Catalytic cracking gasoline hydrodesulfurization catalyst and its preparation method and application

By combining SBA-15 and MCFs composite carriers with alumina, a catalyst with a stepped pore structure is prepared, and combined with cobalt salt and molybdenum salt active components, it solves the problem of sulfur and olefin content in the catalytic cracking gasoline hydrodesulfurization process in the existing technology. Reduce the problem and achieve efficient hydrodesulfurization and octane number maintenance.

CN114192182BActive Publication Date: 2024-10-29PETROCHINA CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202010983028.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-17
Publication Date
2024-10-29
Estimated Expiration
2040-09-17

AI Technical Summary

Technical Problem

During the hydrodesulfurization process of catalytically cracked gasoline, it is difficult for existing catalysts to effectively reduce sulfur content and olefin content while maintaining octane number, and the carrier material has insufficient ladder pore structure, which affects catalytic performance.

Method used

The SBA-15 and MCFs composite carrier is mixed with alumina powder, and a catalyst carrier with a stepped pore structure is prepared through crystallization and roasting of a template agent. Cobalt salt and molybdenum salt are used as active components, and modifiers and complexing agents are used. Processed to form a catalyst with high specific surface area and high stability.

Benefits of technology

It achieves high desulfurization activity and selectivity, reduces the sulfur content and olefin content in gasoline, maintains the octane number, and improves the stability and mechanical strength of the catalyst. It is suitable for hydrodesulfurization of olefin-rich gasoline.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114192182B_ABST
    Figure CN114192182B_ABST
Patent Text Reader

Abstract

The present invention discloses a catalytic cracking gasoline hydrodesulfurization catalyst and its preparation method and application. The catalyst includes a carrier and an active component; the carrier is a composite or mixture of SBA-15, MCFs and alumina; the active component is molybdenum oxide MoO3 and cobalt oxide CoO, and the content thereof is 10-20wt% and 2-5wt% respectively; the modifier is magnesium nitrate, boric acid, potassium nitrate, phosphoric acid and potassium dihydrogen phosphate, etc. In the present invention, the pore size of the catalyst carrier of 15-20nm accounts for more than 20%, the pore size of 48-53nm accounts for more than 15%, and the specific surface area is 400-600m 2 / g, pore volume is 1.0~2.0cm 3 / g, and the lateral pressure strength is greater than 120N / cm. The catalyst is suitable for the hydrodesulfurization process of catalytic gasoline with high olefin content, and has the advantages of high desulfurization activity, good selectivity, low olefin saturation and small octane number loss.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a gasoline selective hydrodesulfurization catalyst and a preparation method thereof, in particular to a catalyst for catalytic cracking gasoline (FCC gasoline) hydrodesulfurization catalyst and a preparation method and application thereof, more specifically to a catalyst for deep hydrodesulfurization of a full fraction of catalytic cracking gasoline or a heavy gasoline fraction, wherein the olefin saturation is less and the octane number loss is small during the deep desulfurization process. Background Art

[0002] In recent years, smog weather has shrouded major cities across the country, causing great harm to people's health and travel. Studies have found that motor vehicle exhaust is one of the main sources of smog weather, and sulfide in motor vehicle exhaust is one of the main pollutants. The composition of gasoline in my country is mainly FCC gasoline components, accounting for about 80%, which is characterized by insufficient high sulfur, high olefins and high octane components. Moreover, as the raw materials processed by FCC develop towards the direction of heavy quality, the sulfur content and olefin content in FCC gasoline will further increase. Therefore, FCC gasoline desulfurization, olefin reduction, and octane maintenance have become key issues that need to be solved in my country's clean gasoline production technology.

[0003] In the long-term research process of hydrodesulfurization catalysts, the research of carriers is one of the key points. For supported catalysts, the carrier has an important influence on the catalytic performance of the catalyst. The carrier not only needs to provide a large specific surface area to make full use of the active components of the catalyst and reduce economic costs, but also can improve the performance of the catalyst by interacting with the active components. For example, it can serve as the skeleton of the catalyst to improve its stability and mechanical strength, and ensure that the catalyst has a certain shape and size to meet the needs of fluid mechanics conditions in industrial reactors, reduce fluid flow resistance and many other advantages. At present, the most commonly used catalyst carriers are γ-Al2O3, activated carbon and molecular sieves. In recent years, studies have found that mesoporous materials such as SBA-15 and mesoporous silica foams (MCFs) are mixed or composited with microporous materials such as ZSM-5 and Beta as carriers. CN106433758A discloses a FCC gasoline hydrodesulfurization process, wherein the catalyst comprises a carrier and an active component; the carrier is a composite or mixture of MSU-G, SBA-15 and HMS, and the catalyst further comprises a catalyst promoter, wherein the catalyst promoter is a mixture of Cr2O3, ZrO2, CeO2, V2O5 and NbOPO4. The process can reduce the total sulfur content in FCC gasoline to below 5ppm to meet the National Five Standard for gasoline. At the same time, the process also does not significantly reduce the octane number of FCC gasoline. However, the carrier material prepared by the method is a simple mixture or composite, and a gradual step pore structure cannot be formed, and there is room for further improvement in the synthesis of carrier materials. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a catalytic cracking gasoline hydrodesulfurization catalyst. The catalyst obtained by the preparation method has high desulfurization activity and high desulfurization selectivity.

[0005] To achieve the above object, the present invention provides a method for preparing a catalytic cracking gasoline hydrodesulfurization catalyst, comprising the following steps:

[0006] Step 1: Using F127 or P123 as a template, adding a silicon source, a pore expander and deionized water in an acidic environment, crystallizing and calcining to obtain a composite carrier of SBA-15 and MCFs, kneading the composite carrier with alumina powder, extruding into strips, drying at 100-150°C for 3-6h, and calcining at 550-750°C for 3-6h to obtain a catalyst carrier;

[0007] Step 2: Modifying the catalyst support using a modifier;

[0008] Step 3: dissolve the active component in the complexing agent to prepare an active metal component complexing solution, use an equal volume of the active metal component complexing solution to impregnate the catalyst carrier, let it stand for 6-12 hours, dry at 100-150°C for 3-6 hours, and calcine at 400-600°C for 3-6 hours to obtain a catalytic cracking gasoline hydrodesulfurization catalyst.

[0009] In the preparation method of the catalytic cracking gasoline hydrodesulfurization catalyst of the present invention, preferably, the SBA-15 content in the catalyst carrier is 28-44wt%, the MCFs content is 26-44wt% and the alumina content is 6-19wt%.

[0010] In the preparation method of the catalytic cracking gasoline hydrodesulfurization catalyst of the present invention, preferably, the active components are cobalt salt and molybdenum salt, the cobalt salt is at least one of basic cobalt carbonate, cobalt nitrate, cobalt oxide and cobalt acetate, and the molybdenum salt is at least one of ammonium molybdate and molybdenum oxide.

[0011] In the preparation method of the catalytic cracking gasoline hydrodesulfurization catalyst of the present invention, preferably, the molybdenum salt is molybdenum oxide MoO3, and the cobalt salt is cobalt oxide CoO, and the contents thereof are 10-20wt% and 2-5wt% respectively.

[0012] In the preparation method of the catalytic cracking gasoline hydrodesulfurization catalyst of the present invention, preferably, the MoO3 content is 10-15wt%, and the CoO content is 2.5-3.5wt%.

[0013] In the method for preparing the catalytic cracking gasoline hydrodesulfurization catalyst of the present invention, preferably, the modifier is at least one of magnesium nitrate, boric acid, potassium nitrate, phosphoric acid and potassium dihydrogen phosphate.

[0014] In the method for preparing the catalytic cracking gasoline hydrodesulfurization catalyst of the present invention, preferably, the complexing agent is at least one of citric acid, ammonia water and phosphoric acid.

[0015] The preparation method of the catalytic cracking gasoline hydrodesulfurization catalyst of the present invention, preferably, the catalyst carrier has a pore size of 15 to 20 nm accounting for more than 20%, a pore size of 48 to 53 nm accounting for more than 15%, and a specific surface area of ​​400 to 600 m 2 / g, pore volume is 1.0~2.0cm 3 / g, lateral compression strength is greater than 120N / cm.

[0016] The preparation method of the catalytic cracking gasoline hydrodesulfurization catalyst of the present invention preferably has a catalyst specific surface area of ​​480 to 520 m 2 / g, pore volume is 1.5~1.8cm 3 / g, pore sizes of 15 to 20 nm account for more than 20%, and pore sizes of 48 to 53 nm account for more than 15%.

[0017] The method for preparing the catalytic cracking gasoline hydrodesulfurization catalyst of the present invention preferably comprises the following steps: in step 1, the acidic environment has a pH of 1 to 3, the crystallization temperature is 100 to 200° C., the crystallization time is 24 hours, the calcination temperature is 400 to 600° C., and the calcination time is 6 hours.

[0018] The preparation method of the catalytic cracking gasoline hydrodesulfurization catalyst of the present invention, preferably, the silicon source is at least one of tetraethyl orthosilicate, water glass, silica gel and sodium silicate; the pore expanding agent is at least one of hexane, cyclohexane, 1,3,5-triisopropylbenzene and mesitylene, and the added amount is 30-60wt% of the template agent.

[0019] In the preparation method of the catalytic cracking gasoline hydrodesulfurization catalyst of the present invention, preferably, the silicon source is tetraethyl orthosilicate, and the added amount is 10-50wt% of the template agent.

[0020] The present invention also provides a catalytic cracking gasoline hydrodesulfurization catalyst, which is prepared by the preparation method of the catalytic cracking gasoline hydrodesulfurization catalyst.

[0021] The present invention also provides an application of a catalytic cracking gasoline hydrodesulfurization catalyst, wherein the catalytic cracking gasoline hydrodesulfurization catalyst is used for catalytic gasoline or catalytic heavy gasoline hydrodesulfurization reaction, and the hydrodesulfurization reaction conditions are hydrogen pressure of 1.5-2.5MPa, temperature of 200-280°C, and air velocity of 2.0-4.0h -1 and hydrogen to oil ratio of 200:1-500:1.

[0022] In the application of the catalytic cracking gasoline hydrodesulfurization catalyst of the present invention, preferably, the sulfur content of the catalytic cracking gasoline or catalytic heavy gasoline is less than 1000 mg / kg, the olefin content is less than 45v%, the sulfur content of the product blending component is less than 15 mg / kg, the olefin content reduction is less than 10v%, and the octane number loss is less than 2.0.

[0023] Mesoporous molecular sieve SBA-15 has high specific surface area, good hydrothermal stability and large pore size, which is conducive to the diffusion of oil molecules in its pores; MCFs is a new type of mesoporous material with ultra-large pore size, uniform pore size distribution, large pore volume and high specific surface area. Mixing or compounding two mesoporous materials with different pore sizes and pore structures with alumina powder can change the acidity of hydrorefining catalysts, improve the dispersion of active components, and promote the reduction and sulfidation of metal components. Therefore, the preparation of mesoporous composite carriers with high specific surface area, ladder pore structure and good stability will become an important way to improve the activity of hydrorefining catalysts.

[0024] The present invention has the following advantages:

[0025] (1) In the catalytic cracking gasoline hydrodesulfurization catalyst provided by the present invention, SBA-15 is a mesoporous material with a body-centered cubic structure; MCFs is a new type of mesoporous material with ultra-large pore size, uniform pore size distribution, large pore volume, and high specific surface area. The two mesoporous materials are compounded or mixed with alumina to form a stepped pore structure, in which the pore size is 15-20 nm and accounts for more than 20%, and the pore size is 48-53 nm and accounts for more than 15%, which can achieve a synergistic improvement in the hydrorefining effect.

[0026] (2) The catalytic cracking gasoline hydrodesulfurization catalyst provided by the present invention has low metal content and high desulfurization selectivity. For olefin-rich catalytic gasoline, the olefin saturation is low and the octane number loss is small during the desulfurization process, which has a good hydrogenation and upgrading effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is a pore size distribution curve diagram of the composite carrier material of Example 1 of the present invention;

[0028] Figure 2 This is the SEM image of the composite carrier material of Example 1 of the present invention.

[0029] from Figure 1 It can be seen that the pore size of the synthesized composite carrier material presents a stepped pore structure and is relatively concentrated in distribution, with most pore sizes concentrated between 18 nm and 55 nm.

[0030] from Figure 2 It can be seen that the synthesized composite carrier material presents a spherical particle morphology with high dispersion. DETAILED DESCRIPTION

[0031] Embodiment 1:

[0032] Preparation of MCFs-SBA-15 / Al2O3 Composite Support

[0033] ① Take P123 as the template, weigh 40g of deionized water, 60g of hydrochloric acid of a certain concentration and 2g of P123 template, and stir in a water bath at 35℃ until a uniform solution is formed;

[0034] ② Weigh 30wt% of the template agent and the pore-enlarging agent mesitylene and slowly add it dropwise into solution ①, and continue stirring in a water bath;

[0035] ③ Weigh 10 wt% of tetraethyl orthosilicate (TEOS) as the template, slowly add it dropwise into solution ②, place it in a sealed environment and continue stirring in a water bath, then transfer it to a crystallization kettle and place it in a 120°C oven for crystallization for 24 hours;

[0036] ④ After the crystallization process is completed, the crystallization kettle is taken out for cooling with cooling water, and the product is filtered, washed, dried at 120°C for about 6 hours, and calcined in a muffle furnace at 550°C for 6 hours to obtain the mesoporous composite material.

[0037] 1 wt% of magnesium nitrate as a template is dissolved in deionized water to prepare a stable modification solution, and then the catalyst carrier is modified.

[0038] A total of 100 g of SBA-15-MCFs composite material and alumina were mixed in a mixing ratio of 2.1:0.4, 3 g of sesbania powder, 5 g of nitric acid, 2.5 g of citric acid, and 100 ml of deionized water were added, and the mixture was kneaded evenly. The mixture was extruded on a single-screw extruder using a blade grass perforated plate, and the mixture was left for 3 hours and then dried at 120°C for 4 hours to obtain a catalyst carrier.

[0039] Preparation of Co-Mo Co-Immersion Solution and Catalyst

[0040] The active component impregnation solution was prepared according to the equal volume impregnation method. First, 50 ml of ammonia water was weighed, and then 7.4 g of EDTA, 7.4 g of basic cobalt carbonate, and 5.6 g of ammonium molybdate were added and stirred until dissolved, and then 9.6 g of magnesium nitrate was added, and finally the volume was adjusted to 78 mL with ammonia water. The carrier was impregnated with the equal volume impregnation method to allow the catalyst carrier to fully absorb the active component impregnation solution, and then after being placed for 12 hours, the catalyst was dried at 120 ° C for 4 hours and calcined at 500 ° C for 4 hours to obtain the hydrodesulfurization catalyst sample cat-1.

[0041] Embodiment 2:

[0042] Preparation of MCFs-SBA-15 / Al2O3 Composite Support

[0043] ① Take F127 as the template, weigh 40g of deionized water, 60g of hydrochloric acid of a certain concentration and 2g of F127 template, and stir in a water bath at 35℃ until a uniform solution is formed;

[0044] ② Weigh 30wt% of the template agent and the pore-enlarging agent hexane and slowly add it dropwise into solution ①, and continue stirring in a water bath;

[0045] ③ Weigh 30wt% of water glass as the template, slowly add it dropwise into solution ②, place it in a sealed environment and continue stirring in a water bath, then transfer it to a crystallization kettle and place it in a 120℃ oven for crystallization for 24h;

[0046] ④ After the crystallization process is completed, the crystallization kettle is taken out for cooling with cooling water, and the product is filtered, washed, dried at 120°C for about 12 hours, and calcined in a muffle furnace at 550°C for 6 hours to obtain the SBA-15-MCFs composite material.

[0047] ⑤ Dissolve 3wt% of boric acid in deionized water to form a stable modified solution, and then modify the catalyst carrier. Use the equal volume impregnation method to impregnate the carrier so that the catalyst carrier fully absorbs the modifier impregnation solution, and then place it for 12 hours, dry the material at 120℃ for 4 hours, and calcine it at 500℃ for 4 hours to obtain the modified composite material.

[0048] ⑥ Mix 100 g of SBA-15-MCFs composite material and alumina in a mixing ratio of 2.1:0.4, add 3 g of sesbania powder, 5 g of nitric acid, 2.5 g of citric acid, and 100 ml of deionized water, mix evenly, extrude strips on a single-screw extruder with a blade grass perforated plate, leave it for 3 hours, and then dry it at 120°C for 4 hours to obtain a catalyst carrier.

[0049] Preparation of Co-Mo Co-Immersion Solution and Catalyst

[0050] The active component impregnation solution was prepared according to the equal volume impregnation method. First, 50 ml of ammonia water was weighed, and then 7.4 g of EDTA, 7.4 g of cobalt nitrate, and 5.6 g of molybdenum oxide were added and stirred until dissolved, and then 9.6 g of magnesium nitrate was added, and finally the volume was adjusted to 78 mL with ammonia water. The carrier was impregnated with the equal volume impregnation method to allow the catalyst carrier to fully absorb the active component impregnation solution, and then after being placed for 12 hours, the catalyst was dried at 120 ° C for 4 hours and calcined at 500 ° C for 4 hours to obtain the hydrodesulfurization catalyst sample cat-2.

[0051] Embodiment 3:

[0052] Preparation of MCFs-SBA-15 / Al2O3 Composite Support

[0053] ① Take F127 as the template, weigh 40g of deionized water, 60g of hydrochloric acid of a certain concentration and 2g of F127 template, and stir in a water bath at 35℃ until a uniform solution is formed;

[0054] ② Weigh 30wt% of the template agent and the pore-enlarging agent hexane and slowly add it dropwise into solution ①, and continue stirring in a water bath;

[0055] ③ Weigh 50wt% of sodium silicate as the template, slowly add it dropwise into solution ②, place it in a sealed environment and continue stirring in a water bath, then transfer it to a crystallization kettle and place it in a 120℃ oven for crystallization for 24h;

[0056] ④ After the crystallization process is completed, the crystallization kettle is taken out for cooling with cooling water, and the product is filtered, washed, dried at 120°C for about 12 hours, and calcined in a muffle furnace at 550°C for 6 hours to obtain the SBA-15-MCFs composite material.

[0057] ⑤ Dissolve 5wt% potassium nitrate of the composite material in deionized water to prepare a stable modified solution, and then modify the catalyst carrier. Use the equal volume impregnation method to impregnate the carrier so that the catalyst carrier fully absorbs the modifier impregnation solution, and then place it for 12 hours, dry the material at 120℃ for 4 hours, and calcine it at 500℃ for 4 hours to obtain the modified composite material.

[0058] ⑥ Mix 100 g of SBA-15-MCFs composite material and alumina in a mixing ratio of 2.1:0.4, add 3 g of sesbania powder, 5 g of nitric acid, 2.5 g of citric acid, and 100 ml of deionized water, mix evenly, extrude strips on a single-screw extruder with a blade grass perforated plate, leave it for 3 hours, and then dry it at 120°C for 4 hours to obtain a catalyst carrier.

[0059] Preparation of Co-Mo Co-Immersion Solution and Catalyst

[0060] The active component impregnation solution was prepared according to the equal volume impregnation method. First, 50 ml of ammonia water was weighed, and then 7.4 g of EDTA, 7.4 g of cobalt acetate, and 5.6 g of ammonium molybdate were added and stirred until dissolved, and then 9.6 g of magnesium nitrate was added, and finally the volume was adjusted to 78 mL with ammonia water. The carrier was impregnated with the equal volume impregnation method to allow the catalyst carrier to fully absorb the active component impregnation solution, and then after being placed for 12 hours, the catalyst was dried at 120 ° C for 4 hours and calcined at 500 ° C for 4 hours to obtain the hydrodesulfurization catalyst sample cat-3.

[0061] Embodiment 4:

[0062] Preparation of MCFs-SBA-15 composite carrier

[0063] ① Take F127 as the template, weigh 40g of deionized water, 60g of hydrochloric acid of a certain concentration and 2g of F127 template, and stir in a water bath at 35℃ until a uniform solution is formed;

[0064] ② Weigh 45wt% of the template agent and the pore-enlarging agent hexane and slowly add it dropwise into solution ①, and continue stirring in a water bath;

[0065] ③ Weigh 50wt% of sodium silicate as the template, slowly add it dropwise into solution ②, place it in a sealed environment and continue stirring in a water bath, then transfer it to a crystallization kettle and place it in a 120℃ oven for crystallization for 24h;

[0066] ④ After the crystallization process is completed, the crystallization kettle is taken out for cooling with cooling water, and the product is filtered and washed, dried at 120°C for about 12 hours, and calcined in a muffle furnace at 550°C for 6 hours to obtain the SBA-15-MCFs composite material (the ratio is controlled to be 1:1.1).

[0067] ⑤ Dissolve 5wt% potassium nitrate of the composite material in deionized water to prepare a stable modified solution, and then modify the catalyst carrier. Use the equal volume impregnation method to impregnate the carrier so that the catalyst carrier fully absorbs the modifier impregnation solution, and then place it for 12 hours, dry the material at 120℃ for 4 hours, and calcine it at 500℃ for 4 hours to obtain the modified composite material.

[0068] ⑥ Mix 100 g of SBA-15-MCFs composite material with 3 g of sesbania powder, 5 g of nitric acid, 2.5 g of citric acid and 100 ml of deionized water, extrude into strips on a single-screw extruder using a blade grass perforated plate, place for 3 hours and then dry at 120°C for 4 hours to obtain a catalyst carrier.

[0069] Preparation of Co-Mo Co-Immersion Solution and Catalyst

[0070] The active component impregnation solution was prepared according to the equal volume impregnation method. First, 50 ml of ammonia water was weighed, and then 7.4 g of EDTA, 7.4 g of cobalt acetate, and 5.6 g of ammonium molybdate were added and stirred until dissolved, and then 9.6 g of magnesium nitrate was added, and finally the volume was adjusted to 78 mL with ammonia water. The carrier was impregnated with the equal volume impregnation method to allow the catalyst carrier to fully absorb the active component impregnation solution, and then after being placed for 12 hours, the catalyst was dried at 120 ° C for 4 hours and calcined at 500 ° C for 4 hours to obtain the hydrodesulfurization catalyst sample cat-4.

[0071] Embodiment 5:

[0072] ① Take F127 as the template, weigh 40g of deionized water, 60g of hydrochloric acid of a certain concentration and 2g of F127 template, and stir in a water bath at 35℃ until a uniform solution is formed;

[0073] ② Weigh 50wt% of sodium silicate as the template, slowly add it dropwise into solution ②, place it in a sealed environment and continue stirring in a water bath, then transfer it to a crystallization kettle and place it in a 120℃ oven for crystallization for 24h;

[0074] ③ After the crystallization process is completed, the crystallization kettle is taken out for cooling with cooling water, and the product is filtered and washed, dried at 120°C for about 12 hours, and calcined in a muffle furnace at 550°C for 6 hours to obtain SBA-15.

[0075] ④ Dissolve 5wt% potassium nitrate of SBA-15 carrier material in deionized water to prepare a stable modified solution, and then modify the catalyst carrier. Use the equal volume impregnation method to impregnate the carrier so that the catalyst carrier fully absorbs the modifier impregnation solution, and then place it for 12 hours, dry the material at 120℃ for 4 hours, and calcine it at 500℃ for 4 hours to obtain the modified SBA-15.

[0076] ⑤ Mix 100g of SBA-15 and alumina in a ratio of 1:0.4, add 3g of sesbania powder, 5g of nitric acid, 2.5g of citric acid, and 100ml of deionized water, knead evenly, extrude on a single-screw extruder with a blade grass perforated plate, leave for 1-4h, and then dry at 120℃ for 4h to obtain a carrier powder.

[0077] Preparation of Co-Mo Co-Immersion Solution and Catalyst

[0078] The active component impregnation solution was prepared according to the equal volume impregnation method. First, 50 ml of ammonia water was weighed, and then 7.4 g of EDTA, 7.4 g of cobalt acetate, and 5.6 g of ammonium molybdate were added and stirred until dissolved, and then 9.6 g of magnesium nitrate was added, and finally the volume was fixed to 78 mL with ammonia water. The carrier was impregnated with the equal volume impregnation method to allow the catalyst carrier to fully absorb the active component impregnation solution, and then after being placed for 12 hours, the catalyst was dried at 120 ° C for 4 hours and calcined at 500 ° C for 4 hours to obtain the hydrodesulfurization catalyst sample cat-5.

[0079] Embodiment 6:

[0080] Preparation of MCFs carrier

[0081] ① Take F127 as the template, weigh 40g of deionized water, 60g of hydrochloric acid of a certain concentration and 2g of F127 template, and stir in a water bath at 35℃ until a uniform solution is formed;

[0082] ② Weigh 60wt% of the template agent and the pore-enlarging agent hexane and slowly add it dropwise into solution ①, and continue stirring in a water bath;

[0083] ③ Weigh 50wt% of sodium silicate as the template, slowly add it dropwise into solution ②, place it in a sealed environment and continue stirring in a water bath, then transfer it to a crystallization kettle and place it in a 120℃ oven for crystallization for 24h;

[0084] ④ After the crystallization process is completed, the crystallization kettle is taken out for cooling with cooling water, and the product is filtered and washed, dried at 120°C for about 12 hours, and calcined in a muffle furnace at 550°C for 6 hours to obtain the MCFs carrier material.

[0085] ⑤ Dissolve 5wt% potassium nitrate of the composite material in deionized water to prepare a stable modified solution, and then modify the catalyst carrier. Use the equal volume impregnation method to impregnate the carrier so that the catalyst carrier fully absorbs the modifier impregnation solution, and then place it for 12 hours, dry the material at 120℃ for 4 hours, and calcine it at 500℃ for 4 hours to obtain the modified MCFs.

[0086] ⑥ Mix 100 g of MCFs carrier material with 3 g of sesbania powder, 5 g of nitric acid, 2.5 g of citric acid, and 100 ml of deionized water, and extrude into strips using a blade grass perforated plate on a single screw extruder. After leaving for 3 hours, dry at 120°C for 4 hours to obtain a catalyst carrier.

[0087] Preparation of Co-Mo Co-Immersion Solution and Catalyst

[0088] The active component impregnation solution was prepared according to the equal volume impregnation method. First, 50 ml of ammonia water was weighed, and then 7.4 g of EDTA, 7.4 g of cobalt acetate, and 5.6 g of ammonium molybdate were added and stirred until dissolved, and then 9.6 g of magnesium nitrate was added, and finally the volume was adjusted to 78 mL with ammonia water. The carrier was impregnated with the equal volume impregnation method to allow the catalyst carrier to fully absorb the active component impregnation solution, and then after being placed for 12 hours, the catalyst was dried at 120 ° C for 4 hours and calcined at 500 ° C for 4 hours to obtain the hydrodesulfurization catalyst sample cat-6.

[0089] Embodiment 7:

[0090] The carrier SBA-15 was synthesized by the method in Example 5 without mixing with alumina, and other conditions remained unchanged to obtain a hydrodesulfurization agent sample cat-7.

[0091] Embodiment 8:

[0092] The carrier MCFs was synthesized by the method in Example 6 without mixing with alumina, and other conditions remained unchanged to obtain a hydrodesulfurization catalyst sample cat-8.

[0093] Embodiment 9:

[0094] The carrier in Example 1 was replaced with alumina while other conditions remained unchanged to prepare a hydrodesulfurization catalyst sample cat-9.

[0095] The catalytic cracking gasoline hydrodesulfurization catalyst prepared in the above embodiment has a stepped pore structure, with pores of 15 to 20 nm accounting for more than 20%, pores of 48 to 53 nm accounting for more than 15%, and a specific surface area of ​​480 to 520 m 2 / g, pore volume is 1.5~1.8cm 3 / g, can be used in FCC gasoline hydrodesulfurization process.

[0096] Catalyst evaluation process: The catalytic cracking gasoline hydrodesulfurization agent is loaded into a fixed bed reactor. First, it is pre-sulfurized. The sulfurized oil is a straight-run gasoline containing 3wt% CS2, the sulfurization pressure is 2.0MPa, the hydrogen-oil volume ratio is 300:1, and the sulfurization treatment is carried out at 230℃ for 8h, then the temperature is raised to 320℃, and then the sulfurization treatment is carried out at 320℃ for about 8h. After the sulfurization is completed, the raw oil is added for reaction. The properties of the raw oil are shown in Table 1, and the reaction conditions are shown in Table 2. The operating process conditions of each embodiment are the same (the results are shown in Tables 3 and 4).

[0097] Table 1 Properties of catalytic cracking fractions and heavy gasoline fractions

[0098]

[0099] Table 2 Operating process conditions

[0100] Process conditions Full fraction catalytic gasoline Heavy gasoline Reaction temperature (℃) 250 260 Reaction pressure (MPa) 2.0 2.0 <![CDATA[Space velocity (h -1 )]]> 3.0 3.0 Hydrogen to oil ratio (V / V) 400:1 400:1

[0101] Table 3 Example data

[0102]

[0103]

[0104] Table 4 Example data

[0105]

[0106] Table 5 Properties of Catalysts

[0107]

[0108] The results show that: under the process conditions listed in Table 2, cat-1 is used to treat full-fraction gasoline and heavy gasoline, and they are hydrodesulfurized respectively. The sulfur content of full-fraction catalytic gasoline is reduced from 731.8 mg / kg to below 20 mg / kg, and the octane number is basically not reduced. The sulfur content of heavy gasoline is reduced from 777.6 mg / kg to below 50 mg / kg, and the octane number loses about 2 units. This shows that the composite carrier material has strong adaptability to raw materials. Compared with a single mesoporous material carrier (i.e., cat-7 to cat-9), the composite carrier material catalyst provided in the present invention is more suitable for catalytic gasoline raw materials for hydro-reforming.

[0109] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims attached to the present invention.

Claims

1. A method for preparing a catalytic cracking gasoline hydrodesulfurization catalyst, characterized in that: The following steps are involved: Step 1: Using F127 or P123 as a template, a silicon source, a pore-enlarging agent, and deionized water are added in an acidic environment, crystallized at 100-200°C for 24 hours, and calcined at 400-600°C for 6 hours to obtain a composite support of SBA-15 and mesoporous silica foam material MCFs. The composite support is kneaded with alumina powder and extruded into strips, dried at 100-150°C for 3-6 hours, and calcined at 550-750°C for 3-6 hours to obtain a catalyst support; Step 2: Modifying the catalyst support using a modifier; Step 3: dissolving the active component in a complexing agent to prepare an active metal component complexing solution, using an equal volume of the active metal component complexing solution to impregnate the catalyst support, allowing it to stand for 6-12 hours, drying it at 100-150° C. for 3-6 hours, and calcining it at 400-600° C. for 3-6 hours to obtain a catalytic cracking gasoline hydrodesulfurization catalyst; Wherein, in said step 1, the acidic environment is pH 1-3; The pore-enlarging agent is at least one of hexane, cyclohexane, 1,3,5-triisopropylbenzene and mesitylene, and the amount added is 30-60wt% of the template agent; The catalytic cracking gasoline hydrodesulfurization catalyst has a stepped pore structure.

2. The method for preparing a catalytic cracking gasoline hydrodesulfurization catalyst according to claim 1, wherein: The silicon source is at least one of tetraethyl orthosilicate, silica gel and sodium silicate, and the added amount is 10-50wt% of the template.

3. The method for preparing a catalytic cracking gasoline hydrodesulfurization catalyst according to claim 1, wherein: The modifier is at least one of magnesium nitrate, boric acid, potassium nitrate, phosphoric acid and potassium dihydrogen phosphate.

4. The method for preparing a catalytic cracking gasoline hydrodesulfurization catalyst according to claim 1, wherein: The complexing agent is at least one of citric acid, ammonia water and phosphoric acid.

5. A catalytic cracking gasoline hydrodesulfurization catalyst, characterized in that: The catalyst is prepared by the preparation method of the catalytic cracking gasoline hydrodesulfurization catalyst according to any one of claims 1 to 4, wherein the pore size of 15 to 20 nm accounts for more than 20%, the pore size of 48 to 53 nm accounts for more than 15%, and the specific surface area is 480 to 520 m 2 / g, pore volume of 1.5~1.8 cm 3 / g.

6. The catalytic cracking gasoline hydrodesulfurization catalyst according to claim 5, characterized in that: The composite carrier of the catalyst has an SBA-15 content of 28-44 wt %, an MCFs content of 26-44 wt % and an alumina content of 6-19 wt %.

7. The catalytic cracking gasoline hydrodesulfurization catalyst according to claim 5, characterized in that: The specific surface area of ​​the composite support of the catalyst is 400-600 m 2 / g, pore volume is 1.0~2.0cm 3 / g, pore sizes of 15-20 nm account for more than 20%, and pore sizes of 48-53 nm account for more than 15%.

8. The catalytic cracking gasoline hydrodesulfurization catalyst according to claim 5, characterized in that: The active components are cobalt salt and molybdenum salt, the cobalt salt is at least one of basic cobalt carbonate, cobalt nitrate, cobalt oxide and cobalt acetate, and the molybdenum salt is at least one of ammonium molybdate and molybdenum oxide.

9. An application of a catalytic cracking gasoline hydrodesulfurization catalyst, characterized in that: The catalytic cracking gasoline hydrodesulfurization catalyst according to any one of claims 5 to 8 is used for the hydrodesulfurization reaction of catalytic cracking gasoline or catalytic cracking heavy gasoline, wherein the catalytic cracking heavy gasoline is obtained by cutting the catalytic cracking gasoline according to a cutting ratio of 3:7 and the cutting temperature is 52° C. The hydrodesulfurization reaction conditions are a hydrogen pressure of 1.5-2.5 MPa, a temperature of 200-280° C., and a space velocity of 2.0-4.0 h -1 and hydrogen to oil ratio of 200:1-500:

1.

10. Use of the catalytic cracking gasoline hydrodesulfurization catalyst according to claim 9, characterized in that: The sulfur content of the catalytic cracking gasoline or catalytic cracking heavy gasoline is less than 1000 mg / kg, and the olefin content is less than 45% by volume.

Citation Information

Patent Citations

  • HDS (hydrodesulfurization) technology of FCC (fluid catalytic cracking) gasoline

    CN106433758A

  • RFCC high octane gasoline additive and preparation method thereof

    CN102049290A

  • Preparing method of FCC gasoline desulfurization-hydrogenation upgrading catalyst

    CN108465484A