A solid film stripping method based on substrate surface chemical reaction

By injecting chloride ions on the surface of the semiconductor substrate and forming a low-boiling compound, and turning it into a gaseous substance by using a laser beam or slow annealing, the high cost problem in the prior art is solved, and efficient film peeling and cost reduction are achieved.

CN114188270BActive Publication Date: 2024-11-22BEIJING UNIV OF TECH +1

Patent Information

Application Number
CN202111500772.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-09
Publication Date
2024-11-22
Estimated Expiration
2041-12-09

AI Technical Summary

Technical Problem

In the prior art, injecting H and He ions into Si substrates requires a high ion implantation concentration to achieve peeling of thin film materials, resulting in high material preparation costs and lack of ions that can react chemically with the substrate material to reduce the implantation. Concentration method.

Method used

Using solid film peeling method based on matrix surface chemical reaction, a passivation layer is prepared on the surface of the semiconductor substrate and chloride ions are injected into it to form a low-boiling compound, and a laser beam or slow annealing is used to turn it into a gaseous substance, and the expansion is applied. Force to achieve film peeling.

Benefits of technology

It reduces the ion dose required for material peeling, reduces the cost of film preparation, and improves the utilization efficiency of implanted ions, and is suitable for large-scale industrial promotion and application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114188270B_ABST
    Figure CN114188270B_ABST
Patent Text Reader

Abstract

The present invention discloses a solid film stripping method based on a substrate surface chemical reaction, comprising: preparing a layer of SiO on the surface of a silicon substrate A; 2 The invention relates to a method for preparing a passivation layer on the surface of semiconductor substrate B, and injecting ions into semiconductor substrate B from one side of the passivation layer to form an ion implantation layer on semiconductor substrate B; wherein the injected ions can form a low-boiling-point compound with the material of semiconductor substrate B; removing the passivation layer on the surface of semiconductor substrate B, and polishing silicon substrate A and semiconductor substrate B; activating the polished silicon substrate A and semiconductor substrate B, and after activation, converting SiO 2 Wafer bonding is performed on one side of the wafer substrate A and the side of the semiconductor substrate B where the passivation layer is removed; a laser beam is used to irradiate the surface of the wafer bonding pair to separate the semiconductor substrate B at the ion implantation layer; after the separation is completed, a layer of substrate B film is retained on the silicon wafer substrate A, and the substrate B film is polished to complete the solid film peeling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor thin film material preparation, and in particular to a solid thin film stripping method based on substrate surface chemical reaction. Background Art

[0002] Ion implantation technology is a high-tech method for modifying the surface of materials that is widely used internationally. Its basic principle is: when an ion beam of a certain energy is incident into the material, a series of physical and chemical interactions will occur between the ion beam and the atoms or molecules in the target material. The incident ions gradually lose energy and finally stay in the target material, causing changes in the composition, structure and properties of the material surface, thereby optimizing the surface properties of the material or obtaining some new excellent properties. Ion implantation technology has been widely used in semiconductor material doping, surface modification of metals, ceramics, polymers, etc.

[0003] Ion implantation is the process of introducing additives (in the form of ions) into the matrix material with the help of electric field force. The dopant is not limited by factors such as diffusion coefficient and chemical bonding force. In principle, all kinds of elements can be doped, and doping can be performed under three different conditions: low temperature, room temperature, and high temperature. Ion implantation does not produce lateral diffusion as serious as thermal diffusion. Generally, when processed at a lower temperature, due to the straight-forward nature of ions, the injected impurities are selectively doped nearly vertically inward according to the graphic template. This doping has a much smaller lateral diffusion than thermal diffusion. Ion implantation selects a single implanted ion through a mass analyzer, thereby ensuring that the doping concentration is not affected by the purity of the ion source.

[0004] Due to the outstanding advantages of ion implantation, it has been widely used in the manufacturing process of semiconductor materials and devices. Based on the surface delamination effect produced by light gas ion implantation of Si, Bruel et al. proposed a new technology for preparing high-performance silicon on insulating substrate (SOI) materials in 1995, which is the currently popular "smart-cut" technology. Its process flow mainly includes the following four steps: first, H ions with a certain energy and dose are implanted into the silicon wafer at room temperature, thereby generating a bubble layer at a certain depth below the silicon surface; bonding the H-injected silicon wafer with another silicon wafer, and a layer of SiO2 has been grown on the surface of the silicon wafer by thermal oxidation; then annealing is performed to crack the H-injected silicon wafer at the bubble layer; finally, the surface of the sample is polished to obtain a high-performance SOI structure. In the Smart-cut technology, H ions and He ions are injected into the Si substrate to achieve the stripping of the thin film material. In this technology, since the H and He elements do not react chemically with the substrate material, a very high implantation concentration is usually required to achieve the stripping of the material surface. Therefore, it is necessary to find an ion that can react with the substrate material and achieve the stripping of the material surface, thereby reducing the required ion implantation concentration and thus reducing the cost of thin film material preparation. Summary of the invention

[0005] In view of the above problems existing in the prior art, the present invention provides a solid film stripping method based on substrate surface chemical reaction.

[0006] The present invention discloses a solid film stripping method based on a substrate surface chemical reaction, comprising:

[0007] Step 1, preparing a SiO2 layer on the surface of silicon substrate A;

[0008] Step 2: prepare a passivation layer on the surface of semiconductor substrate B, and inject ions into the semiconductor substrate B from one side of the passivation layer to form an ion implantation layer on the semiconductor substrate B; wherein the implanted ions meet at least one of the following requirements: damage the crystal lattice inside the semiconductor substrate B material, and / or form a low-boiling-point compound with the semiconductor substrate B material;

[0009] Step 3, removing the passivation layer on the surface of the semiconductor substrate B, and polishing the silicon substrate A and the semiconductor substrate B;

[0010] Step 4, activating the polished silicon substrate A and the semiconductor substrate B, and after activation, performing wafer bonding on the SiO2 layer side of the silicon substrate A and the side of the semiconductor substrate B where the passivation layer is removed;

[0011] Step 5: irradiating the surface of the wafer bonding pair with a laser beam to separate the semiconductor substrate B at the ion implantation layer;

[0012] Step 6: After separation, a layer of substrate B film is retained on the silicon wafer substrate A, and the substrate B film is polished to complete the solid film peeling.

[0013] As a further improvement of the present invention, in step 2, the material of the semiconductor substrate B includes one of silicon, gallium arsenide, germanium and gallium nitride, and the implanted ions are chloride ions.

[0014] As a further improvement of the present invention, the injection energy of chloride ions is 30-700 keV, and the injection dose is 1×10 15 ~9×10 17 / cm 2 , keep the vacuum degree in the injection chamber at 10 -2 ~10 -5 Pa.

[0015] As a further improvement of the present invention, in step 3, the surface roughness of the polished silicon substrate A and the semiconductor substrate B is less than 0.5 nm.

[0016] As a further improvement of the present invention, in step 4, argon ions, oxygen ions or nitrogen ions are used to activate the polished silicon substrate A and semiconductor substrate B, the plasma activation power is 200 to 600 W, and the activation time is 20 to 200 s.

[0017] As a further improvement of the present invention, in step 4, the vacuum degree in the bonding chamber is less than 10 -5 Pa, the applied bonding force is 5 to 100 kN, and the bonding time is 10 to 100 s.

[0018] As a further improvement of the present invention, in step 5, after the laser beam irradiation, the temperature generated in the material of the semiconductor substrate B reaches the boiling point of the low-boiling-point compound.

[0019] As a further improvement of the present invention,

[0020] When the semiconductor substrate B is a silicon wafer, the laser irradiation band used is 1000-1200nm;

[0021] When the semiconductor substrate B is a gallium arsenide wafer, the laser irradiation band used is 800-900nm;

[0022] When the semiconductor substrate B is a germanium sheet, the laser irradiation wavelength band used is 1800-1900nm;

[0023] When the semiconductor substrate B is a gallium nitride wafer, the laser irradiation wavelength band used is 300-400 nm.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention adopts the method of injecting ions into the semiconductor substrate B that "cause damage to the crystal lattice inside the semiconductor substrate B material, and / or form low-boiling point compounds with the semiconductor substrate B material". The low-boiling point compounds can be converted into gaseous substances after laser irradiation or slow annealing process, which exert expansion force on the solid material to cause the solid film to peel off. At the same time, the low-boiling point compounds do not require very high annealing temperature, which can improve the utilization efficiency of the injected ions, greatly reduce the ion dose required for material peeling, reduce the cost of film preparation, and facilitate large-scale industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A flow chart of a solid film stripping method based on a substrate surface chemical reaction disclosed in an embodiment of the present invention;

[0027] Figure 2 for Figure 1 Schematic diagram of the structure after step 1;

[0028] Figure 3 for Figure 1 Schematic diagram of the structure after step 2;

[0029] Figure 4 for Figure 1 Schematic diagram of the structure after step 4;

[0030] Figure 5 for Figure 1 Schematic diagram of the structure after step 6.

[0031] In the figure:

[0032] 1. Silicon substrate A; 2. SiO2 layer; 3. Semiconductor substrate B; 4. Passivation layer; 5. Ion implantation layer; 6. Substrate B thin film. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0035] like Figure 1 As shown, the present invention provides a solid film stripping method based on substrate surface chemical reaction, comprising:

[0036] Step 1: Prepare a SiO2 layer 2 on the surface of the silicon substrate A1 to form Figure 2 The structural schematic diagram shown;

[0037] Specifically include:

[0038] A silicon wafer support substrate A is provided, and a SiO2 layer can be prepared on the surface of the substrate A by thermal oxidation or plasma enhanced chemical vapor deposition (PECVD). The thermal oxidation process adopts a wet oxidation method to prepare the SiO2 layer, with a nitrogen flow rate of 5 to 10 sccm, an oxygen flow rate of 100 to 150 sccm, a water bath temperature of 90 to 110°C, an oxidation time of 2 to 5 hours, and an oxidation temperature of 900 to 1100°C. The process parameters for preparing the SiO2 layer by PECVD are SiH4 flow rate of 40 to 50 sccm, N2O flow rate of 350 to 400 sccm, N2 flow rate of 750 to 800 sccm, gas pressure of 500 to 600 mTorr, time of 1 to 5 minutes, and power of 30 to 300 W.

[0039] Step 2: prepare a passivation layer 4 on the surface of the semiconductor substrate B3, and inject ions into the semiconductor substrate B from one side of the passivation layer to form an ion implantation layer 5 on the semiconductor substrate B. Figure 3 The structural schematic diagram shown;

[0040] The implanted ions meet at least one of the following requirements: damage the lattice inside the semiconductor substrate B material, and / or form a low-boiling-point compound with the semiconductor substrate B material; preferably, the material of the semiconductor substrate B includes one of silicon, gallium arsenide, germanium and gallium nitride, and the implanted ions are chloride ions;

[0041] Specifically include:

[0042] A layer of SiO2 is deposited on substrate B or a layer of photoresist is coated to prevent the surface of substrate B from being damaged by ion bombardment. Then, ions are implanted into substrate B. The implanted ions are chloride ions with an implantation energy of 30 to 700 keV. The vacuum degree in the implantation chamber is maintained at 10 -2 ~10 -5 Pa, the injection dose is 1×10 15 ~9×10 17 / cm 2 ; A chloride ion enrichment layer will be formed at the injection depth. The injection of chloride ions will damage the lattice inside the substrate B material, destroy the chemical bonds, and reduce the lattice strength;

[0043] Among them, silicon material can react chemically with injected chloride ions to generate silicon chloride, and the boiling point of silicon chloride material is 57.6°C; gallium arsenide material can react chemically with injected chloride ions to generate gallium chloride and arsenic chloride, wherein the boiling point of gallium chloride material is 201.3°C, and the boiling point of arsenic chloride material is 130.2°C; germanium material can react chemically with injected chloride ions to generate germanium chloride, and the boiling point of germanium chloride material is 82°C to 84°C; gallium nitride material can react chemically with injected chloride ions to generate gallium chloride, and nitrogen ions do not react chemically with chloride ions, but generate nitrogen gas, and the boiling point of gallium chloride material is 201.3°C.

[0044] Step 3, removing the passivation layer on the surface of the semiconductor substrate B, and polishing the silicon substrate A and the semiconductor substrate B;

[0045] Specifically include:

[0046] After the injection of substrate B is completed, the SiO2 layer or photoresist protective layer on the surface of substrate B is removed; after the removal is completed, the substrate B is cleaned with ethanol and acetone; after the cleaning is completed, the silicon wafer substrate A and the semiconductor substrate B are respectively subjected to chemical mechanical polishing (CMP), and the abrasive particles can be selected from silicon dioxide (SiO2), aluminum oxide (Al2O3), cerium oxide (CeO2) and diamond, etc. The diameter of the abrasive particles can be 10-200nm, the polishing pressure is set to 20-200kPa, the average speed of the workbench is 30-100r / min, and the polishing time is 20-200s. Finally, the surface roughness of substrate A and substrate B is less than 0.5nm.

[0047] Step 4: Activate the polished silicon substrate A and the semiconductor substrate B. After activation, bond the SiO2 layer side of the silicon substrate A and the side of the semiconductor substrate B where the passivation layer is removed to form a wafer. Figure 4 The structural schematic diagram shown;

[0048] Specifically include:

[0049] After polishing of substrate A and substrate B, the surfaces of substrate A and substrate B are activated by argon ions, oxygen ions or nitrogen ions. The plasma activation power is set to 200-600W and the activation time is 20-200s. The two substrates are placed in a wafer bonding machine, and substrate B is bonded to silicon wafer substrate A. The vacuum degree in the bonding chamber is less than 10 -5 Pa, the applied bonding force is 5 to 100 kN, and the bonding time is 10 to 100 s; after bonding is completed, the bonded pair is taken out from the wafer bonding machine for backup.

[0050] Step 5: irradiating the surface of the wafer bonding pair with a laser beam or heating the surface of the wafer bonding pair with a quartz tube slow annealing method, so that the semiconductor substrate B is separated at the ion implantation layer; wherein the temperature generated in the semiconductor substrate B material reaches the boiling point of the low-boiling-point compound;

[0051] Specifically include:

[0052] The bonded wafer pair is placed on a base, and the surface of the wafer pair is irradiated with a laser beam or heated by a quartz tube slow annealing method, so that heat is generated inside the wafer; the heat generated by the laser beam inside the material can be adjusted by adjusting the output power of the laser beam; the power range of the laser output is 0.5 to 30W, the temperature range generated in the substrate material is 60 to 250°C, and the irradiation time is 1 to 10 hours; after the wafer pair is heated, the chloride material generated by the chemical reaction at the injection depth will reach the boiling point, generate gaseous substances, and combine with unreacted chlorine to form bubbles; the formed bubbles will be laterally connected at the injection depth, and jointly exert an expansion force on the upper material of the semiconductor substrate B, so that the substrate B material is separated; the remaining substrate B material can be recycled and reused;

[0053] Among them, when the semiconductor substrate B is a silicon wafer, the laser irradiation band used is 1000-1200nm; when the semiconductor substrate B is a gallium arsenide wafer, the laser irradiation band used is 800-900nm; when the semiconductor substrate B is a germanium wafer, the laser irradiation band used is 1800-1900nm; when the semiconductor substrate B is a gallium nitride wafer, the laser irradiation band used is 300-400nm.

[0054] Step 6: After separation, a layer of substrate B film 6 is retained on the silicon wafer substrate A, and the substrate B film is polished to complete the solid film peeling to form a Figure 5 The structural schematic diagram shown;

[0055] Specifically include:

[0056] After the substrate B material is split, a thin film will remain on the silicon wafer substrate A. The top substrate B film is polished using the CMP process so that its surface roughness can reach the wafer level standard, and finally the thin film peeling of the solid material B is completed.

[0057] The principle of the above-mentioned stripping method of the present invention is:

[0058] The present invention mainly injects chloride ions, and the injected chloride ions can collide with the substrate material lattice and stay in an enriched layer at a certain depth; in addition, the chloride ions in the enriched layer can react locally with the substrate material to generate new substances, and the boiling point of the new substances is usually low; after the subsequent annealing process, the boiling point of the substances can be reached, so that the surface of the material is peeled off; in addition, the chloride ions that do not react chemically with the material can be laterally aggregated in the enriched layer to generate chlorine bubbles; after the subsequent annealing process, the chlorine bubbles can be laterally connected, and finally the material is peeled off.

[0059] Example 1

[0060] The present invention provides a solid film stripping method based on a substrate surface chemical reaction, comprising:

[0061] Step 1: Provide a silicon wafer support substrate A, and prepare a SiO2 layer on the surface of substrate A by thermal oxidation or plasma enhanced chemical vapor deposition (PECVD). The thermal oxidation process uses a wet oxidation method to prepare the SiO2 layer, with a nitrogen flow rate of 5 sccm, an oxygen flow rate of 100 sccm, a water bath temperature of 100°C, an oxidation time of 4 hours, and an oxidation temperature of 1000°C to form a SiO2 layer of about 400nm thick;

[0062] Step 2: Provide another silicon wafer substrate B. First, deposit a SiO2 layer with a thickness of about 20 nm on the silicon wafer B to prevent the surface of the silicon wafer B from being damaged by ion bombardment. Then, ion implantation is performed into the silicon wafer B. The ions implanted are chloride ions with an implantation energy of 300 keV. The vacuum degree in the implantation chamber is maintained at 10 -5 Pa, the injection dose is 1×10 16 / cm 2 A chloride ion-rich layer will be formed at the injection depth. The injection of chloride ions will damage the crystal lattice inside the silicon wafer B material, destroy the chemical bonds, and the chloride ions will react with the impacted silicon atoms to form silicon chloride;

[0063] Step 3: After the injection of substrate B is completed, the SiO2 layer on the surface of substrate B is removed. After removal, substrate B is cleaned with ethanol and acetone. After cleaning, chemical mechanical polishing (CMP) is performed on silicon wafer substrate A and semiconductor substrate B respectively, and silicon dioxide (SiO2) can be used as abrasive particles. The diameter of the abrasive particles can be 80nm, the polishing pressure is set to 80kPa, the average speed of the workbench is 60r / min, and the polishing time is 60s. Finally, the surface roughness of substrate A and substrate B is less than 0.5nm;

[0064] Step 4: After polishing of substrate A and substrate B, the surfaces of substrate A and substrate B are activated by argon ions. The plasma activation power is set to 300W and the activation time is 60s. Then the two substrates are placed in a wafer bonding machine, and substrate B is bonded to silicon wafer substrate A. The vacuum degree in the bonding chamber is less than 10 -5 Pa, the bonding force applied is 10 kN, and the bonding time is 60 s. After bonding is completed, the wafer bonding pair is taken out from the wafer bonding machine for backup;

[0065] Step 5: Place the bonded wafer pair on the base, and use the laser beam to irradiate the surface of the wafer pair to generate heat inside the wafer. The heat generated by the laser beam inside the material can be adjusted by adjusting the output power of the laser beam. The power range of the laser output is 10W, the temperature generated in the substrate material is 100°C, and the irradiation time is 5h. After the wafer pair is heated, the chloride material generated by the chemical reaction at the injection depth will reach the boiling point and generate gaseous substances, which will combine with the unreacted chlorine to form bubbles. The bubbles formed will be laterally connected at the injection depth, and together exert an expansion force on the upper material of the semiconductor substrate B, causing the substrate B material to separate. The remaining substrate B material can be recycled and reused;

[0066] Step 6: After the substrate B material is split, a thin film will remain on the silicon wafer substrate A. The top substrate B film is polished using the CMP process to make its surface roughness reach the wafer level standard. Finally, the film peeling of the solid material B is completed;

[0067] Embodiment 2:

[0068] The present invention provides a solid film stripping method based on substrate surface chemical reaction, which is mainly different from Example 1 in that substrate B is gallium arsenide material, and annealing is performed in a quartz tube annealing furnace in step 5; the method comprises:

[0069] Step 1: Provide a silicon wafer support substrate A, and prepare a SiO2 layer on the surface of substrate A by thermal oxidation or plasma enhanced chemical vapor deposition (PECVD). The thermal oxidation process uses a wet oxidation method to prepare the SiO2 layer, with a nitrogen flow rate of 5 sccm, an oxygen flow rate of 120 sccm, a water bath temperature of 100°C, an oxidation time of 4.5h, and an oxidation temperature of 1000°C to form a SiO2 layer of about 500nm thick;

[0070] Step 2: Provide another GaAs substrate B. First, deposit a SiO2 layer with a thickness of about 20 nm on the GaAs substrate B to prevent the surface of the GaAs substrate B from being damaged by ion bombardment. Then, perform ion implantation into the GaAs substrate B. The ions implanted are chloride ions with an implantation energy of 200 keV. Maintain the vacuum degree in the implantation chamber at 10-5 Pa, the injection dose is 1×10 16 / cm 2 A chloride ion enrichment layer will be formed at the injection depth. The injection of chloride ions will damage the lattice inside the gallium arsenide substrate B material, destroy the chemical bonds, and the chloride ions will react with the impacted gallium atoms and arsenic atoms to generate gallium chloride and arsenic chloride;

[0071] Step 3: After the injection of gallium arsenide substrate B is completed, the SiO2 layer on the surface of gallium arsenide substrate B is removed. After removal, gallium arsenide substrate B is cleaned with ethanol and acetone. After cleaning, chemical mechanical polishing (CMP) is performed on silicon wafer substrate A and gallium arsenide substrate B respectively, and silicon dioxide (SiO2) can be used as abrasive particles. The diameter of the abrasive particles can be 70nm, the polishing pressure is set to 80kPa, the average speed of the workbench is 60r / min, and the polishing time is 60s. Finally, the surface roughness of substrate A and gallium arsenide substrate B is less than 0.5nm;

[0072] Step 4: After polishing of substrate A and GaAs substrate B, use argon ions to activate the surfaces of substrate A and substrate B. The plasma activation power is set to 300W and the activation time is 60s. Then the two substrates are placed in a wafer bonding machine, and substrate B is bonded to silicon wafer substrate A. The vacuum degree in the bonding chamber is less than 10 -5 Pa, the bonding force applied is 10 kN, and the bonding time is 60 s. After bonding is completed, the wafer bonding pair is taken out from the wafer bonding machine for backup;

[0073] Step 5: Place the bonded wafer pair in a quartz furnace tube with a nitrogen flow rate of 5 sccm, a heating temperature range of 250°C, and a heating time of 5 hours. After the wafer pair is heated, the chloride material generated by the chemical reaction at the injection depth will reach a boiling point, generating gaseous substances that combine with unreacted chlorine to form bubbles. The bubbles formed will be laterally connected at the injection depth, and together exert an expansion force on the upper material of the gallium arsenide substrate B, causing the substrate B material to separate. The remaining substrate B material can be recycled and reused;

[0074] Step 6: After the substrate B material is split, a thin film will remain on the silicon wafer substrate A. The top substrate B film is polished using the CMP process to make its surface roughness reach the wafer level standard, and finally the thin film peeling of the solid material B is completed.

[0075] Embodiment 3:

[0076] The present invention provides a solid film stripping method based on substrate surface chemical reaction, which is mainly different from Example 1 in that substrate B is a germanium sheet, and comprises:

[0077] Step 1: Provide a silicon wafer support substrate A, and prepare a SiO2 layer on the surface of substrate A by thermal oxidation or plasma enhanced chemical vapor deposition (PECVD). The thermal oxidation process uses a wet oxidation method to prepare the SiO2 layer, with a nitrogen flow rate of 5 sccm, an oxygen flow rate of 120 sccm, a water bath temperature of 100°C, an oxidation time of 4.5h, and an oxidation temperature of 1000°C to form a SiO2 layer of about 500nm thick;

[0078] Step 2: Provide another germanium substrate B. First, deposit a SiO2 layer with a thickness of about 20 nm on the germanium substrate B to prevent the surface of the germanium substrate B from being damaged by ion bombardment. Then, ion implantation is performed into the germanium substrate B. The ions implanted are chloride ions with an implantation energy of 400 keV. The vacuum degree in the implantation chamber is maintained at 10 -5 Pa, the implantation dose is 6×10 16 / cm 2 A chloride ion enrichment layer will be formed at the injection depth. The injection of chloride ions will damage the lattice inside the germanium substrate B material, destroy the chemical bonds, and the chloride ions will react with the impacted germanium atoms to form germanium chloride;

[0079] Step 3: After the germanium substrate B is injected, the SiO2 layer on the surface of the germanium substrate B is removed. After removal, the germanium substrate B is cleaned with ethanol and acetone. After cleaning, the silicon wafer substrate A and the germanium substrate B are subjected to chemical mechanical polishing (CMP) respectively, and silicon dioxide (SiO2) can be used as the abrasive particles. The diameter of the abrasive particles can be 70nm, the polishing pressure is set to 80kPa, the average speed of the workbench is 60r / min, and the polishing time is 60s. Finally, the surface roughness of substrate A and germanium substrate B is less than 0.5nm;

[0080] Step 4: After polishing of substrate A and germanium substrate B, use argon ions to activate the surfaces of substrate A and germanium substrate B. The plasma activation power is set to 300W and the activation time is 60s. Then the two substrates are placed in a wafer bonding machine, and the germanium substrate B is bonded to the silicon wafer substrate A. The vacuum degree in the bonding chamber is less than 10 -5 Pa, the bonding force applied is 10 kN, and the bonding time is 60 s. After bonding is completed, the wafer bonding pair is taken out from the wafer bonding machine for backup;

[0081] Step 5: Place the bonded wafer pair in a quartz furnace tube with a nitrogen flow rate of 5 sccm, a heating temperature range of 250°C, and a heating time of 5 hours. After the wafer pair is heated, the chloride material generated by the chemical reaction at the injection depth will reach a boiling point, generating gaseous substances that combine with unreacted chlorine to form bubbles. The bubbles formed will be laterally connected at the injection depth, and together exert an expansion force on the upper material of the germanium substrate B, causing the germanium substrate B material to separate. The remaining germanium substrate B material can be recycled and reused;

[0082] Step 6: After the substrate B material is split, a thin film will remain on the silicon wafer substrate A. The top substrate B film is polished using the CMP process to make its surface roughness reach the wafer level standard, and finally the thin film peeling of the solid material B is completed.

[0083] Embodiment 4:

[0084] The invention provides a solid film stripping method based on substrate surface chemical reaction, which is mainly different from Example 1 in that substrate B is a gallium nitride sheet, and comprises:

[0085] Step 1: Provide a silicon wafer support substrate A, and prepare a SiO2 layer on the surface of substrate A by thermal oxidation or plasma enhanced chemical vapor deposition (PECVD). The thermal oxidation process uses a wet oxidation method to prepare the SiO2 layer, with a nitrogen flow rate of 5 sccm, an oxygen flow rate of 120 sccm, a water bath temperature of 100°C, an oxidation time of 4.5h, and an oxidation temperature of 1000°C to form a SiO2 layer of about 500nm thick;

[0086] Step 2: Provide another GaN substrate B. First, deposit a SiO2 layer with a thickness of about 20 nm on the GaN substrate B to prevent the surface of the GaN substrate B from being damaged by ion bombardment. Then, ion implantation is performed into the GaN substrate B. The ions implanted are chloride ions with an implantation energy of 350 keV. The vacuum degree in the implantation chamber is maintained at 10 -5 Pa, the injection dose is 1×10 16 / cm 2 A chloride ion-rich layer will be formed at the injection depth. The injection of chloride ions will damage the lattice inside the gallium nitride substrate B material, destroy the chemical bonds, and the chloride ions will react with the impacted gallium atoms and nitrogen atoms to generate gallium chloride and nitrogen gas;

[0087] Step 3: After the injection of gallium nitride substrate B is completed, the SiO2 layer on the surface of gallium nitride substrate B is removed. After removal, gallium nitride substrate B is cleaned with ethanol and acetone. After cleaning, chemical mechanical polishing (CMP) is performed on silicon wafer substrate A and gallium nitride substrate B respectively, and silicon dioxide (SiO2) can be used as abrasive particles. The diameter of the abrasive particles can be 70nm, the polishing pressure is set to 80kPa, the average speed of the workbench is 60r / min, and the polishing time is 60s. Finally, the surface roughness of substrate A and gallium nitride substrate B is less than 0.5nm;

[0088] Step 4: After polishing of substrate A and gallium nitride substrate B, the surfaces of substrate A and substrate B are activated using argon ions. The plasma activation power is set to 300W and the activation time is 60s. The two substrates are then placed in a wafer bonding machine, and substrate B is bonded to silicon wafer substrate A. The vacuum degree in the bonding chamber is less than 10 -5 Pa, the bonding force applied is 10 kN, and the bonding time is 60 s. After bonding is completed, the wafer bonding pair is taken out from the wafer bonding machine for backup;

[0089] Step 5: Place the bonded wafer pair in a quartz furnace tube with a nitrogen flow rate of 5 sccm, a heating temperature range of 250°C, and a heating time of 5 hours. After the wafer pair is heated, the chloride material generated by the chemical reaction at the injection depth will reach a boiling point, generating gaseous substances that combine with unreacted chlorine to form bubbles. The bubbles formed will be laterally connected at the injection depth, and together exert an expansion force on the upper material of the gallium nitride substrate B, causing the substrate B material to separate. The remaining substrate B material can be recycled and reused;

[0090] Step 6: After the substrate B material is split, a thin film will remain on the silicon wafer substrate A. The top substrate B film is polished using the CMP process to make its surface roughness reach the wafer level standard, and finally the thin film peeling of the solid material B is completed.

[0091] The advantages of the present invention are:

[0092] The present invention mainly adopts the method of injecting chloride ions into solid materials, and the injected chloride ions react chemically with the substrate material to generate new substances. The new substance has a low boiling point and can be converted into a gaseous substance after laser irradiation or slow annealing process. The generated gaseous substance and the chlorine gas generated by the injection are used to jointly exert an expansion force on the solid material to cause the solid film to peel off; the difference from the traditional H and He ion injection is that the injected chloride ions can react locally with the solid material to generate new substances. The new substance has a low boiling point and does not require a very high annealing temperature, which can improve the utilization efficiency of the injected ions. The ion dose required for material peeling is greatly reduced, the cost of film preparation is reduced, and it is conducive to large-scale industrial promotion and application.

[0093] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A solid film stripping method based on substrate surface chemical reaction, characterized in that: include: Step 1, preparing a SiO2 layer on the surface of silicon substrate A; Step 2: prepare a passivation layer on the surface of semiconductor substrate B, and inject ions into the semiconductor substrate B from one side of the passivation layer to form an ion implantation layer on the semiconductor substrate B; wherein the implanted ions meet at least one of the following requirements: damage the crystal lattice inside the semiconductor substrate B material, and / or form a low-boiling point compound with the semiconductor substrate B material; wherein the material of the semiconductor substrate B includes one of silicon, gallium arsenide, germanium and gallium nitride, and the implanted ions are chloride ions; the injection energy of the chloride ions is 30 to 700 keV, and the injection dose is 1×10 15 ~9×10 17 / cm 2 , keep the vacuum degree in the injection chamber at 10 -2 ~10 -5 Pa; Step 3, removing the passivation layer on the surface of the semiconductor substrate B, and polishing the silicon substrate A and the semiconductor substrate B; Step 4, activating the polished silicon substrate A and the semiconductor substrate B, and after activation, performing wafer bonding on the SiO2 layer side of the silicon substrate A and the side of the semiconductor substrate B with the passivation layer removed; wherein argon ions, oxygen ions or nitrogen ions are used to activate the polished silicon substrate A and the semiconductor substrate B, the plasma activation power is 200 to 600 W, and the activation time is 20 to 200 s; Step 5, using a laser beam to irradiate the surface of the wafer bonding pair or using a slow annealing process to process the wafer bonding pair, so that the semiconductor substrate B is separated at the ion implantation layer; wherein the temperature generated in the semiconductor substrate B material reaches the boiling point of the low-boiling point compound; when the semiconductor substrate B is a silicon wafer, the laser irradiation band used is 1000-1200nm; when the semiconductor substrate B is a gallium arsenide wafer, the laser irradiation band used is 800-900nm; when the semiconductor substrate B is a germanium wafer, the laser irradiation band used is 1800-1900nm; when the semiconductor substrate B is a gallium nitride wafer, the laser irradiation band used is 300-400nm; Step 6: After separation, a layer of substrate B film is retained on the silicon wafer substrate A, and the substrate B film is polished to complete the solid film peeling.

2. The solid film peeling method according to claim 1, characterized in that: In step 3, the surface roughness of the polished silicon substrate A and the semiconductor substrate B is less than 0.5 nm.

3. The solid film peeling method according to claim 1, characterized in that: In step 4, the vacuum degree in the bonding chamber is less than 10 -5 Pa, the applied bonding force is 5 to 100 kN, and the bonding time is 10 to 100 s.

Citation Information

Patent Citations

  • Method for manufacturing SOI substrate

    CN101510524A

  • Silicon substrates with doped surface contacts formed from doped silicon inks and corresponding processes

    CN103460345A

  • Method for manufacturing thin film on substrate

    CN107785235A

  • Thin film transfer method

    CN110718486A

  • Annealing method, composite film and electronic component

    CN112768354A

Cited By

  • Method for removing film layer on surface of wafer by using laser effect

    CN120502848A