A graphene composite bulletproof plate and preparation method thereof
Through the design of graphene composite bulletproof board, the graphene bulletproof ceramic layer and multi-layer structure are used, combined with the hot melt adhesive film layer and the hot pressing process, the existing bulletproof armor has been solved, and the problem of insufficient protection capabilities and excessive quality has been achieved. High protection effect based on lightweight can effectively resist attacks of 7.62mm API.
Patent Information
- Application Number
- CN202111391565.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-11-23
AI Technical Summary
Existing bulletproof armor lacks protection capabilities when facing anti-tank shells, missiles and rockets, and at the same time, due to excessive mass, the maneuverability is degraded, making it difficult to find a balance between lightweight and high protection.
The design of graphene composite bulletproof board is adopted, including crack-resistance layer, graphene bulletproof ceramic layer, first transition layer, second transition layer and back plate. The bulletproof structure is optimized through hot melt adhesive film layer, and the laying heat is used. Prepared by pressing process and phased heating and vacuum process, the amount of graphene powder added to the bulletproof ceramic layer is 0.5-1%, and the surface density is controlled at 40-45kg/m2.
It has achieved improved protection capabilities on the basis of lightweight, can effectively resist the impact of 3 7.62mm APIs, and the surface density is within the range of 40-45kg/m2, providing a stable protection effect.
Smart Images

Figure CN114216372B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of military (police) equipment, and in particular relates to a graphene composite bulletproof plate and a preparation method thereof. Background Art
[0002] In modern warfare, the protection of vehicles is extremely important. In the First World War, protective armor was mainly made of metal materials. Such as steel armor, aluminum alloy armor, also known as homogeneous armor. Among them, metal materials have great advantages in bulletproof performance, processability and cost, but excessive mass will greatly reduce the mobility of vehicles and combatants equipped with metal armor, and lose their original combat effectiveness. At the same time, as the penetration power of anti-tank shells, missiles and rockets continues to increase, homogeneous armor can no longer withstand the attacks of these weapons.
[0003] With the development of science and technology, bulletproof armor has undergone many upgrades, from hard metal to ceramic materials, to high-performance composite fiber materials, from simple synthetic materials to composite systems of multiple materials. The development of bulletproof armor can be simply summarized into three stages: steel plate armor plate - ceramic armor plate - high-performance fiber-reinforced resin-based composite armor plate, gradually developing in the direction of lightweight. For this reason, all countries have begun to reduce the weight of bulletproof armor. How to improve the protective ability of armor through structural design under the premise of lightweight is the top priority of technical personnel in this field.
[0004] At present, ultra-high molecular weight polyethylene fiber is the fiber with the highest specific strength, and its specific modulus is second only to carbon fiber. Patent application with application number 201911175070.X - "A method for preparing a PE bulletproof plate" discloses a method for preparing a pure PE bulletproof plate. Patent application with application number 201620566289.8 - "A composite structure of a PE bulletproof plate" discloses a composite structure of a PE bulletproof plate. In the above two patent applications, the bulletproof plates are made of a single material, namely ultra-high molecular weight polyethylene fiber.
[0005] Aramid bulletproof composite laminates have the characteristics of high strength, high toughness, high limiting oxygen index, and not easy to melt, but their density and price are much higher than those of ultra-high molecular weight polyethylene fibers. Patent application with application number 201920053656.8 - "Composite bulletproof panels, bulletproof vehicles" proposed composite bulletproof panels and bulletproof vehicles. The composite bulletproof panel includes: a panel formed of a ceramic material, arranged on the lower surface of the first adhesive layer and formed of foamed aluminum, and the outer surface of the energy-absorbing layer is coated with aramid fiber; a second adhesive layer, arranged on the lower surface of the energy-absorbing layer; a back plate, arranged on the lower surface of the second adhesive layer and formed of a high-strength steel plate: an outer shell, which completely covers the upper surface of the panel and the lower surface of the back plate, and the outer shell is formed of polyurea. However, the surface density of the composite bulletproof plate is 60-70kg / cm 2, the surface density is higher. Summary of the invention
[0006] In view of this, the present invention aims to overcome the defects in the prior art and proposes a graphene composite bulletproof plate and a preparation method thereof.
[0007] To achieve the above object, the technical solution created by the present invention is implemented as follows:
[0008] A graphene composite bulletproof plate comprises a crack arresting layer, a graphene bulletproof ceramic layer, a first transition layer, a second transition layer and a back plate arranged in sequence on a bullet-facing surface, and two adjacent layers are bonded by a hot-melt adhesive film layer, wherein the material of the graphene bulletproof ceramic layer is one or more of Al2O3 bulletproof ceramic, SiC bulletproof ceramic and B4C bulletproof ceramic added with graphene powder, and the addition amount of the graphene powder is 0.5-1% of the total weight of the layer.
[0009] Preferably, the first transition layer is made of a carbon fiber plate with a thickness of 0.3-2 mm.
[0010] Preferably, the carbon fiber plate is formed by laminating and hot-pressing 2-6 layers of carbon fiber prepreg.
[0011] Preferably, the second transition layer is made of aramid UD board with a thickness of 0.3-4 mm.
[0012] Preferably, the aramid UD board is formed by laminating and hot-pressing 2 to 6 layers of aramid UD cloth.
[0013] Preferably, the crack-stop layer is an aramid woven fabric layer with a thickness of 0.3-3 mm.
[0014] Preferably, the thickness of the hot melt adhesive film layer is 0.12-0.15 mm, and the surface density is 100-150 g / m 2 .
[0015] Preferably, the material of the hot melt adhesive film layer is one of TPU film, PU film, EVA film, PO film, epoxy resin film, silicone film, polyurethane film, thermosetting film, thermoplastic film, phenolic resin film, polyacrylic resin film, polymethacrylate film, polycarbonate film, polyvinyl acetate film, and polyvinyl acetal film.
[0016] Preferably, the surface density of the graphene composite bulletproof plate is 60-70 kg / cm 2 .
[0017] The present invention also provides a preparation process of the graphene composite bulletproof plate, which specifically comprises the following steps:
[0018] (1) preparing a first transition layer, a second transition layer and a back plate by a lamination hot pressing process;
[0019] (2) Laying the layers in the order of a crack-stop layer, a graphene bulletproof ceramic layer, a first transition layer, a second transition layer, and a back plate, and adding a hot-melt adhesive film between the layers to form a preform;
[0020] (3) placing the preform into a vacuum bag, placing the vacuum bag into an autoclave for staged heating and vacuuming, and obtaining a composite bulletproof plate after cooling.
[0021] Preferably, the staged heating and vacuuming operation steps in step (3) are as follows:
[0022] The first stage lasts for 30-80 minutes, the vacuum pressure is controlled at 0.5-2MPa, and the temperature is controlled at 80-120℃;
[0023] The second stage lasts for 60-120 minutes, the vacuum pressure is controlled at 1-4MPa, and the temperature is controlled at 100-150℃;
[0024] The third stage lasts for 60-120 minutes, the vacuum pressure is controlled at 1-4MPa, and the temperature is controlled at 100-150℃.
[0025] Preferably, the hot pressing process of the layering in step (1) comprises the following steps: placing the raw material into a mold and performing three-stage heating and pressurizing operations, the specific operations are as follows:
[0026] The first stage: the mold temperature is raised to 60-90°C, the pressure is 6-8MPa, and the heating rate is 2-5°C / min;
[0027] The second stage: the mold temperature rises to 100-120℃, and the pressure is 12-17MPa;
[0028] The third stage: the mold temperature rises to 110-150℃ and the pressure is 20-25MPa;
[0029] When the mold temperature and pressure reach the third stage, stop heating and pressurizing, keep the temperature and pressure for 20-60 minutes, and the cooling rate is 2-5℃ / min. When the temperature drops to 30-60℃, start to release the pressure, and when the pressure drops to 0MPa, the mold is opened and taken out.
[0030] Compared with the prior art, the present invention has the following advantages:
[0031] The composite bulletproof plate of the present invention can provide stable protection capability. By optimizing the bulletproof structure design, the total surface density of the composite bulletproof plate is 40-45kg / m 2 Within the range, it can effectively prevent the impact of three rounds of Type 53 7.62mm API at a distance of 100m. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a schematic diagram of the structure of the graphene composite bulletproof plate described in an embodiment of the present invention.
[0033] Description of reference numerals:
[0034] 1. Crack-stop layer; 2. Hot-melt adhesive film layer; 3. Graphene bulletproof ceramic layer; 4. First transition layer; 5. Second transition layer; 6. Back panel. DETAILED DESCRIPTION
[0035] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.
[0036] The present invention is described in detail below in conjunction with embodiments.
[0037] Example 1
[0038] (1) Preparation of graphene bulletproof ceramic layer
[0039] 100 parts by mass of silicon carbide and 0.5 parts by mass of graphene powder were mixed, stirred and mixed in a ball mill for 45 minutes at a speed of 400 r / min. After mixing evenly, the powder was poured into a mold and hot-pressed and sintered. The mixed powder was placed in a press and pressed at a pressure of 7 MPa for 12 minutes. The pressed ceramic plate was then placed in an atmosphere furnace for sintering. The initial heating rate was 3°C / min, the temperature was raised to 850°C, and then the temperature was raised to 1480°C at a heating rate of 2°C / min, and the temperature was kept at that for 2 hours. The temperature was then lowered to 80°C at a rate of 5°C to obtain a graphene bulletproof ceramic plate.
[0040] (2) Preparation of the first transition layer
[0041] Lay two layers of carbon fiber prepreg in the corresponding mold and perform three-stage heating and pressurizing operations. The specific operations are as follows:
[0042] The first stage: the mold temperature is raised to 80°C, the pressure is 7MPa, and the heating rate is 5°C / min;
[0043] The second stage: the mold temperature rises to 120°C and the pressure is 15MPa;
[0044] The third stage: the mold temperature rises to 130°C and the pressure is 20MPa;
[0045] When the mold temperature and pressure reach the third stage, stop heating and pressurizing, keep the temperature and pressure for 60 minutes, and the cooling rate is 5℃ / min. When the temperature drops to 30℃, start to release the pressure and the pressure drops to 0MPa. The mold is opened and taken out to obtain the first transition layer with a thickness of 0.3mm.
[0046] (3) Preparation of the second transition layer
[0047] Two layers of aramid UD cloth were placed in the corresponding mold, and the rest of the preparation method was the same as that of the carbon fiber plate, and finally a second transition layer with a thickness of 0.3 mm was obtained.
[0048] (4) Preparation of PE backsheet
[0049] Put 15 layers of PEUD cloth in the corresponding mold, and the rest of the preparation method is the same as the carbon fiber board, and finally a PE backboard with a thickness of 8 mm is obtained.
[0050] (5) Preparation of graphene composite bulletproof plate
[0051] The layers are laid in the order of aramid woven fabric, graphene bulletproof ceramic layer, first transition layer, second transition layer, and back plate. The thickness between each layer is 0.12mm and the surface density is 150g / m 2 The TPU film is bonded to form a preform; the preform is placed in a vacuum bag, the vacuum bag is placed in an autoclave for staged heating and vacuuming, and a composite bulletproof plate is obtained after cooling. The staged heating and vacuuming operation steps are as follows: the first stage time is 50 minutes, the vacuuming pressure is controlled at 2MPa, and the temperature is controlled at 120℃; the second stage time is 120 minutes, the vacuuming pressure is controlled at 4MPa, and the temperature is controlled at 120℃; the third stage time is 120 minutes, the vacuuming pressure is controlled at 4MPa, and the temperature is controlled at 150℃.
[0052] The composite bulletproof plate was taken out from the vacuum bag for grinding operation. The specific steps were as follows: the composite bulletproof plate was ground with an angle grinder at a speed of 2000 rpm. The composite bulletproof plate was ground with 500-mesh coarse sandpaper for 10 min. Then, it was changed to 1500-mesh fine sandpaper for post-grinding treatment. The grinding time was 10 min.
[0053] The prepared graphene composite bulletproof plate was tested and its surface density was 41.6kg / m 2 .
[0054] Example 2
[0055] The preparation method of the graphene bulletproof ceramic layer, the first transition layer, the second transition layer, the PE back plate and the final graphene composite bulletproof plate is the same as that of Example 1, except that the mass fraction of graphene powder in the graphene bulletproof ceramic layer is 0.8 parts. The prepared graphene composite bulletproof plate is tested and its surface density is 42.3kg / m 2 .
[0056] Example 3
[0057] The preparation method of the graphene bulletproof ceramic layer, the first transition layer, the second transition layer, the PE back plate and the final graphene composite bulletproof plate is the same as that of Example 1, except that the mass fraction of graphene powder in the graphene bulletproof ceramic layer is 1 part. The prepared graphene composite bulletproof plate is tested and its surface density is 42.7 kg / m 2 .
[0058] Example 4
[0059] The preparation method of the graphene bulletproof ceramic layer, the first transition layer, the second transition layer, the PE back plate and the final graphene composite bulletproof plate is the same as that of Example 1, except that the number of carbon fiber prepreg layers in the first transition layer is 6 layers with a thickness of 4 mm, the number of aramid UD cloth layers in the second transition layer is 6 layers with a thickness of 4 mm, and the number of PEUD cloth layers in the PE back plate is 19 layers with a thickness of 10 mm. The prepared graphene composite bulletproof plate was tested and its surface density was 44.6 kg / m 2 .
[0060] The graphene composite bulletproof plates prepared in Examples 1-4 were subjected to a shooting test, wherein the shooting test was conducted by firing three 7.62 mm armor-piercing incendiary bullets at a shooting distance of 100 meters. The results of the shooting test are shown in the following table:
[0061]
[0062] From the shooting test results in the above table, it can be seen that the graphene composite bulletproof plates prepared in Examples 1-4 of the present invention can resist the attack of three 7.62mm armor-piercing incendiary bullets, and the back plate is not penetrated.
[0063] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A graphene composite bulletproof plate, characterized in that: The anti-crack layer, the graphene bulletproof ceramic layer, the first transition layer, the second transition layer and the back plate are sequentially arranged on the bullet-facing surface, and the adjacent layers are bonded by a hot-melt adhesive film layer, wherein the material of the graphene bulletproof ceramic layer is one or more of Al2O3 bulletproof ceramic, SiC bulletproof ceramic and B4C bulletproof ceramic added with graphene powder, and the addition amount of the graphene powder is 0.5%-1% of the total mass of the layer; The first transition layer is made of carbon fiber board with a thickness of 0.3-2mm; the second transition layer is made of aramid UD board with a thickness of 0.3-4mm; the crack arrest layer is aramid woven fabric layer with a thickness of 0.3-3mm; the thickness of the hot melt adhesive film layer is 0.12-0.15mm, and the surface density is 100-150g / m 2 ; The preparation method of the graphene composite bulletproof plate comprises the following steps: (1) preparing a first transition layer, a second transition layer and a back plate by a lamination hot pressing process; (2) Laying the layers in the order of a crack-stop layer, a graphene bulletproof ceramic layer, a first transition layer, a second transition layer, and a back plate, and adding a hot-melt adhesive film between the layers to form a prefabricated part; (3) placing the preform into a vacuum bag, placing the vacuum bag into an autoclave for staged heating and vacuuming, and obtaining a composite bulletproof plate after cooling; The staged heating and vacuuming operation steps in step (3) are as follows: The first stage lasts for 30-80 minutes, the vacuum pressure is controlled at 0.5-2MPa, and the temperature is controlled at 80-120℃; The second stage lasts for 60-120 minutes, the vacuum pressure is controlled at 1-4MPa, and the temperature is controlled at 100-150℃; The third stage lasts for 60-120 minutes, the vacuum pressure is controlled at 1-4MPa, and the temperature is controlled at 100-150℃.
2. The graphene composite bulletproof plate according to claim 1, characterized in that: The carbon fiber board is made by laminating and hot pressing 2-6 layers of carbon fiber prepreg.
3. The graphene composite bulletproof plate according to claim 1, characterized in that: Aramid UD board is made of 2-6 layers of aramid UD cloth laid and hot pressed.
4. The graphene composite bulletproof plate according to claim 1, characterized in that: The material of the hot melt adhesive film layer is one of TPU film, PU film, EVA film, PO film, epoxy resin film, silicone film, polyurethane film, thermosetting film, thermoplastic film, phenolic resin film, polyacrylic resin film, polymethacrylate film, polycarbonate film, polyvinyl acetate film, and polyvinyl acetal film.
5. The graphene composite bulletproof plate according to claim 1, characterized in that: The hot pressing process of the layering in step (1) includes the following steps: placing the raw material into the mold and performing three-stage heating and pressurizing operations, the specific operations are as follows: The first stage: the mold temperature is raised to 60-90°C, the pressure is 6-8MPa, and the heating rate is 2-5°C / min; The second stage: the mold temperature rises to 100-120℃, and the pressure is 12-17MPa; The third stage: the mold temperature rises to 110-150℃ and the pressure is 20-25MPa; When the mold temperature and pressure reach the third stage, stop heating and pressurizing, keep the temperature and pressure for 20-60 minutes, and the cooling rate is 2-5℃ / min. When the temperature drops to 30-60℃, start to release the pressure, and when the pressure drops to 0MPa, the mold is opened and taken out.