frequency). In this case, the frequency was set to 2, 5, 10, 20, 50, 100, 200, 500, 1,000, and 2,000 cpm.

[0138] Furthermore, the present invention provides a rubber composition comprising the modified conjugated diene-based polymer and a molded product produced from the rubber composition.

[0139] The rubber composition may include 0.1 wt % to 100 wt %, specifically 10 wt % to 100 wt %, or 20 wt % to 90 wt % of the modified conjugated diene polymer. If the amount of the modified conjugated diene polymer is less than 0.1 wt %, the molded product manufactured by using the rubber composition, for example, the improvement effect of the wear resistance and crack resistance of the tire will not be obvious.

[0140] In addition, as required, in addition to the modified conjugated diene polymer, the rubber composition may also include other rubber components, in which case the content of the rubber component may be 90% by weight or less based on the total weight of the rubber composition. Specifically, the content of the rubber component may be 1 to 900 parts by weight based on 100 parts by weight of the modified conjugated diene polymer.

[0141] The rubber component may be a natural rubber or a synthetic rubber, and, for example, the rubber component may be a natural rubber (NR) including cis-1,4-polyisoprene; a modified natural rubber in which a conventional natural rubber is modified or purified, such as epoxidized natural rubber (ENR), deproteinized natural rubber (DPNR), and hydrogenated natural rubber; and a synthetic rubber, such as styrene-butadiene rubber (SBR), polybutadiene (BR), polyisoprene (IR), butyl rubber (IIR), ethylene-propylene copolymer, polyisobutylene-co-isoprene, chloroprene rubber, poly(ethylene-co-propylene), poly(styrene-co-butadiene), poly(styrene-co-isoprene), poly(styrene-co-isoprene-co-butadiene), poly(isoprene-co-butadiene), poly(ethylene-co-propylene-co-diene), polysulfide rubber, acrylic rubber, polyurethane rubber, silicone rubber, epichlorohydrin rubber, and halogenated butyl rubber. Any one of them or a mixture of two or more thereof may be used.

[0142] In addition, based on 100 parts by weight of the conjugated diene polymer, the rubber composition may include 0.1 to 150 parts by weight of a filler, and the filler may include a silica filler, a carbon black filler, or a combination thereof. Specifically, the filler may be carbon black.

[0143] The carbon black filler is not particularly limited, but, for example, the nitrogen surface area per gram (N2SA, measured according to JIS K6217-2:2001) may be 20 m 2 / g to 250m 2 / g. In addition, the carbon black may have a dibutyl phthalate (DBP) oil absorption of 80cc / 100g to 200cc / 100g. If the nitrogen surface area per gram of the carbon black is greater than 250m 2 / g, the processing properties of the rubber composition will be reduced, and if the nitrogen surface area per gram of carbon black is less than 20m 2 / g, the reinforcement by carbon black will not be significant. In addition, if the DBP oil absorption of carbon black is greater than 200cc / 100g, the processability of the rubber composition will be reduced, and if the DBP oil absorption of carbon black is less than 80cc / 100g, the reinforcement by carbon black will not be significant.

[0144] In addition, there is no particular limitation on silicon dioxide, but, for example, wet silicon dioxide (hydrated silicic acid), dry silicon dioxide (anhydrous silicic acid), calcium silicate, aluminum silicate, or colloidal silicon dioxide may be included. Specifically, silicon dioxide may be wet silicon dioxide which has the most significant effect of improving both fracture characteristics and anti-wet skid characteristics. In addition, the nitrogen surface area per gram (N2SA) of silicon dioxide may be 120 m 2 / g to 180m 2 / g, and the surface area per gram of hexadecyltrimethylammonium bromide (CTAB) can be 100m 2 / g to 200m 2 / g. If the nitrogen surface area per gram of silicon dioxide is less than 120m 2 / g, the enhancement by silica decreases, and if the nitrogen surface area per gram of silica is greater than 180 m 2 / g, the processing properties of the rubber composition will be reduced. In addition, if the CTAB surface area per gram of silica is less than 100m 2 / g, the reinforcement of silica as a filler will decrease, and if the CTAB surface area per gram of silica is greater than 200m 2 / g, the processability of the rubber composition will decrease.

[0145] Meanwhile, if silica is used as a filler, a silane coupling agent may be used together for improving reinforcement and low exothermic properties.

[0146] Specific examples of the silane coupling agent may be bis(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyltetrasulfide, 3-triethoxysilylpropyl-N,N-dimethylthiocarbamoyltetrasulfide, sulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-trimethoxysilylpropylbenzothiazolyl tetrasulfide, 3-triethoxysilylpropylbenzoyl tetrasulfide, 3-triethoxysilylpropylmethacrylate monosulfide, 3-trimethoxysilylpropylmethacrylate monosulfide, bis(3-diethoxymethylsilylpropyl)tetrasulfide, 3-mercaptopropyldimethoxymethylsilane, dimethoxymethylsilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, or dimethoxymethylsilylpropylbenzothiazolyl tetrasulfide, and any one thereof or a mixture of two or more thereof may be used. More specifically, the silane coupling agent may be bis(3-triethoxysilylpropyl)polysulfide or 3-trimethoxysilylpropylbenzothiazolyl tetrasulfide in view of the enhanced improvement effect.

[0147] Furthermore, the rubber composition of the present invention may be sulfur-crosslinkable and, therefore, may further contain a vulcanizing agent.

[0148] The vulcanizing agent may be specifically sulfur powder, and may contain 0.1 to 10 parts by weight based on 100 parts by weight of the rubber component. If the vulcanizing agent within the above range is included, the elastic modulus and strength required for the vulcanized rubber composition may be ensured, and at the same time, low fuel consumption may be obtained.

[0149] In addition, the rubber composition according to one embodiment of the present invention may contain various additives used in the conventional rubber industry, such as vulcanization accelerators, processing oils, plasticizers, anti-aging agents, scorch retardants, zinc white, stearic acid, thermosetting resins, or thermoplastic resins in addition to the above-mentioned components.

[0150] The vulcanization accelerator is not particularly limited, but specifically, thiazole compounds such as 2-mercaptobenzothiazole (M), dibenzothiazolyl disulfide (DM), and N-cyclohexylbenzothiazolyl-2-sulfenamide (CZ), or guanidine compounds such as diphenylguanidine (DPG) can be used. Based on 100 parts by weight of the rubber component, the vulcanization accelerator may include 0.1 parts by weight to 5 parts by weight.

[0151] In addition, the processing oil acts as a softener in the rubber composition, and specifically, the processing oil may be paraffin, cycloalkane, or aromatic compound, and more specifically, in view of tensile strength and wear resistance, aromatic compound may be used, and in view of hysteresis loss and low temperature characteristics, cycloalkane or paraffin processing oil may be used. The content of the processing oil may be 100 parts by weight or less based on 100 parts by weight of the rubber component, and if the processing oil is included in the above amount, the tensile strength and low heat release performance (low fuel consumption rate) of the vulcanized rubber may be prevented from decreasing.

[0152] In addition, specific examples of the anti-aging agent may be N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, or a high temperature condensate of diphenylamine and acetone. Based on 100 parts by weight of the rubber component, the anti-aging agent may be used in an amount of 0.1 to 6 parts by weight.

[0153] The rubber composition of the present invention can be obtained by mixing the above-mentioned formula using a mixer such as a Banbury mixer, a roller and an internal mixer, and can be obtained by a vulcanization process after molding to obtain a rubber composition with excellent wear resistance and low heat release performance.

[0154] Therefore, the rubber composition can be suitably used for manufacturing various components of a tire such as a tire tread, a base tread, a sidewall, a carcass coating rubber, a belt coating rubber, a bead core, a chafer and a bead coating rubber, or various industrial rubber products such as anti-vibration rubber, a conveyor belt and a hose.

[0155] A molded article manufactured by using the rubber composition may include a tire or a tire tread.

[0156] Example

[0157] Hereinafter, the present invention will be described in more detail according to Examples. However, the following Examples are provided only to illustrate the present invention, and the scope of the present invention is not limited thereto.

[0158] [Preparation of Modifier]

[0159] 1.77 ml of triethylamine (Et3N) and 1.62 ml of trimethylsilyl chloride (TMSCl) were added to a solution of 2 g of ethyl piperidine-4-carboxylate dissolved in dichloromethane (CH2Cl2) at 0°C, and the mixture thus obtained was stirred at 0°C for 5 hours. Then, the solvent in the obtained solution was evaporated under reduced pressure, and the obtained residue was redissolved in hexane and filtered twice with hexane. The raw material thus filtered was separated by reduced pressure distillation to obtain ethyl 1-(trimethylsilyl)piperidine-4-carboxylate having the following structure, and observed 1 H NMR spectroscopy.

[0160]

[0161] 1 H NMR (500MHz, CDCl3): δ4.11-4.08(m,2H), δ3.13-3.11(m,2H), δ2.61-2.54(m,2H), δ2. 34-2.32(m,1H), δ1.74(m,2H), δ1.42(m,2H), δ1.23-1.22(m,3H), δ0.05-0.00(m,9H).

[0162] [Preparation of Catalyst Composition]

[0163] Preparation Example 1

[0164] Under nitrogen conditions, neodymium tert-carbonate (NdV, 0.80 mmol) was added to a hexane solvent, and methylaluminoxane (MAO, 80.0 mmol), diisobutylaluminum hydride (DIBAH, 16.0 mmol), diethylaluminum chloride (DEAC, 1.92 mmol) and 1,3-butadiene (16.0 mmol) were injected therein in sequence, and then mixed at -20°C for 12 hours to prepare a catalyst composition (NdV: DIBAH = 1: 20). The catalyst composition thus prepared was stored at -30°C to -20°C under nitrogen conditions for 24 hours and then used.

[0165] Preparation Example 2

[0166] Under nitrogen conditions, neodymium tert-carbonate (NdV, 0.60 mmol) was added to a hexane solvent, and methylaluminoxane (MAO, 60.0 mmol), diisobutylaluminum hydride (DIBAH, 18.0 mmol), diethylaluminum chloride (DEAC, 1.44 mmol) and 1,3-butadiene (12.0 mmol) were injected therein in sequence, and then mixed at -20°C for 12 hours to prepare a catalyst composition (NdV: DIBAH = 1: 30). The catalyst composition thus prepared was stored at -30°C to -20°C under nitrogen conditions for 24 hours and then used.

[0167] Preparation Example 3

[0168] Under nitrogen conditions, neodymium tert-carbonate (NdV, 0.40 mmol) was added to a hexane solvent, and methylaluminoxane (MAO, 40.0 mmol), diisobutylaluminum hydride (DIBAH, 14.0 mmol), diethylaluminum chloride (DEAC, 0.96 mmol) and 1,3-butadiene (8.0 mmol) were sequentially injected therein, and then mixed at -20°C for 12 hours to prepare a catalyst composition (NdV: DIBAH = 1: 35). The catalyst composition thus prepared was stored at -30°C to -20°C under nitrogen conditions for 24 hours and then used.

[0169] Comparative Preparation Example 1

[0170] Under nitrogen conditions, neodymium tert-carbonate (NdV, 1.00 mmol) was added to a hexane solvent, and methylaluminoxane (MAO, 40.0 mmol), diisobutylaluminum hydride (DIBAH, 10.0 mmol), diethylaluminum chloride (DEAC, 2.40 mmol) and 1,3-butadiene (30.0 mmol) were injected therein in sequence, and then mixed at -20°C for 12 hours to prepare a catalyst composition (NdV: DIBAH = 1: 10). The catalyst composition thus prepared was stored at -30°C to -20°C under nitrogen conditions for 24 hours and then used.

[0171] Comparative Preparation Example 2

[0172] Under nitrogen conditions, neodymium tert-carbonate (NdV, 0.20 mmol) was added to a hexane solvent, and methylaluminoxane (MAO, 20.0 mmol), diisobutylaluminum hydride (DIBAH, 10.0 mmol), diethylaluminum chloride (DEAC, 0.48 mmol) and 1,3-butadiene (4.0 mmol) were injected therein in sequence, and then mixed at -20°C for 12 hours to prepare a catalyst composition (NdV: DIBAH = 1: 50). The catalyst composition thus prepared was stored at -30°C to -20°C under nitrogen conditions for 24 hours and then used.

[0173] [Preparation of modified or unmodified conjugated diene polymer]

[0174] Example 1

[0175] To the completely dried reactor, vacuum and nitrogen were alternately applied, 4.2 kg of hexane and 500 g of 1,3-butadiene were injected into the 15 L reactor in a vacuum state, and the temperature was raised to 40° C. The catalyst composition of Preparation Example 1 was added thereto, and polymerization was performed for 60 minutes to prepare a living polymer.

[0176] To the living polymer, a hexane solution containing 2.5 g of the thus prepared modifier compound was added, and a modification reaction was performed for 60 minutes under the same temperature conditions as the polymerization conditions.

[0177] Then, a hexane solution containing 1.0 g of a polymerization quencher and a hexane solution containing 2.0 g of an antioxidant were added to terminate the reaction and prepare a modified conjugated diene-based polymer.

[0178] Example 2

[0179] A modified conjugated diene-based polymer was prepared by the same method as in Example 1, except that the temperature of the reactor was increased to 50°C.

[0180] Example 3

[0181] A modified conjugated diene-based polymer was prepared by the same method as in Example 1, except that the temperature of the reactor was increased to 60°C.

[0182] Example 4

[0183] A modified conjugated diene-based polymer was prepared by the same method as in Example 1, except that the catalyst composition of Preparation Example 2 was used instead of Preparation Example 1, and the temperature of the reactor was increased to 50°C.

[0184] Example 5

[0185] A modified conjugated diene-based polymer was prepared by the same method as in Example 1, except that the catalyst composition of Preparation Example 3 was used instead of Preparation Example 1, and the temperature of the reactor was increased to 50°C.

[0186] Comparative Example 1

[0187] As unmodified Nd-BR, BR1208 (manufacturer, LG Chem, Co.) was used.

[0188] Comparative Example 2

[0189] As unmodified Nd-BR, CB24 (manufacturer, Lanxess Co.) was used.

[0190] Comparative Example 3

[0191] A modified conjugated diene-based polymer was prepared by the same method as in Example 1, except that the catalyst composition of Comparative Preparation Example 1 was used instead of Preparation Example 1, and the temperature of the reactor was increased to 50°C.

[0192] Comparative Example 4

[0193] A modified conjugated diene-based polymer was prepared by the same method as in Example 1, except that the catalyst composition of Comparative Preparation Example 1 was used instead of Preparation Example 1, and the temperature of the reactor was increased to 70°C.

[0194] Comparative Example 5

[0195] A modified conjugated diene-based polymer was prepared by the same method as in Example 1, except that the catalyst composition of Comparative Preparation Example 2 was used instead of Preparation Example 1, and the temperature of the reactor was increased to 50°C.

[0196] Comparative Example 6

[0197] A modified conjugated diene-based polymer was prepared by the same method as in Example 1, except that the temperature of the reactor was increased to 70°C.

[0198] Comparative Example 7

[0199] A modified conjugated diene-based polymer was prepared by the same method as in Example 1, except that the catalyst composition of Preparation Example 2 was used instead of Preparation Example 1, and the temperature of the reactor was increased to 70°C.

[0200] Comparative Example 8

[0201] A modified conjugated diene-based polymer was prepared by the same method as in Example 1, except that the catalyst composition of Preparation Example 3 was used instead of Preparation Example 1, and the temperature of the reactor was increased to 70°C.

[0202] [Table 1]

[0203]

[0204] [Analysis of physical properties of modified conjugated diene polymers]

[0205] Experimental Example 1

[0206] For the polymers prepared in Examples and Comparative Examples, physical properties were analyzed according to the following methods, and the results are shown in Table 1.

[0207] (1) Microstructure analysis

[0208] The cis-1,4 bond content, the trans-1,4 bond content, and the vinyl content in the conjugated diene portion were measured by Fourier transform infrared spectroscopy (FT-IR).

[0209] Specifically, after measuring the FT-IR transmission spectrum of a carbon disulfide solution of a conjugated diene-based polymer prepared at a concentration of 5 mg / mL by using carbon disulfide of the same cell as a blank, the FT-IR spectrum was measured by using a wavelength of 1130 cm -1 The largest peak near (a, baseline) shows the trans-1,4 bond at 967 cm -1 The smallest peak near (b) shows the vinyl bond at 911 cm -1 The smallest peak near (c) and 736 cm showing cis-1,4 bonds -1 The minimum peak (d) near each content was obtained.

[0210] (2) Weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (MWD)

[0211] Each polymer was dissolved in tetrahydrofuran (THF) at 40°C for 30 minutes, and the resulting solution was loaded into a gel permeation chromatography (GPC) and flowed. In this case, two PLgelOlexis columns and one PLgel mixed-C column (trade name, Polymer Laboratories Co.) were used in combination. Moreover, the newly replaced columns were all mixed bed type columns, and polystyrene was used as a standard substance for gel permeation chromatography.

[0212] (3) Mooney viscosity (MV, ML1+4, @100℃)

[0213] Mooney viscosity (ML1+4, @100°C) (MU) is measured by using MV-2000E of Monsanto Co. using a large rotor at a rotor speed of 2±0.02 rpm at 100°C. In this case, the sample used is left at room temperature (23±3°C) for more than 30 minutes, and 27±3g of the sample is collected and put into the mold cavity, and then the pressing plate is operated to measure the Mooney viscosity while applying torque.

[0214] (4) β value (β-value)

[0215] The β value of each polymer was measured using a rubber process analyzer (RPA2000, Alpha Technologies Co.).

[0216] Specifically, frequency sweep was performed for each polymer under the conditions of 7% strain and 100° C. In this case, the frequency was set to 2, 5, 10, 20, 50, 100, 200, 500, 1,000 and 2,000 cpm, and the slope of Log(1 / tanδ) versus Log(frequency) was calculated to obtain the β value.

[0217] (5) Modification rate (%)

[0218] The modification rate was calculated using the chromatogram obtained by the chromatographic measurement. Specifically, each polymer was dissolved in tetrahydrofuran (THF) at 40°C to prepare a sample, and each sample was injected into a gel permeation chromatography (GPC) with tetrahydrofuran flowing as an eluent to obtain a chromatogram, and based on the chromatogram thus obtained, the modification rate was calculated by the following mathematical formula.

[0219] Modification rate (%)=[(peak area of ​​modified polymer) / (peak area of ​​unmodified polymer+peak area of ​​modified polymer)]×100.

[0220] [Table 2]

[0221]

[0222] According to the preparation method of the present invention, in Examples 1 to 5, a catalyst composition having a molar ratio of NdV (neodymium compound) to the second alkylating agent (DIBAH) of 1:20 to 1:35 is used, and polymerization is carried out at a temperature of 30°C to 65°C to prepare a modified conjugated diene polymer having excellent activity performance of an active polymer, showing a high modification rate and having excellent linearity.

[0223] Meanwhile, in Comparative Examples 3 and 4 using the catalyst composition of Comparative Preparation Example 1 having an extremely small amount of the second alkylating agent (DIBAH), in Comparative Example 5 using the catalyst composition of Comparative Preparation Example 2 having an excessive amount of the second alkylating agent (DIBAH), and in Comparative Examples 6 to 8 using the catalyst compositions of Preparation Examples 1 to 3 but polymerized at an excessively high polymerization temperature of 70° C., it was confirmed that the modification rate was low when compared with the Examples.

[0224] [Preparation of rubber composition and analysis of physical properties]

[0225] Experimental Example 2

[0226] After preparing rubber compositions and rubber specimens using the butadiene polymers prepared in Examples and the butadiene polymers prepared in Comparative Examples, tensile strength, 300% modulus, elongation, and viscoelastic properties were measured by the following methods, respectively. The results are shown in Table 3 below.

[0227] Specifically, 70 parts by weight of carbon black, 22.5 parts by weight of processing oil, 2 parts by weight of anti-aging agent (TMDQ), 3 parts by weight of zinc oxide (ZnO) and 2 parts by weight of stearic acid were mixed with 100 parts by weight of each polymer to prepare each rubber composition. Afterwards, 2 parts by weight of sulfur, 2 parts by weight of vulcanization accelerator (CZ) and 0.5 parts by weight of vulcanization accelerator (DPG) were added to each rubber composition and gently mixed at 50 rpm for 1.5 minutes at 50°C, and then, a sheet-like vulcanized mixture compound was obtained using a 50°C roller. The vulcanized mixture compound was vulcanized at 160°C for 25 minutes to prepare a rubber specimen.

[0228] (1) Tensile properties

[0229] After each rubber composition was vulcanized at 150° C. for 90 minutes, the tensile strength (kg·f / cm 2 ), modulus at 300% elongation (300% modulus, M-300%, kg·f / cm 2 ) and elongation at break.

[0230] (2) Viscoelastic properties (Tanδ value at 60℃)

[0231] Tan δ performance, which is an important factor for low fuel consumption performance, was measured using DMTS 500N from Gabo Co., Germany, at a frequency of 10 Hz, a pre-strain of 3%, and a dynamic strain of 3%, and the viscoelastic coefficient (Tan δ) at 60° C. was measured. In this case, as the Tan δ value at 60° C. increases, the hysteresis loss decreases, and the rotational resistance is excellent, that is, the fuel consumption performance is excellent.

[0232] [Table 3]

[0233]

[0234] The index value of the tensile property was calculated by the following mathematical formula 1, and the value of Comparative Example 1 was taken as 100. The index value of the viscoelastic property was calculated by the following mathematical formula 2, and the value of Comparative Example 1 was taken as 100.

[0235] [Mathematical formula 1]

[0236] Indication = (measured value / standard value) x 100

[0237] [Mathematical formula 2]

[0238] Indication = (standard value / measured value) x 100

[0239] As shown in Table 3, it was confirmed that if the modified conjugated diene-based polymer prepared by the preparation method of the present invention was processed into a rubber sample, excellent tensile properties and viscoelastic properties were exhibited.

[0240] Specifically, Example 2, Example 4 and Example 5 used the catalyst compositions of Preparation Examples 1 to 3, respectively, Comparative Example 3 used the catalyst composition of Comparative Preparation Example 1, and Comparative Example 5 used the catalyst composition of Comparative Preparation Example 2, and used the same polymerization temperature of 50° C. As a result, all of Example 2, Example 4 and Example 5 showed improved tensile properties and viscoelastic properties compared to Comparative Example 3 or Comparative Example 5. It can be found that, although the polymerization temperature is included in the range of the present invention, if the molar ratio of the neodymium compound and the second alkylating agent of the catalyst composition deviates from the range of the present invention, the mixing performance of the modified conjugated diene polymer deteriorates.

[0241] In addition, Examples 1 to 3 and Comparative Example 6 used the catalyst composition of Preparation Example 1, Examples 4 and Comparative Example 7 used the catalyst composition of Preparation Example 2, and Examples 5 and Comparative Example 8 used the catalyst composition of Preparation Example 3. However, with respect to the polymerization temperature, Examples 1 to 5 were polymerized at a temperature of 40° C., 50° C., or 60° C. included in the range of the present invention (30° C. to 65° C.), and Comparative Examples 6 to 8 were polymerized at 70° C., which is higher than the range of the present invention. In this case, all of Examples 1 to 5 showed significantly improved tensile properties and viscoelastic properties compared to Comparative Examples 6 to 8. In particular, if the Examples and Comparative Examples using the same catalyst composition are compared, it can be clearly confirmed that, although the catalyst composition satisfies the molar ratio of the neodymium compound and the second alkylating agent defined in the present invention, if the polymerization temperature deviates from 30° C. to 65° C., physical properties deteriorate.

[0242] As described above, if a catalyst composition having a molar ratio of the neodymium compound to the second alkylating agent of 1:20 to 1:35 is used and polymerization is performed at a temperature of 30° C. to 65° C. according to the preparation method of the present invention, a modified conjugated diene polymer having a high modification rate and excellent mixing performance can be prepared.

Claims

1. A method for preparing a modified conjugated diene polymer, the method comprising: In a hydrocarbon solvent, polymerizing a conjugated diene monomer in the presence of a catalyst composition comprising a neodymium compound, a first alkylating agent, a second alkylating agent, and a halide to prepare a living polymer; and reacting or coupling the living polymer with a modifying agent, wherein the molar ratio of the neodymium compound to the second alkylating agent is 1:20 to 1:35, and The polymerization was carried out at a temperature of 40°C. Wherein, the modifier is 1-(trimethylsilyl)piperidine-4-carboxylic acid ethyl ester, Wherein, the first alkylating agent is aluminoxane, and Wherein, the second alkylating agent is dialkylaluminum hydride or alkylaluminum dihydride.

2. The method for preparing a modified conjugated diene polymer according to claim 1, wherein: The polymerization is carried out for 15 minutes to 3 hours.

3. The method for preparing the modified conjugated diene polymer according to claim 1, further comprising: Prior to preparing the living polymer, the neodymium compound, the first alkylating agent, the second alkylating agent and the halide are mixed at -30 to -20°C and the resulting mixture is allowed to stand at -30 to -20°C for 24 to 36 hours to prepare the catalyst composition.

4. The method for preparing a modified conjugated diene polymer according to claim 1, wherein: The neodymium compound, the first alkylating agent, the second alkylating agent, and the halide contained in the catalyst composition have a molar ratio of 1:(50 to 200):(20 to 35):(2 to 5).

5. The method for preparing a modified conjugated diene polymer according to claim 1, wherein: The neodymium compound is present in an amount of 0.01 mmol to 0.50 mmol based on 100 g of the conjugated diene-based monomer.

6. The method for preparing a modified conjugated diene polymer according to claim 1, wherein: The neodymium compound is a compound represented by the following formula 1: [Formula 1] In formula 1, R a To R c are each independently hydrogen or an alkyl group of 1 to 12 carbon atoms, Among them, R a To R c Not at the same time hydrogen.

7. The method for preparing a modified conjugated diene polymer according to claim 6, wherein: R a is an alkyl group of 4 to 12 carbon atoms, and R b and R c Each is independently hydrogen or an alkyl group of 1 to 8 carbon atoms.

8. The method for preparing a modified conjugated diene polymer according to claim 1, wherein: The neodymium compound is selected from Nd(neodecanoic acid)3, Nd(2-ethylhexanoic acid)3, Nd(2,2-dimethyldecanoic acid)3, Nd(2,2-diethyldecanoic acid)3, Nd(2,2-dipropyldecanoic acid)3, Nd(2,2-dibutyldecanoic acid)3, Nd(2,2-dihexyldecanoic acid)3, Nd(2,2-dioctyldecanoic acid)3, Nd(2-ethyl-2-propyldecanoic acid)3, Nd(2-ethyl-2-butyldecanoic acid)3, Nd(2-ethyl-2-hexyldecanoic acid)3, Nd(2-propyl-2-butyldecanoic acid)3, Nd(2-propyl-2-hexyldecanoic acid)3, Nd(2-propyl-2-isopropyldecanoic acid)3, Nd( One or more of Nd(2-butyl-2-hexyldecanoic acid)3, Nd(2-hexyl-2-octyldecanoic acid)3, Nd(2,2-diethyl-octanoic acid)3, Nd(2,2-dipropyloctanoic acid)3, Nd(2,2-dibutyloctanoic acid)3, Nd(2,2-dihexyloctanoic acid)3, Nd(2-ethyl-2-propyloctanoic acid)3, Nd(2-ethyl-2-hexyloctanoic acid)3, Nd(2,2-diethylnonanoic acid)3, Nd(2,2-dipropylnonanoic acid)3, Nd(2,2-dibutylnonanoic acid)3, Nd(2,2-dihexylnonanoic acid)3, Nd(2-ethyl-2-propylnonanoic acid)3 and Nd(2-ethyl-2-hexylnonanoic acid)3.

9. The method for preparing a modified conjugated diene polymer according to claim 1, wherein: The first alkylating agent is 60 mol to 150 mol based on 1 mol of the neodymium compound.

10. The method for preparing a modified conjugated diene polymer according to claim 1, wherein: The first alkylating agent is one or more selected from methylaluminoxane, modified methylaluminoxane, ethylaluminoxane, n-propylaluminoxane, isopropylaluminoxane, butylaluminoxane, isobutylaluminoxane, n-pentylaluminoxane, neopentylaluminoxane, n-hexylaluminoxane, n-octylaluminoxane, 2-ethylhexylaluminoxane, cyclohexylaluminoxane, 1-methylcyclopentylaluminoxane, phenylaluminoxane and 2,6-dimethylphenylaluminoxane.

11. The method for preparing a modified conjugated diene polymer according to claim 1, wherein: The first alkylating agent is methylaluminoxane, modified methylaluminoxane or a mixture thereof.

12. The method for preparing a modified conjugated diene polymer according to claim 1, wherein: The second alkylating agent is selected from diethylaluminum hydride, di-n-propylaluminum hydride, diisopropylaluminum hydride, di-n-butylaluminum hydride, diisobutylaluminum hydride, di-n-octylaluminum hydride, diphenylaluminum hydride, di-p-tolylaluminum hydride, dibenzylaluminum hydride, phenylethylaluminum hydride, phenyl-n-propylaluminum hydride, phenylisopropylaluminum hydride, phenyl-n-butylaluminum hydride, phenylisobutylaluminum hydride, phenyl-n-octylaluminum hydride, p-tolylethylaluminum hydride, p-tolyl-n-propylaluminum hydride The invention can be selected from the group consisting of aluminum, p-tolyl isopropyl aluminum hydride, p-tolyl n-butyl aluminum hydride, p-tolyl isobutyl aluminum hydride, p-tolyl n-octyl aluminum hydride, benzyl ethyl aluminum hydride, benzyl n-propyl aluminum hydride, benzyl isopropyl aluminum hydride, benzyl n-butyl aluminum hydride, benzyl isobutyl aluminum hydride, benzyl n-octyl aluminum hydride, ethyl aluminum hydride, n-propyl aluminum hydride, isopropyl aluminum hydride, n-butyl aluminum hydride, isobutyl aluminum hydride and n-octyl aluminum hydride.

13. The method for preparing a modified conjugated diene polymer according to claim 1, wherein: The second alkylating agent is one or more selected from diethylaluminum hydride, di-n-propylaluminum hydride, diisopropylaluminum hydride, di-n-butylaluminum hydride and diisobutylaluminum hydride.

14. The method for preparing a modified conjugated diene polymer according to claim 1, wherein: The halide is included in an amount of 2.1 mol to 3.0 mol based on 1 mol of the neodymium compound.

15. The method for preparing a modified conjugated diene polymer according to claim 1, wherein: The halide is one or more selected from elemental halogen, interhalogen compound, hydrogen halide, organic halide, non-metallic halide, metal halide and organic metal halide.

16. The method for preparing a modified conjugated diene polymer according to claim 1, wherein: The halide is one or more selected from dimethylaluminum chloride, diethylaluminum chloride, methylaluminum dichloride, ethylaluminum dichloride, sesquimethylaluminum chloride, sesquiethylaluminum chloride and sesquiisobutylaluminum chloride.