Phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin, preparation method and flame-retardant fabric prepared therefrom

By using tubular kaolin and a phosphorus-nitrogen synergistic composition in the fabric flame-retardant coating to form a dense carbon layer, the toxicity and water resistance problems of the existing fabric flame-retardant coating glue are solved, and an efficient and environmentally friendly flame retardant is achieved. performance, meeting green environmental protection standards.

CN114232350BActive Publication Date: 2024-10-22SHANDONG ACAD OF MARINE CHEM ENG
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202111507252.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-10
Publication Date
2024-10-22
Estimated Expiration
2041-12-10

AI Technical Summary

Technical Problem

The existing fabric flame-retardant coating glue contains halogen and antimony, which produce toxic substances when burned. The halogen-free expanded flame-retardant coating glue is not easy to self-extinguish when exposed to fire and is not resistant to water. It cannot meet the needs of green environmental protection and efficient flame retardancy.

Method used

A phosphorus-nitrogen synergistic water-based flame retardant coating composition containing tubular kaolin is used. By combining cyclic phosphate ester, ammonium polyphosphate, piperazine pyrophosphate and triazine carbon-forming agents, a dense porous foam carbon layer is formed to improve the resistance. It improves the combustion performance and stores liquid cyclic phosphate ester through the internal space of the tubular kaolin clay to reduce water loss.

Benefits of technology

It achieves the flame retardant effect of halogen-free, low smoke, low toxicity and anti-droplet. The coating has good water resistance and significant flame retardant effect. It can pass the BS5852 sofa flame retardant test and meet the requirements of green environmental protection and efficient flame retardancy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin, wherein the raw material composition comprises, by weight ratio, 25-45 parts of a film-forming agent, 5-15 parts of tubular kaolin, 5-15 parts of a carbon-forming agent, 10-35 parts of a phosphorus-containing flame retardant, 2-10 parts of an inorganic salt filler, 0.5-5 parts of a water-based coating additive, and 20-40 parts of water. The flame-retardant coating composition has good flame-retardant effect and excellent water resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin, a preparation method and a flame-retardant fabric made from the same. Background Art

[0002] Fabrics are a kind of polymer material, most of which are easy to burn. Many fire accidents in China are caused by textiles or interior decorations. Therefore, the country pays more and more attention to the field of fabric flame retardancy. Among them, polyester fabrics, which are widely used in textiles and industrial products, are flammable fibers. When burning, they are easy to burn through, curl, and melt and drip, causing secondary ignition of other objects and secondary injuries to people.

[0003] Flame retardant finishing of polyester fabric is the most commonly used flame retardant treatment process, and flame retardant coating adhesive is used in the process of fabric flame retardant finishing. Its flame retardant performance directly determines the flame retardant effect of polyester fabric after flame retardant treatment. At present, the most widely used in the market are bromine antimony fabric flame retardant coating adhesive and halogen-containing fabric flame retardant coating adhesive. For example, the Chinese patent CN200810104239.8 of the fabric flame retardant finishing process can obtain good fabric flame retardant effect, but the flame retardant coating adhesive contains halogen, which is easy to produce toxic substances when burning, which does not conform to the green and environmentally friendly development direction of flame retardants. Therefore, the application restrictions are increasing, and even banned. Chinese patent CN 105256572 B introduces a halogen-free coating adhesive flame retardant. Although it avoids the use of halogen-containing flame retardants, it fails to explain and demonstrate the two major problems of halogen-free intumescent flame retardant coating adhesive, which is not easy to self-extinguish and not water-resistant. This patent can prepare an environmentally friendly and non-toxic water-based coating adhesive with excellent charring performance through the use of halogen-free flame retardants. After being applied to the secondary flame retardant finishing of polyester yarn, it has the characteristics of burn-through resistance, self-extinguishing when away from fire, good water resistance and relatively low price. It can basically pass the BS5852:2006 sofa flame retardant test.

[0004] Public safety is the cornerstone of national security and social stability. Fire is one of the major disasters threatening public safety, causing a large number of casualties and huge economic losses every year. Textiles are an indispensable part of daily life. For example, textiles can be seen in curtains, fabrics, furniture and car interiors, toys, packaging materials and many other applications. Fire accident investigations have shown that a considerable number of fires are caused by textiles and interior decorations. China is the world's largest textile manufacturer, with total textile exports reaching US$284.1 billion in 2013. In recent years, flame retardant textiles, especially green and environmentally friendly new flame retardant textiles, have gradually become mandatory standards for high-rise buildings, public places, large aircraft and high-speed railways. my country's GB20286-2006 "Combustion Performance Requirements and Labeling of Flame Retardant Products and Components in Public Places" is a mandatory national standard, which also includes flame retardant requirements for textiles. The "Oeko-Tex Standard 100 General and Special Technical Conditions" and "Oeko-Tex Standard 200 Test Procedures" of the international ecological textile certification also have strict regulations on flame retardants applied to textiles.

[0005] At present, the most commonly used and effective flame retardant coating adhesive is still the bromine antimony type system. The bromine antimony type flame retardant system has excellent performance in gas phase flame retardancy and high cost performance, and is widely popular. However, the safety of halogen flame retardants and antimony-containing flame retardants has become a serious safety and environmental protection issue. Various countries and regions are establishing environmental protection standards to restrict the use of halogen flame retardants and antimony-containing flame retardants. At present, the most promising and most studied is the phosphorus nitrogen expansion composite flame retardant.

[0006] Intumescent composite flame retardant system (IFR) is a new type of composite flame retardant that has attracted wide attention in the field of flame retardancy in my country in recent years, replacing bromine antimony flame retardant. Intumescent composite flame retardant adopts acid source, carbon source and gas source to synergistically enhance flame retardancy, which is another classic synergistic combination in the field of flame retardancy. Intumescent flame retardant system can achieve efficient carbonization flame retardancy through condensed phase flame retardancy, forming a dense porous foam carbon layer on the surface of the fabric. It can not only prevent the further degradation of the inner polymer and the release of combustibles to the surface, but also prevent the transfer of heat source to the polymer and isolate the oxygen source, thereby preventing the spread and propagation of flames. It has the advantages of halogen-free, low smoke, low toxicity, anti-drip and no corrosive gas. However, when used in fabric flame retardants, halogen-free liquid phosphate flame retardants are slightly soluble in water or easily soluble in water, which can easily lead to the loss of flame retardants during the soaking and rinsing of fabrics, and the flame retardant effect is reduced. Summary of the invention

[0007] One of the purposes of the present invention is to provide a phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin, wherein the raw material composition comprises, by weight ratio:

[0008] 25-45 parts of film-forming agent, 5-15 parts of tubular kaolin, 5-15 parts of carbon-forming agent, 10-35 parts of phosphorus-containing flame retardant, 2-10 parts of inorganic salt filler, 0.5-5 parts of water-based coating additives, and 20-40 parts of water.

[0009] The film-forming agent is acrylate copolymer emulsion.

[0010] The tubular kaolin is tubular refractory kaolin, the average particle size of the tubular refractory kaolin particles is less than 200 nm, the inner diameter of the tubular refractory kaolin particles is 15-30 nm; the outer surface of the tubular refractory kaolin is a siloxane surface, and the inner surface has highly active aluminum alcohol acid points. The tubular refractory kaolin is a product of FMT Co., Ltd., product model: DRAGONITE-APA:M.

[0011] The carbon-forming agent is one of a triazine carbon-forming agent and a liquid epoxy resin or a combination of the two in any proportion.

[0012] The phosphorus-containing flame retardant is a combination flame retardant formed by cyclic phosphate and one or more of ammonium polyphosphate, piperazine pyrophosphate and alkyl hypophosphite. That is, the phosphorus-containing flame retardant can be a combination of two substances, for example, a combination of cyclic phosphate and ammonium polyphosphate, a combination of cyclic phosphate and piperazine pyrophosphate, and a combination of cyclic phosphate and alkyl hypophosphite; the phosphorus-containing flame retardant can be a combination of three substances, for example, a combination of cyclic phosphate and ammonium polyphosphate and piperazine pyrophosphate, a combination of cyclic phosphate and ammonium polyphosphate and alkyl hypophosphite, a combination of cyclic phosphate and piperazine pyrophosphate and alkyl hypophosphite; the phosphorus-containing flame retardant can be a combination of four substances, for example, a combination of cyclic phosphate and ammonium polyphosphate, piperazine pyrophosphate and alkyl hypophosphite. The mass proportion of cyclic phosphate in the combined flame retardant is not less than 20%.

[0013] The ammonium polyphosphate is a hydrophobically modified and coated ammonium polyphosphate, selected from one or a combination of any proportion of modified ammonium polyphosphate coated with melamine resin, modified ammonium polyphosphate coated with silicone gel, modified ammonium polyphosphate coated with polyurethane, modified ammonium polyphosphate coated with urea-formaldehyde resin, and modified ammonium polyphosphate coated with epoxy resin. Melamine-modified ammonium polyphosphate (APP-Ⅱ) is modified with melamine on the basis of type II ammonium polyphosphate, has a high degree of polymerization and does not contain formaldehyde, can effectively reduce the hygroscopicity of flame retardants, reduce the viscosity in the solution, improve heat resistance, and increase the compatibility of flame retardant systems with polymers and resins, significantly improving flame retardant efficiency and water resistance; therefore, melamine-modified ammonium polyphosphate (APP-Ⅱ) or a combination of melamine-modified ammonium polyphosphate (APP-Ⅱ) and the above-mentioned other phosphorus-containing flame retardants is preferred.

[0014] The inorganic salt filler is titanium dioxide.

[0015] The water-based paint additive is selected from one of a dispersant, an emulsifier, a thickener and a pH regulator, or a combination of two or more of them in any proportion; that is, the water-based paint additive may include a dispersant and a thickener, the water-based paint additive may include a dispersant, a pH regulator and a thickener, the water-based paint additive may include a dispersant, an emulsifier and a thickener, and the water-based paint additive may include a dispersant, an emulsifier, a thickener and a pH regulator.

[0016] The dispersant is an anionic dispersant, such as commercially available polyacrylic acid sodium salt dispersant 5040 or 731.

[0017] The emulsifier is a nonionic surfactant, such as commercially available BASF emulsifier XL-70 or X405.

[0018] The thickener is selected from any one of hydroxyethyl cellulose, polyacrylic acid thickener, polyvinyl alcohol and polyurethane thickener, or a mixture of two or more of them in any proportion; the polyacrylic acid thickener, polyvinyl alcohol and polyurethane thickener can specifically be selected from the following models: acrylic alkali thickener 8201 (alkali thickener), associative polyurethane thickener RM-8W (Rohm and Haas) and polyvinyl alcohol 1788.

[0019] The pH regulator is AMP-95.

[0020] The second object of the present invention is to provide a method for preparing a phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin, wherein the raw materials are taken according to the ratio of the above raw materials, and the steps taken include:

[0021] (1) Add water, dispersant and part of thickener in water-based coating additives into a dispersion kettle and stir and mix;

[0022] (2) Then, add the phosphorus-containing flame retardant, the carbonizing agent, the tubular kaolin, the inorganic salt filler, and the film-forming agent in sequence, and stir them thoroughly to disperse them so that the particle diameter of the dispersion liquid is less than 20 μm; an emulsifier may be added in this step as needed;

[0023] (3) Finally, the remaining thickener is added to adjust the viscosity, and the mixture is fully stirred and filtered to obtain the finished product. A pH adjuster can be added as needed in this step.

[0024] The third object of the present invention is to provide a flame retardant fabric; the flame retardant fabric is prepared by coating the phosphorus-nitrogen synergistic water-based flame retardant coating composition containing tubular kaolin described in the present invention on textiles and then drying the resulting fabric.

[0025] The textile is selected from textiles of any one fiber of nylon fiber, cotton fiber and polyester fiber, or blended products of any two fibers or blended products of the three fibers.

[0026] The flame retardant fabric is antimony-free and halogen-free.

[0027] The term "antimony-free" as used herein refers to a composition to which antimony (as elemental antimony or an antimony-containing alloy, compound or other similar substance) is not specifically added, so that antimony is present in the flame retardant composition only as a trace component or as an impurity of 0.1 wt % or less.

[0028] The term "halogen-free" used in the present invention refers to a composition in which no halogen-containing compound or other similar substances are particularly added so that halogen exists in the flame retardant composition as a trace component or as an impurity of 0.09 wt % or less.

[0029] The traditional intumescent (IFR) flame retardant system is composed of an acid source, a carbon source and a gas source. The carbon-forming agent selected by the present invention is a triazine macromolecular carbon-forming agent (CFA) and a liquid epoxy resin. During use, it has good water resistance and durability, is not easy to migrate to the surface of the substrate, and improves the shortcomings of the small molecule carbon-forming agent. At the same time, it can achieve a good carbon-forming effect in coordination with the acid source (P), and has the advantages of high decomposition temperature, good compatibility, no exudation and excellent flame retardant performance, so the use of a macromolecular carbon-forming agent has great practicality.

[0030] The outer surface of tubular refractory kaolin is a siloxane surface, and the inner part is a highly active aluminum alcohol acid point. When the temperature reaches a certain level, the internal aluminum alcohol acid point can promote the decomposition of polymer materials, form a heat-insulating, gas-isolating carbonized layer, and improve the flame retardancy and drip resistance. At the same time, when used in conjunction with phosphorus flame retardants, it can form highly heat-resistant aluminum phosphate to improve flame retardancy. When used in conjunction with liquid cyclic phosphate esters for flame-retardant fabric coatings, while improving flame retardancy and carbonization, it can also store liquid cyclic phosphate esters in the inner space of tubular kaolin, and solidify them in the tubular kaolin inside the fabric coating glue under high-temperature baking, thereby improving the disadvantage of cyclic phosphate esters in fabric coatings that are not water-resistant.

[0031] The present invention introduces micron-sized tubular kaolin and cyclic phosphate into the traditional PN intumescent composite flame retardant system (IFR). When the PN flame retardant synergy is realized, the aluminum alcohol acid point inside the tubular kaolin is decomposed to form a carbonized layer that insulates heat and isolates gas, thereby improving the flame retardancy. At the same time, the tubular internal space can also store the cyclic phosphate flame retardant, thereby reducing the loss caused by soaking in water and improving the flame retardant effect after soaking in water. A heavy metal-free textile flame retardant coating system is provided that retains the advantages of the intumescent composite flame retardant system (IFR) while overcoming the disadvantage that the flame retardant efficiency of the intumescent composite flame retardant system decreases greatly after soaking in water. That is to say, after the phosphorus-nitrogen synergistic water-based flame retardant coating composition containing tubular kaolin of the present invention forms a coating on the fabric, the coating not only has good water resistance, but also has a very significant flame retardant effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1This is the effect diagram of the sample of Example 1 after burning for 20 seconds;

[0033] Figure 2 This is the effect diagram of the sample of Example 2 after burning for 20 seconds;

[0034] Figure 3 This is the effect diagram of the sample of Example 3 after burning for 20 seconds;

[0035] Figure 4 This is the effect diagram of the sample of Example 4 after burning for 20 seconds.

[0036] Figure 5 This is the effect diagram of the sample of Example 5 after burning for 20 seconds.

[0037] Figure 6 This is the effect diagram of the sample of Example 6 after burning for 20 seconds. DETAILED DESCRIPTION

[0038] The feasibility of the technical solution of the present invention is illustrated below by way of examples, but the protection scope of the present invention should not be limited to the following specific examples.

[0039] Example 1

[0040] The raw material composition of the water-based flame retardant coating composition is calculated by weight ratio:

[0041] Acrylic copolymer emulsion 35 parts

[0042] Melamine 8 parts

[0043] 25 parts of melamine resin-coated modified ammonium polyphosphate

[0044] Pentaerythritol 5 parts

[0045] Hydroxyethyl cellulose 0.1 parts

[0046] Acrylic thickener 8201 0.1 parts

[0047] 30 parts water

[0048] Dispersant (polyacrylic acid sodium salt dispersant 5040) 0.4 parts;

[0049] Emulsifier (BASF emulsifier XL-70) 0.1 part;

[0050] AMP-95 0.1 parts.

[0051] Example 2

[0052] The raw material composition of the water-based flame retardant coating composition is calculated by weight ratio:

[0053] Acrylic copolymer emulsion 35 parts

[0054] 8 parts of modified ammonium polyphosphate wrapped with melamine resin

[0055] 5 parts of triazine charcoal forming agent

[0056] Decabromodiphenylethane 16 parts

[0057] 4 parts of titanium dioxide

[0058] Hydroxyethyl cellulose 0.1 parts

[0059] PVA1788 thickener 0.1 part

[0060] 30 parts water

[0061] Dispersant (polyacrylic acid sodium salt dispersant 5040) 0.4 parts;

[0062] Emulsifier (BASF emulsifier XL-70) 0.1 part;

[0063] AMP-95 0.1 parts.

[0064] Example 3

[0065] The raw material composition of the phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin is calculated by weight ratio:

[0066] Film former (acrylic copolymer emulsion) 35 parts;

[0067] Phosphorus-containing flame retardant (melamine resin-wrapped modified ammonium polyphosphate 12 parts + cyclic phosphate ester 4 parts) 16 parts;

[0068] Carbon former (triazine carbon former 4 parts + liquid epoxy resin 6 parts) 10 parts;

[0069] 5 parts of tubular refractory kaolin;

[0070] 2 parts of inorganic salt filler (titanium dioxide);

[0071] 30 parts water;

[0072] 0.9 parts of water-based paint additives; the specific composition of the water-based paint additives is as follows:

[0073] Thickener (0.1 part hydroxyethyl cellulose + 0.2 part PVA1788 thickener) 0.3 part

[0074] Dispersant (polyacrylic acid sodium salt dispersant 5040) 0.4 parts;

[0075] Emulsifier (BASF emulsifier XL-70) 0.1 part;

[0076] pH adjuster (AMP-95) 0.1 parts.

[0077] Example 4

[0078] The raw material composition of the phosphorus-nitrogen synergistic water-based flame-retardant coating composition is calculated by weight ratio:

[0079] Film former (acrylic copolymer emulsion) 35 parts;

[0080] Phosphorus-containing flame retardant (melamine resin-wrapped modified ammonium polyphosphate 14 parts + cyclic phosphate ester 4 parts) 18 parts;

[0081] Carbon former (5 parts of triazine carbon former + 7 parts of liquid epoxy resin) 12 parts;

[0082] Inorganic salt filler (titanium dioxide) 2 parts;

[0083] 30 parts water;

[0084] 0.8 parts of water-based paint additives; the specific composition of water-based paint additives is as follows:

[0085] Thickener (hydroxyethyl cellulose 0.1 part + PVA1788 thickener 0.1 part) 0.2 part;

[0086] Dispersant (polyacrylic acid sodium salt dispersant 731) 0.4 parts;

[0087] Emulsifier (BASF emulsifier XL-70) 0.1 part;

[0088] pH adjuster (AMP-95) 0.1 parts.

[0089] Example 5

[0090] The raw material composition of the phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin is calculated by weight ratio:

[0091] Film former (acrylic copolymer emulsion) 25 parts;

[0092] Phosphorus-containing flame retardant (10 parts of modified ammonium polyphosphate wrapped in urea-formaldehyde resin + 5 parts of cyclic phosphate ester) 15 parts;

[0093] Carbon former (5 parts of triazine carbon former + 6 parts of liquid epoxy resin) 11 parts;

[0094] 7 parts of tubular refractory kaolin;

[0095] 2 parts of inorganic salt filler (titanium dioxide);

[0096] 35 parts water;

[0097] 0.8 parts of water-based paint additives; the specific composition of water-based paint additives is as follows:

[0098] Thickener (hydroxyethyl cellulose 0.1 part + PVA1788 thickener 0.1 part) 0.2 part;

[0099] Dispersant (polyacrylic acid sodium salt dispersant 5040) 0.3 parts;

[0100] Emulsifier (BASF emulsifier X405) 0.2 parts;

[0101] pH adjuster (AMP-95) 0.1 parts.

[0102] Example 6

[0103] The raw material composition of the phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin is calculated by weight ratio:

[0104] Film former (acrylic copolymer emulsion) 30 parts;

[0105] Phosphorus-containing flame retardant (14 parts of epoxy resin-coated modified ammonium polyphosphate + 4 parts of cyclic phosphate) 18 parts;

[0106] Carbon former (6 parts of triazine carbon former + 5.5 parts of liquid epoxy resin) 11.5 parts;

[0107] 6 parts of tubular refractory kaolin;

[0108] Inorganic salt filler (titanium dioxide) 3 parts;

[0109] 35 parts water;

[0110] 0.8 parts of water-based paint additives; the specific composition of water-based paint additives is as follows:

[0111] Thickener (hydroxyethyl cellulose 0.1 part + PVA1788 thickener 0.1 part) 0.2 part;

[0112] Dispersant (polyacrylic acid sodium salt dispersant 5040) 0.3 parts;

[0113] Emulsifier (BASF emulsifier XL-70) 0.2 parts;

[0114] pH adjuster (AMP-95) 0.1 parts.

[0115] Example 1, Example 2 and Example 4 are used as comparative examples, and their preparation methods can refer to the preparation methods of Examples 3, 5 and 6. The steps of the preparation methods of Examples 3, 5 and 6 are as follows:

[0116] (1) Add water, dispersant and part of thickener into a dispersion kettle and stir and mix;

[0117] (2) Then add the phosphorus-containing flame retardant, carbonizing agent, tubular kaolin, inorganic salt filler, emulsifier, and film-forming agent in sequence, stir and disperse them thoroughly, and make the particle diameter of the dispersion liquid less than 20 μm;

[0118] (3) Finally, add the remaining thickener and pH regulator to adjust the viscosity and pH value, stir thoroughly and filter to obtain the finished product.

[0119] The physical indicators of the water-based flame retardant coating adhesive prepared by the present invention are as follows:

[0120] Appearance: milky white or slightly yellow viscous liquid;

[0121] Solid content: 50±10%;

[0122] Viscosity: 80-130KU;

[0123] pH value: 6.0-9.0.

[0124] The preparation method of flame retardant fabric is as follows:

[0125] Take the phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin prepared in any one of Examples 3, 5 and 6, apply it on a textile, and then dry it to obtain a flame-retardant fabric. The textile is selected from a textile of any fiber selected from nylon fiber, cotton fiber and polyester fiber, or a blend of any two fibers or a blend of three fibers.

[0126] Water resistance test

[0127] The water-based flame retardant coating composition prepared in the above example is applied to a surface with a gram weight of 200 g / m 2 The back of the polyester sofa fabric is dried in an oven at 165 degrees for 2-3 minutes, and the coating weight is controlled at 105g±5g / m 2 range. Weigh the weight W1 of the dried coated adhesive sofa cloth, soak it in a 40℃ warm water bath for 30 minutes, then take it out and dry it in a 105℃ oven for 1 hour, and weigh it W2. Calculate the weight loss rate of the water-based flame retardant coating adhesive after soaking in water, that is, the weight loss rate %=100*(W1-W2) / W1. The water-based flame retardant coating composition prepared in each embodiment is applied to 3 pieces of sofa cloth respectively, and the weight loss rate is calculated according to the above steps, and the average value is taken; the test results are shown in Table 1;

[0128] Table 1

[0129] Flame retardant system type Example Weight loss rate% illustrate Halogen-free intumescent flame retardant system Example 1 27.9 Halogen-free PN system Bromine-phosphorus synergistic system Example 2 6.5 P-Br synergistic, macromolecular triazine carbon forming agent Halogen-free intumescent flame retardant system Example 3 9.8 Halogen-free PN system, macromolecular triazine and liquid epoxy, tubular kaolin charring flame retardant Halogen-free intumescent flame retardant system Example 4 15.5 Halogen-free PN system, macromolecular triazine and liquid epoxy carbonization flame retardant Halogen-free intumescent flame retardant system Example 5 10.0 Halogen-free PN system, macromolecular triazine and liquid epoxy, tubular kaolin charring flame retardant Halogen-free intumescent flame retardant system Example 6 9.6 Halogen-free PN system, macromolecular triazine and liquid epoxy, tubular kaolin charring flame retardant

[0130] The water loss rate represents the water resistance of the flame retardant coating composition. The greater the water loss rate, the worse the water resistance of the flame retardant coating composition. As can be seen from the above table, the water loss rate of Example 1 is 27.9%, and the water resistance is the worst. The weight loss rate of Example 2 is 6.5%, mainly because it is a phosphorus-halogen synergistic system, part of the flame retardant used is water-resistant decabromodiphenylethane, and there is no water-soluble flame retardant such as pentaerythritol and melamine, so the water resistance is improved. The weight loss rates of Examples 3, 5, and 6 are about 10%, which is higher than that of Example 2. This is mainly because Examples 3, 5, and 6 use water-soluble cyclic phosphate flame retardants, which leads to an increase in their weight loss rates. At the same time, compared with Example 4 (weight loss rate 15.5%), the weight loss rates of Examples 3, 5, and 6 are reduced to about 10%. This is mainly because Example 4 does not add tubular kaolin, while Examples 3, 5, and 6 add tubular kaolin, so that a part of the cyclic phosphate flame retardant is stored inside the tubular kaolin, and solidified inside the coating during high-temperature drying, thereby improving its water resistance.

[0131] Flame retardant performance test

[0132] Flame retardant properties refer to BS5852 flame retardant test standard. The samples are covered with specified polyurethane sponges and ignited under specified burners. The butane flame height is 35mm. After the flame is stable for 30s, the sample is burned with the flame for 20s to test the flame retardant properties of the sample. The test results are shown in Table 2.

[0133] Table 2

[0134] Example Name Experimental phenomenon Whether it passes BS5852 flame retardant standard Example 1 The sample will have a large hole after burning for 5-8 seconds. After burning for 20 seconds, the fire will not extinguish itself and ignite the polyurethane sponge (see Appendix). Figure 1 ) Not passed Example 2 The sample will have a large hole after burning for 5-8 seconds, and will go out after burning for 20 seconds without igniting the polyurethane sponge (see Appendix Figure 2 ) pass Example 3 The sample burns to form an expansive carbon layer with bubbles on the surface, and small holes appear, but the holes do not expand. After burning for 20 seconds, the fire goes out and the polyurethane sponge is not ignited (see Appendix Figure 3 ) pass Example 4 The sample burns to form an expansive carbon layer with small holes, which continue to expand. After burning for 20 seconds, it does not extinguish itself when the fire is removed. After leaving the fire for 10 seconds, it ignites the polyurethane sponge (see Appendix). Figure 4 ) Not passed Example 5 The sample burns to form an expansive carbon layer with bubbles on the surface, and small holes appear, but the holes do not expand. After burning for 20 seconds, the fire goes out and the polyurethane sponge is not ignited (see Appendix Figure 5 ) pass Example 6 The sample burns to form an expansive carbon layer with bubbles on the surface, and small holes appear, but the holes do not expand. After burning for 20 seconds, the fire goes out and the polyurethane sponge is not ignited (see Appendix Figure 6 ) pass

[0135] It can be seen from the results in the above table that Example 1 simply uses the classic halogen-free PN flame retardant system, and the flame retardant performance cannot reach the flame retardant standard of BS5852 because the mass loss after soaking in water is too large. The phosphorus-nitrogen-inorganic synergistic flame retardant coating formula of the present invention is used in combination with tubular refractory kaolin and cyclic phosphate ester to reduce the loss of soaking in water, improve water resistance, and provide gas phase flame retardancy and solid phase flame retardancy to enhance flame retardancy. In combination with tubular kaolin and liquid epoxy resin, the flame retardant performance of the flame retardant coating can be greatly improved, and can reach the flame retardant standard of B1.

Claims

1. A phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin, characterized in that: The raw material composition includes the following by weight ratio: 25-45 parts of film-forming agent, 5-15 parts of tubular kaolin, 5-15 parts of carbon-forming agent, 10-35 parts of phosphorus-containing flame retardant, 2-10 parts of inorganic salt filler, 0.5-5 parts of water-based coating additive, 20-40 parts of water; the film-forming agent is an acrylic copolymer emulsion; the tubular kaolin is tubular refractory kaolin, and the average particle size of the tubular refractory kaolin particles is 200 nm or less, the inner diameter of the tubular refractory kaolin particles is 15-30nm; the outer surface of the tubular refractory kaolin is a siloxane surface, and the inner surface has highly active aluminum alcohol acid points. The product model of the tubular refractory kaolin is DRAGONITE-APA:M; the carbon former is a combination of a triazine carbon former and a liquid epoxy resin in any proportion; the phosphorus-containing flame retardant is a combined flame retardant formed by a cyclic phosphate ester and ammonium polyphosphate, and the mass proportion of the cyclic phosphate ester in the combined flame retardant is not less than 20%; the ammonium polyphosphate is a hydrophobically modified and coated ammonium polyphosphate, selected from one or a combination of any two or more of modified ammonium polyphosphate coated with melamine resin, modified ammonium polyphosphate coated with silicone gel, modified ammonium polyphosphate coated with polyurethane, modified ammonium polyphosphate coated with urea-formaldehyde resin, and modified ammonium polyphosphate coated with epoxy resin.

2. The phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin according to claim 1, characterized in that: The inorganic salt filler is titanium dioxide.

3. The phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin according to claim 1, characterized in that: The water-based coating additive is selected from one of a dispersant, an emulsifier, a thickener and a pH regulator, or a combination of two or more of them in any proportion.

4. The phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin according to claim 3, characterized in that: The dispersant is an anionic dispersant; The emulsifier is a nonionic surfactant; The thickener is selected from any one of hydroxyethyl cellulose, polyacrylic thickener, polyvinyl alcohol and polyurethane thickener, or a mixture of two or more of them in any proportion; The pH regulator is AMP-95.

5. A method for preparing the phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin according to claim 1, characterized in that: The following steps are involved: (1) Add water, dispersant and part of thickener in water-based coating additives into a dispersion kettle and stir and mix; (2) Then, add the phosphorus-containing flame retardant, the carbonizing agent, the tubular kaolin, the inorganic salt filler, and the film-forming agent in sequence, and stir them thoroughly to disperse them so that the particle diameter of the dispersion liquid is less than 20 μm; an emulsifier may be added in this step as needed; (3) Finally, the remaining thickener is added to adjust the viscosity, and the mixture is fully stirred and filtered to obtain the finished product. A pH adjuster can be added as needed in this step.

6. A flame retardant fabric, characterized in that: The coating is prepared by coating the phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin as described in any one of claims 1 to 4 on textiles and drying the coating; or the coating is prepared by coating the phosphorus-nitrogen synergistic water-based flame-retardant coating composition containing tubular kaolin obtained by the method described in claim 5 on textiles and drying the coating.

7. The flame retardant fabric according to claim 6, characterized in that: The textile is selected from textiles of any one fiber of nylon fiber, cotton fiber and polyester fiber, or blended products of any two fibers or blended products of the three fibers.

8. The flame retardant fabric according to claim 6 or 7, characterized in that: The flame retardant fabric is antimony-free and halogen-free.

Citation Information

Patent Citations

  • Composite type flame-retardant adhesive for high-strength terylene filament fabric and flame-retardant finishing method

    CN101280523A

  • A kind of halogen-free flame-retardant coating glue and preparation method thereof

    CN105256572B

  • High-efficiency halogen-free environment-friendly fire retardant for textile coating and preparation method of high-efficiency halogen-free environment-friendly fire retardant

    CN106930093A

  • Preparation method of special precipitation-resistant halogen-free flame retardant for polypropylene

    CN108822400A

  • Intumescent steel structure fireproof coating

    CN112322167A