A method for preparing multi-element pre-alloyed powder based on ferrothermal reaction and a method for preparing a diamond tool matrix
Through ferrothermal reaction eutectic combustion synthesis and reducing gas treatment, the problems of complex alloy powder preparation and unfriendly environment in the existing technology are solved. Multi-component pre-alloyed powder with high alloying degree and good uniformity is obtained, which can be used to prepare high-quality alloy powder. Performance diamond tool carcass.
Patent Information
- Application Number
- CN202210068921.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-01-21
AI Technical Summary
Existing alloy powder preparation methods have problems such as complex operation, unfriendly environment, low alloying degree, component segregation and coarse powder grains, making it difficult to obtain efficient, simple and environmentally friendly multi-component pre-alloyed powders.
The eutectic combustion synthesis method based on ferrothermal reaction is adopted, and high-purity iron powder and additives are used for eutectic combustion synthesis to generate high-purity multi-component pre-alloyed powder, and the metal oxide is further reduced by reducing gas to obtain multi-component pre-alloyed powder with high alloying degree. alloy powder.
The preparation of multi-component pre-alloyed powder with high purity and good uniformity is achieved, which reduces the preparation cost and environmental impact, avoids the generation of by-products, improves the market competitiveness of the powder, and is used to prepare high-performance diamond tool bodies.
Smart Images

Figure CN114273665B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alloy powder preparation, and in particular relates to a method for preparing multi-element pre-alloyed powder based on ferrothermic reaction and a method for preparing a diamond tool matrix. Background Art
[0002] Metal combustion synthesis was first proposed by Goldschmidt in 1908 as the "aluminothermic method" to describe the exothermic reaction of metal oxides with aluminum to produce aluminum oxide and metal or alloy.
[0003] In 1953, the British first proposed the concept of self-propagation of metal powder combustion in the paper "Self-propagation of Strongly Exothermic Chemical Reaction". In 1967, Merzhanov et al. proposed the self-propagating high-temperature synthesis method. The main advantages of this method are that the energy required for the reaction synthesis is generated by itself (energy saving), the product purity is high (low boiling point impurities are volatilized at high temperature), the reaction speed is fast, and the output is high, so it has very great economic value.
[0004] At present, the main methods for preparing alloy powders used in the field of powder metallurgy are as follows:
[0005] Method 1: Mix various elemental powders, also known as "solid-solid" mixing, and the resulting mixture is called alloy powder.
[0006] Method 2: The preparation method of pre-alloyed powder is mainly divided into atomization method, hydrometallurgical method and mechanical diffusion method, as follows:
[0007] (1) Atomization method: At present, the most commonly used method is high-pressure atomization to produce pre-alloyed powders. The single metals of various components are smelted into alloys, and then atomized and sprayed to obtain pre-alloyed powders of the required particle size. The atomization method can be water atomization or gas atomization. Gas atomization can use gases such as air, nitrogen or argon. Gas atomization has a fast cooling speed and a high powder yield, but the powder grains are coarse.
[0008] (2) Hydrometallurgical method: The hydrometallurgical method is to dissolve metal ions in water, and mix different elemental metals in the alloy (such as cobalt, copper, and iron salt solutions) in the solution in the correct proportion to form metal salts, and then obtain very fine metal alloy powders through precipitation and reduction. Since each powder particle of the wet pre-alloyed powder contains various metal elements that make up the alloy, the pre-alloyed powder has a very good uniformity of composition, but this method will put pressure on the ecological environment.
[0009] (3) Mechanical diffusion method: In the preparation process of solid + solid alloy powder, the element powder is continuously deformed, welded, and broken during the ball milling process, so that the size of the layered structure of different powders overlapping each other becomes smaller and smaller, and the atoms gradually alloy through interface diffusion. This method is simple and has low production cost, but the ball milling process is time-consuming and the components in the obtained alloy are segregated.
[0010] In summary, the precursor pre-alloyed powders of the alloy powders prepared by the above methods all have problems. Therefore, designing a preparation method of a multi-component pre-alloyed powder with simpler operation, environmental friendliness, high alloying degree, no segregation and finer powder grains has become a new goal pursued by technical personnel in this field. Summary of the invention
[0011] In order to overcome the problems existing in the prior art, one of the purposes of the present invention is to provide a method for preparing multi-component pre-alloyed powder based on ferrothermal reaction, which is simple to operate, environmentally friendly, and has a high degree of alloying and no segregation of the obtained multi-component pre-alloyed powder.
[0012] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is as follows:
[0013] A method for preparing multi-element pre-alloyed powder based on ferrothermal reaction specifically comprises the following steps:
[0014] Step S1: preparing an alloy system containing iron powder and additives;
[0015] Step S2: Ignite the alloy system to undergo eutectic combustion synthesis, so that the iron powder and the additive surface are welded together to obtain a precursor containing metal oxides; wherein the igniter is high-purity iron powder contained in the iron powder, the mass of the high-purity iron powder is not less than 10% of the mass of the alloy system, and the average particle size is less than 30 μm; currently, the market generally agrees that high-purity iron powder refers to iron powder with an iron content of more than 98%;
[0016] Step S3: reducing the metal oxides in the precursor to obtain multi-element pre-alloyed powder.
[0017] Preferably, the alloy system in step S2 is fully mixed with the reducing agent before eutectic combustion synthesis, and the reducing agent is used to reduce part of the metal oxides in the precursor.
[0018] Preferably, the mass of the iron powder is not less than 50% of the mass of the alloy system material.
[0019] Preferably, the mass of the reducing agent is 15%-66.7% of the mass of the iron powder, and the reducing agent is selected from any one or more of carbon powder, charcoal powder and coke powder with an average particle size of 325-500 meshes.
[0020] Preferably, the additive is any one or more of metal oxide, metal salt and metal element powder, and the mass of the additive is 1%-50% of the mass of the alloy system.
[0021] Preferably, when the additive is a metal oxide or a metal element powder, the average particle size is less than 200 mesh or less than or equal to 30 μm; and the element is any one or more of copper, zinc, cobalt, nickel and aluminum; the metal oxide is any one or more of CuO, ZnO, CoO, Co2O3, Co3O4, NiO and Ni2O3; when the additive is a metal salt, the metal salt is any one or more of NiCO3, CoCO3, Cu CO3, Cu2(OH)2CO3, Ni2(OH)2CO3, Co2(OH)2CO3, CoC2O4, CuC2O4 and NiC2O4.
[0022] Preferably, in step S2, the alloy system undergoes eutectic combustion synthesis in a burner with a stirring function.
[0023] Preferably, in step S3, the metal oxide is reduced by using reducing gas, the reduction temperature is 350-750° C., and the reduction time is 6-8 hours; and the precursor is crushed before reduction, and the processing time is 30-60 minutes.
[0024] Preferably, in step S2, a combustion aid is added to increase the rate of eutectic combustion synthesis of iron powder and additives; the mass of the combustion aid is 1%-5% of the mass of the alloy system.
[0025] Another object of the present invention is to provide a method for preparing a diamond tool matrix by mixing multi-element pre-alloyed powder prepared based on ferrothermal reaction with diamond and then sintering the mixture.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] (1) The present invention utilizes the high-purity iron powder with an average particle size of less than 30 μm, which has extremely strong flammability, so that the iron powder is ignited and releases a large amount of heat, and the heat released can reach a high temperature of 800-1100°C, thereby promoting the eutectic combustion synthesis of the iron powder and the additive, allowing the iron powder and the additive surface to be welded together (when the additive is a metal salt, the additive decomposes into metal oxides at high temperature, and the iron powder and the decomposed metal oxides are welded together at this time), and a precursor with a high degree of alloying, uniform composition and no segregation and containing metal oxides is obtained. In this way, the method of preparing the precursor based on the iron heat reaction adopted by the present invention solves the problem of pre-alloy powder segregation in the prior art. Secondly, the iron powder and additives in the precursor prepared by the method of the present invention are both involved in the preparation of the precursor, there is no waste of raw materials, and the yield is relatively high; and in the process of preparing the multi-component pre-alloyed powder by the method of the present invention, no by-products and environmentally harmful substances are generated. Therefore, the preparation method of the present invention has the characteristics of being environmentally friendly and simple to operate, and the precursor of the present invention can be obtained by only igniting the alloy system containing iron powder and additives.
[0028] (2) The present invention utilizes the heat released during the eutectic combustion synthesis of iron powder and additives to prompt the reducing agent to reduce part of the metal oxides in the precursor, and finally uses the reducing gas to reduce the remaining metal oxides in the precursor to obtain the multi-component pre-alloyed powder of the present invention. Therefore, the preparation method of the multi-component pre-alloyed powder of the present invention greatly simplifies the complicated multi-component pre-alloyed powder preparation process on the existing market; in addition, in the present invention, the heat released by the eutectic combustion synthesis prompts the reducing agent to reduce part of the metal oxides in the precursor, reducing the amount of metal oxides that need to be reduced by reducing gas, reducing the consumption of reducing gas and energy, and thus reducing the preparation cost of the multi-component pre-alloyed powder, so that the multi-component pre-alloyed powder has a good market prospect. In addition, in order to further reduce the preparation cost of the multi-component pre-alloyed powder, the present invention generally selects metal oxides and metal salts with lower prices, which further enhances the market competitiveness of the multi-component pre-alloyed powder prepared by the invention.
[0029] (3) In the present invention, the alloy system is added to the burner with stirring function, which ensures that the additive and the iron powder are mixed evenly, thereby avoiding the iron powder and the additive from being welded together during the eutectic combustion synthesis to form large-particle precursor powder, preventing segregation during the precursor preparation process, and making the multi-element pre-alloyed powder obtained after the metal oxide in the precursor is fully reduced have the characteristics of high alloying degree, uniform composition and no segregation. In addition, the burner with stirring function can also promote the eutectic combustion of iron powder and additives, further avoiding the problem of segregation during the preparation of alloy powder.
[0030] (4) The method described in the present invention utilizes the self-propagating principle to prepare multi-component pre-alloyed powder. The multi-component pre-alloyed powder prepared by the method described in the present invention only needs to ignite the iron powder with an average particle size of less than 30 μm in the alloy system, thereby prompting all the iron powder to ignite, and utilizing the heat released by the iron powder after combustion to form a high temperature of 800-1100°C to promote the eutectic combustion synthesis of the iron powder and the additive, so that the iron powder and the additive are welded together or the iron powder is coated on the additive, and the precursor described in the present invention can be obtained. Therefore, in the entire reaction process of preparing the precursor using the present invention, except for the need to provide a heat source when the alloy system is ignited, no additional heat source is required in the entire process, which also reduces the preparation cost of the multi-component pre-alloyed powder obtained after the metal oxides in the precursor are fully reduced.
[0031] (5) The alloy system in the present invention can also be subjected to eutectic combustion synthesis together with a combustion aid. The combustion aid utilizes the heat released during the eutectic combustion synthesis process to decompose and release active oxygen. On the one hand, this shortens the time for the eutectic combustion synthesis of the iron powder and the additive, thereby not only improving the eutectic rate of the precursor described in the present invention, but also improving the yield of the multi-component pre-alloyed powder described in the present invention, and reducing the preparation cost of the multi-component pre-alloyed powder described in the present invention; on the other hand, it promotes a more complete eutectic combustion synthesis between the iron powder and the additive, thereby further avoiding the problem of segregation of the multi-component pre-alloyed powder prepared by precursor reduction, effectively improving the alloying degree of the multi-component pre-alloyed powder, improving the product quality of the multi-component pre-alloyed powder, and greatly enhancing its market competitiveness.
[0032] (6) The multi-element pre-alloyed powder prepared by the present invention is made into a diamond tool matrix together with diamond, which not only has the advantages of high sharpness and high hardness, but also the diamond tool made of the diamond tool matrix can be used for cutting harder 635# granite, C35 threaded steel, hard pebbles in addition to ordinary materials such as stone and ceramic tiles, and all of them show the characteristics of long life and low loss. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 EDS image of the FeCu binary pre-alloyed powder prepared by the present invention;
[0034] Figure 2 The SEM image of the FeCu binary pre-alloyed powder prepared by the present invention;
[0035] Figure 3 The metallographic diagram of the FeCu binary pre-alloyed powder prepared by the present invention;
[0036] Figure 4 EDS image of the FeNi binary pre-alloyed powder prepared by the present invention;
[0037] Figure 5 The SEM image of the FeNi binary pre-alloyed powder prepared by the present invention;
[0038] Figure 6 The metallographic diagram of the FeNi binary pre-alloyed powder prepared by the present invention;
[0039] Figure 7 The EDS image of the FeNiCuSnP alloy powder after the FeNiCuSnP quaternary pre-alloy powder prepared by the present invention is phosphated;
[0040] Figure 8 The SEM image of the FeNiCuSnP alloy powder after the FeNiCuSnP quaternary pre-alloy powder prepared by the present invention is phosphated;
[0041] Fig. 9 The metallographic diagram of the FeNiCuSnP alloy powder after the FeNiCuSnP quaternary pre-alloy powder prepared by the present invention is phosphated;
[0042] Fig.10 The SEM images of the FeCuCo ternary pre-alloyed powder prepared by the present invention are shown in Figure a at a magnification of 5000 times and Figure b at a magnification of 10000 times. DETAILED DESCRIPTION
[0043] 1. Iron powder: The iron powder with an average particle size of less than 30 μm in the present invention comes from "Ya'an Shijia Weier Technology Co., Ltd.", and the test results of each element component in the iron powder with an average particle size of less than 30 μm are shown in Table 1.
[0044] Table 1 Test table of various element components in iron powder with an average particle size less than 30μm
[0045] Components Test standards for each element Content (wt%) Iron (Fe) GB / T 223.7-2002 Determination of iron content in iron powder 98.95 Carbon (C) RO-444 infrared carbon analyzer ≤0.03 Nitrogen (N) TC-436 Oxygen and Nitrogen Tester ≤0.01 Oxygen (O) GB / T4164-2008 Determination of the content of oxygen that can be reduced by hydrogen in metal powders 0.40 <![CDATA[Hydrogen Loss (H2-Loss)]]> GB / T5158.2 2011 Determination of mass loss of metal powders during reduction in hydrogen 0.40
[0046] In addition, the iron powder contains ≥0.21wt% of unknown impurities.
[0047] 2. Multi-element: The “multi-element” mentioned in the present invention refers to “binary”, “ternary” and “quaternary”.
[0048] 3. Eutectic combustion synthesis: Since part of the iron powder and the additive form an eutectic, the eutectic point of the eutectic is much lower than the melting point of the iron powder and the additive. After the iron powder is ignited, when the temperature of the iron powder in the combustion process is higher than the eutectic point of the eutectic, the iron powder and the additive will begin to decompose and melt, thereby welding the iron powder and the additive (or the metal oxide formed by the thermal decomposition of the additive) together to form a precursor, or the iron powder is coated on the surface of the additive to form a precursor. The precursor described in the present invention is multi-element.
[0049] 4. Combustion aid: The combustion aid in the present invention is a combustion aid that releases active oxygen due to thermal decomposition during the combustion of the alloy system. The combustion aid in the following embodiments is preferably potassium chlorate, potassium perchlorate, potassium permanganate, potassium nitrate, and sodium nitrate.
[0050] 5. The reducing agent does not burn or partially burns during the eutectic combustion synthesis process. When the reducing agent is one or more of carbon powder, charcoal powder and coke powder, and there is oxygen blocking in the closed space of the eutectic combustion reaction, the reducing agent partially burns.
[0051] 6. The method for preparing multi-component pre-alloyed powder of the present invention can be used to prepare multi-component pre-alloyed powder with an average particle size of less than or equal to 25 μm.
[0052] The technical solution of the present invention is further clearly and completely described below in conjunction with the embodiments, wherein the raw materials and preparation raw materials used in the embodiments of the present invention are commercially available.
[0053] Example 1
[0054] A method for preparing multi-element pre-alloyed powder based on ferrothermal reaction specifically comprises the following steps:
[0055] Step S1: fully mix iron powder and copper oxide to obtain an alloy system, then continue to add carbon powder and combustion aid to the alloy system and fully mix to obtain a mixture; wherein the mass of iron powder is 70% of the mass of the alloy system, and the iron powder is composed of high-purity iron powder with an average particle size of 1-15μm and iron powder with an average particle size of 30μm-200 mesh, and the mass of high-purity iron powder with an average particle size of 1-15μm is 10% of the mass of the alloy system; the average particle size of copper oxide is 1-15μm, and the mass of copper oxide is 30% of the mass of the alloy system; the average particle size of carbon powder is 325-500 mesh, and its mass is 10% of the mass of iron powder; the combustion aid is one of potassium chlorate, potassium perchlorate, potassium permanganate, potassium nitrate, and sodium nitrate, and its mass is 5% of the mass of the alloy system. The carbon powder in this embodiment can be charcoal powder and coke powder.
[0056] Step S2: Add the mixture obtained in step S1 to a burner with a stirring function, ignite the high-purity iron powder to ignite the iron powder, and cause the iron powder and copper oxide to undergo eutectic combustion synthesis, and obtain a FeCu binary precursor containing metal oxides after the combustion is completed. The temperature of the mixture obtained by fully mixing the alloy system is as high as 800-1100°C during the combustion process, the surface of the copper oxide melts and welds to the surface of the iron powder, and the FeCu binary precursor is first formed; in addition, the heat released during the combustion of the mixture prompts the carbon powder to reduce part of the metal oxide in the FeCu binary precursor, and obtain a FeCu binary precursor composed of metal oxides and FeCu binary pre-alloyed powder.
[0057] Step S3: The FeCu binary precursor obtained in step S2 is first placed in a ball mill for crushing for 30-60 minutes, and then the crushed FeCu binary precursor is placed in a hydrogen reduction furnace, and the metal oxides in the FeCu binary precursor are reduced with hydrogen at 350-750° C., and finally a high-purity FeCu binary pre-alloyed powder is obtained.
[0058] Example 2
[0059] High-purity FeCu binary pre-alloyed powders with different iron and copper mass ratios were prepared according to the method described in Example 1. The difference from Example 1 is that no combustion aid is added in this embodiment, the mass of the iron powder in this embodiment is 98% of the mass of the alloy system, wherein the mass of the high-purity iron powder with an average particle size of 1-15 μm in the iron powder is 50% of the mass of the alloy system; the average particle size of copper oxide is 1-15 μm, and the mass of copper oxide is 2% of the mass of the alloy system; the mass of carbon powder is 66.5% of the mass of iron powder.
[0060] Example 3
[0061] High-purity FeCu binary pre-alloyed powders with different iron and copper mass ratios were prepared according to the method described in Example 1. The difference from Example 1 is that no combustion aid is added in this embodiment, the mass of the iron powder in this embodiment is 90% of the mass of the alloy system, wherein the mass of the high-purity iron powder with an average particle size of 1-15 μm in the iron powder is 50% of the mass of the alloy system; the average particle size of the copper oxide is 1-15 μm, and the mass of the copper oxide is 10% of the mass of the alloy system; the mass of the carbon powder is 66% of the mass of the iron powder.
[0062] Example 4
[0063] High-purity FeCu binary pre-alloyed powders with different iron and copper mass ratios were prepared according to the method described in Example 1. The difference from Example 1 is that the mass of the iron powder in this example is 80% of the mass of the alloy system material, the mass of the high-purity iron powder with an average particle size of 1-15 μm in the iron powder is 40% of the mass of the alloy system material; the average particle size of the copper oxide is 1-15 μm, and the mass of the copper oxide is 20% of the mass of the alloy system material; the mass of the carbon powder is 32% of the mass of the iron powder.
[0064] Example 5
[0065] High-purity FeCu binary pre-alloyed powders with different iron and copper mass ratios were prepared according to the method described in Example 1. The difference from Example 1 is that: no combustion aid is added in this embodiment, the mass of the iron powder in this embodiment is 87.7% of the mass of the alloy system material, the mass of the high-purity iron powder with an average particle size of 1-15 μm in the iron powder is 68% of the mass of the alloy system material; the average particle size of copper oxide is 1-15 μm, and the mass of copper oxide is 12.3% of the mass of the alloy system material; the mass of carbon powder is 46% of the mass of iron powder.
[0066] Example 6
[0067] High-purity FeZn binary pre-alloyed powder was prepared according to the method described in Example 1. The difference from Example 1 is that: no combustion aid was added in this example, and iron powder and zinc oxide powder were used to prepare FeZn binary pre-alloyed powder; wherein, the mass of the iron powder in this example was 87% of the mass of the alloy system, and the mass of the high-purity iron powder with an average particle size of 1-15 μm in the iron powder was 68% of the mass of the alloy system; the average particle size of zinc oxide was 1-15 μm, and the mass of zinc oxide was 13% of the mass of the alloy system; the mass of carbon powder was 22% of the mass of iron powder.
[0068] Example 7
[0069] High-purity FeZn binary pre-alloyed powder was prepared according to the method described in Example 1. The difference from Example 1 is that: no combustion aid was added in this example, and iron powder and zinc powder were used to prepare FeZn binary pre-alloyed powder in this example; wherein, the mass of the iron powder in this example was 87% of the mass of the alloy system material, and the mass of the high-purity iron powder with an average particle size of 1-15 μm in the iron powder was 68% of the mass of the alloy system material; the average particle size of the zinc powder was 1-15 μm, and the mass of the zinc powder was 13% of the mass of the alloy system material; the mass of the carbon powder was 46% of the mass of the iron powder.
[0070] Example 8
[0071] High-purity FeNi binary pre-alloyed powder was prepared according to the method described in Example 1. The difference from Example 1 is that iron powder and nickel carbonate were used to prepare FeNi binary pre-alloyed powder in this embodiment; wherein the mass of iron powder in this embodiment is 66.4% of the mass of the alloy system, the mass of high-purity iron powder with an average particle size of 1-15 μm in the iron powder is 52% of the mass of the alloy system; the mass of nickel carbonate (NiCO3) is 33.6% of the mass of the alloy system; the mass of carbon powder is 46% of the mass of iron powder; the combustion aid is one of potassium chlorate, potassium perchlorate, potassium permanganate, potassium nitrate, and sodium nitrate, and its mass is 3% of the mass of the alloy system.
[0072] Example 9
[0073] High-purity FeCo binary pre-alloyed powder was prepared according to the method described in Example 1. The difference from Example 1 is that in this embodiment, iron powder and cobalt carbonate are used to prepare FeCo binary pre-alloyed powder; wherein, the mass of iron powder in this embodiment is 66.4% of the mass of the alloy system, the mass of high-purity iron powder with an average particle size of 1-15 μm in the iron powder is 53% of the mass of the alloy system; the mass of cobalt carbonate (CoCO3) is 33.6% of the mass of the alloy system; the mass of carbon powder is 46% of the mass of iron powder; the combustion aid is one of potassium chlorate, potassium perchlorate, potassium permanganate, potassium nitrate, and sodium nitrate, and its mass is 3% of the mass of the alloy system.
[0074] Example 10
[0075] High-purity FeCu binary pre-alloyed powder was prepared according to the method described in Example 1. The difference from Example 1 is that: no combustion aid was added in this embodiment, and iron powder and basic copper carbonate were used to prepare FeCu binary pre-alloyed powder in this embodiment; wherein, the mass of iron powder in this embodiment was 72% of the mass of the alloy system material, the mass of high-purity iron powder with an average particle size of 1-15 μm in the iron powder was 53% of the mass of the alloy system material; the mass of basic copper carbonate (Cu2(OH)2CO3) was 28% of the mass of the alloy system material; the mass of carbon powder was 46% of the mass of iron powder.
[0076] Embodiment 11
[0077] High-purity FeNi binary pre-alloyed powder is prepared according to the method described in Example 1. The difference from Example 1 is that: no combustion aid is added in this embodiment, and iron powder and zinc oxide powder are used to prepare FeNi binary pre-alloyed powder in this embodiment; wherein, the mass of iron powder in this embodiment is 87% of the mass of the alloy system, and the mass of high-purity iron powder with an average particle size of 1-15μm in the iron powder is 80% of the mass of the alloy system; the average particle size of nickel oxide is 150-180 mesh, and the mass of nickel oxide is 13% of the mass of the alloy system; the mass of carbon powder is 22% of the mass of iron powder. Since the melting point of nickel oxide is higher than that of iron powder and its average particle size is also larger, when iron powder and nickel oxide undergo eutectic combustion synthesis, the iron powder with an average particle size of 1-15μm melts first relative to nickel oxide, and is coated on the surface of nickel oxide under the action of heat.
[0078] Example 12
[0079] High-purity FeCuNi ternary pre-alloyed powder was prepared according to the method described in Example 1. The difference from Example 1 is that in this embodiment, iron powder, copper oxide and nickel carbonate are used to prepare FeCuNi ternary pre-alloyed powder, wherein the mass of the iron powder in this embodiment is 76% of the mass of the alloy system, and the mass of the high-purity iron powder with an average particle size of 1-15 μm in the iron powder is 68% of the mass of the alloy system; the average particle size of copper oxide is 1-15 μm, and the mass of copper oxide is 9.7% of the mass of the alloy system; the mass of nickel carbonate is 14.3% of the mass of the alloy system, and the mass of carbon powder is 32% of the mass of iron powder; the combustion aid is one of potassium chlorate, potassium perchlorate, potassium permanganate, potassium nitrate and sodium nitrate, and its mass is 3% of the mass of the alloy system.
[0080] Embodiment 13
[0081] The high-purity FeCuCo ternary pre-alloyed powder is prepared according to the method described in Example 1. The difference from Example 1 is that in this embodiment, iron powder, copper oxide and cobalt carbonate are used to prepare FeNiCo ternary pre-alloyed powder, wherein the mass of the iron powder in this embodiment is 78% of the mass of the alloy system, and the mass of the high-purity iron powder with an average particle size of 1-15μm in the iron powder is 68% of the mass of the alloy system; the average particle size of the copper oxide is 1-15μm, and the mass of the copper oxide is 10.3% of the mass of the alloy system; the mass of the cobalt carbonate is 11.7% of the mass of the alloy system, and the mass of the carbon powder is 32% of the mass of the iron powder; the combustion aid is one of potassium chlorate, potassium perchlorate, potassium permanganate, potassium nitrate and sodium nitrate, and its mass is 4% of the mass of the alloy system.
[0082] Embodiment 14
[0083] High-purity FeNiCo ternary pre-alloyed powder is prepared according to the method described in Example 1. The difference from Example 1 is that in this embodiment, iron powder, nickel carbonate and cobalt carbonate are used to prepare FeNiCo ternary pre-alloyed powder, wherein the mass of the iron powder in this embodiment is 78% of the mass of the alloy system, the mass of the high-purity iron powder with an average particle size of 1-15 μm in the iron powder is 68% of the mass of the alloy system; the mass of nickel carbonate is 10.3% of the mass of the alloy system; the mass of cobalt carbonate is 11.7% of the mass of the alloy system, and the mass of carbon powder is 32% of the mass of iron powder; the combustion aid is one of potassium chlorate, potassium perchlorate, potassium permanganate, potassium nitrate and sodium nitrate, and its mass is 5% of the mass of the alloy system.
[0084] Embodiment 15
[0085] According to the method described in Example 1, a high-purity FeNiCuSn quaternary pre-alloyed powder is prepared into a FeNiCuSnP alloy powder after being phosphated. Different from Example 1, in this embodiment, iron powder, nickel carbonate, copper oxide, and tin oxide are first selected to prepare FeNiCuSn quaternary pre-alloyed powder, and then the FeNiCuSn quaternary pre-alloyed powder is phosphated to obtain FeNiCuSnP alloy powder; wherein, the mass of the iron powder in this embodiment is 39.3% of the mass of the alloy system, and the mass of the high-purity iron powder with an average particle size of 1-15μm in the iron powder is 18% of the mass of the alloy system; the mass of copper oxide is 15.2% of the mass of the alloy system, and the mass of nickel carbonate is 30.2% of the mass of the alloy system; the mass of tin oxide is 15.3% of the mass of the alloy system, and the mass of carbon powder is 38% of the mass of the iron powder; the combustion aid is one of potassium chlorate, potassium perchlorate, potassium permanganate, potassium nitrate, and sodium nitrate, and its mass is 5% of the mass of the alloy system.
[0086] Example 16
[0087] High-purity FeZn binary pre-alloyed powders with different iron and zinc mass ratios were prepared according to the method described in Example 1. The difference from Example 1 is that: no combustion aid is added in this embodiment, the mass of the iron powder in this embodiment is 92% of the mass of the alloy system, the mass of the high-purity iron powder with an average particle size of 19-28μm in the iron powder is 88% of the mass of the alloy system; the average particle size of zinc oxide is 40μm-200 mesh, and the mass of zinc oxide is 8% of the mass of the alloy system; the mass of carbon powder is 10% of the mass of iron powder.
[0088] Embodiment 17
[0089] High-purity FeCu binary pre-alloyed powders with different iron and copper mass ratios were prepared according to the method described in Example 1. The difference from Example 1 is that no combustion aid is added in this embodiment, the mass of the iron powder in this embodiment is 90% of the mass of the alloy system, wherein the mass of the iron powder with an average particle size of 19-28 μm is 88% of the mass of the alloy system; the average particle size of copper oxide is 1-15 μm, and the mass of copper oxide is 10% of the mass of the alloy system; the mass of carbon powder is 66% of the mass of iron powder.
[0090] Embodiment 18
[0091] High-purity FeCuCo ternary pre-alloyed powder is prepared according to the method described in Example 1. Different from Example 1, in this embodiment, iron powder, copper oxide and cobalt carbonate are used to prepare FeNiCo ternary pre-alloyed powder, wherein the mass of iron powder in this embodiment is 81% of the mass of the alloy system, the mass of high-purity iron powder with an average particle size of 1-15μm in the iron powder is 68% of the mass of the alloy system; the mass of copper oxide is 12% of the mass of the alloy system; the mass of cobalt carbonate is 7% of the mass of the alloy system, and the mass of carbon powder is 32% of the mass of iron powder; the combustion aid is one of potassium chlorate, potassium perchlorate, potassium permanganate, potassium nitrate and sodium nitrate, and its mass is 5% of the mass of the alloy system.
[0092] Embodiment 19
[0093] According to the method described in Example 1, a FeCuSnP alloy powder after phosphating high-purity FeCuSn ternary pre-alloyed powder is prepared. Different from Example 1, in this embodiment, iron powder, copper oxide, and tin oxide are first selected to prepare FeCuSn ternary pre-alloyed powder, and then the FeCuSn ternary pre-alloyed powder is phosphated to obtain FeCuSnP ternary pre-alloyed powder. Among them, the mass of iron powder in this embodiment is 88% of the mass of the alloy system, and the average particle size of the iron powder is 1-15μm. The mass of high-purity iron powder is 65% of the mass of the alloy system; the mass of copper oxide is 10.8% of the mass of the alloy system, the mass of tin oxide is 1.2% of the mass of the alloy system, and the mass of carbon powder is 38% of the mass of iron powder; the combustion aid is one of potassium chlorate, potassium perchlorate, potassium permanganate, potassium nitrate, and sodium nitrate, and its mass is 5% of the mass of the alloy system.
[0094] The FeCuSnP ternary pre-alloyed powder prepared in this embodiment has an average particle size of 20-35 microns and an oxygen content of 2000-7000 PPM. The mass contents of Fe, Cu, Sn and P in the ternary pre-alloyed powder are 87-88%, 10-11%, 0.7-1% and 1-1.2% respectively.
[0095] Embodiment 20
[0096] According to the method described in Example 1, a FeCuSnP alloy powder after phosphating high-purity FeCuSn ternary pre-alloyed powder is prepared. Different from Example 1, in this embodiment, iron powder, copper oxide, and tin oxide are first selected to prepare FeCuSn ternary pre-alloyed powder, and then the FeCuSnP ternary pre-alloyed powder is obtained by phosphating the FeCuSn ternary pre-alloyed powder. Among them, the mass of iron powder in this embodiment is 82.7% of the mass of the alloy system, and the mass of high-purity iron powder with an average particle size of 1-15μm in the iron powder is 65% of the mass of the alloy system; the mass of copper oxide is 15.2% of the mass of the alloy system, the mass of tin oxide is 2.1% of the mass of the alloy system, and the mass of carbon powder is 14.5% of the mass of iron powder; the combustion aid is one of potassium chlorate, potassium perchlorate, potassium permanganate, potassium nitrate, and sodium nitrate, and its mass is 5% of the mass of the alloy system.
[0097] The FeCuSnP ternary pre-alloyed powder prepared in this embodiment has an average particle size of 20-35 microns and an oxygen content of 2000-7000 PPM. The contents of Fe, Cu, Sn and P in the ternary pre-alloyed powder are 82-85%, 14-15%, 1.5-2.2% and 1-1.2% respectively.
[0098] Embodiment 21
[0099] According to the method described in Example 1, a FeCuSnP alloy powder after phosphating high-purity FeCuSn ternary pre-alloyed powder is prepared. Different from Example 1, in this embodiment, iron powder, copper oxide, and tin oxide are first selected to prepare FeCuSn ternary pre-alloyed powder, and then the FeCuSnP ternary pre-alloyed powder is obtained by phosphating the FeCuSn ternary pre-alloyed powder. Among them, the mass of iron powder in this embodiment is 63% of the mass of the alloy system, and the mass of high-purity iron powder with an average particle size of 1-15μm in the iron powder is 48% of the mass of the alloy system; the mass of copper oxide is 32% of the mass of the alloy system, the mass of tin oxide is 5% of the mass of the alloy system, and the mass of carbon powder is 14.5% of the mass of iron powder; the combustion aid is one of potassium chlorate, potassium perchlorate, potassium permanganate, potassium nitrate, and sodium nitrate, and its mass is 5% of the mass of the alloy system.
[0100] The FeCuSnP ternary pre-alloyed powder prepared in this embodiment has an average particle size of 20-35 microns and an oxygen content of 2000-7000 PPM. The contents of Fe, Cu, Sn and P in the ternary pre-alloyed powder are 62-65%, 31-32%, 4-5% and 0.7-1% respectively.
[0101] Embodiment 22
[0102] The FeCuSnP ternary pre-alloyed powder prepared in Example 19 is prepared together with diamond into a diamond tool matrix. The preparation method of the diamond tool matrix specifically comprises the following steps:
[0103] Step 1: Wetting diamond with liquid paraffin and mixing it with the FeCuSnP ternary pre-alloyed powder prepared in Example 19 for 30-60 minutes to obtain a mixture containing diamond; wherein the mass fraction of diamond in the mixture is 1-3%, and the mass fraction of the FeCuSnP ternary pre-alloyed powder is 95-99%.
[0104] Step 2: Feed the mixture obtained in step 1 into a cold press at a pressure of 0.5t-1.5t / cm 2 Under the conditions of , it is pressed into a cutter head blank.
[0105] Step 3: hot press the blank obtained in step 2 at a temperature of 750-850°C, a holding time of 90s, and a hydraulic pressure of 250kgf / cm 2 Hot pressing sintering is carried out under conditions of , and the diamond tool matrix is obtained after hot pressing sintering is completed and cooled.
[0106] The performance test of the diamond tool matrix prepared in this embodiment is carried out. The hardness of the diamond tool matrix prepared in this embodiment is 95-102HRB, the bending strength is 1000-1400Mpa, the density is 95-98%, and the deflection is 0.7-1.2mm.
[0107] At the same time, the diamond tool matrix prepared in this embodiment is made into a diamond water drill, and the water drill is used to drill and cut C35 threaded steel. The drilling and cutting data of the water drill are shown in Table 2.
[0108] Embodiment 23
[0109] The FeCuSnP ternary pre-alloyed powder prepared in Example 19 was prepared together with diamond to form a diamond tool matrix according to the preparation method of the diamond tool matrix in Example 22. The difference from Example 22 is that the hot pressing sintering temperature is 890-910°C, the holding time is 60-120min, and the hot pressing pressure is 20-70kgf / cm 2 .
[0110] The performance test of the diamond tool matrix prepared in this embodiment is carried out. The hardness of the diamond tool matrix prepared in this embodiment is 88-94HRB, the tooth resistance is 9-12N.M, and the density is 94-96%.
[0111] Meanwhile, the diamond tool matrix prepared in this embodiment was made into a diamond stone saw blade, and the saw blade was used to cut South African black and 635# granite. The cutting data of the saw blade is shown in Table 2.
[0112] Embodiment 24
[0113] The FeCuSnP ternary pre-alloyed powder prepared in Example 20 was prepared together with diamond to form a diamond tool matrix according to the preparation method of the diamond tool matrix in Example 22. The difference from Example 22 is that the hot pressing sintering temperature is 890-910°C, the holding time is 60-120min, and the hot pressing pressure is 20-70kgf / cm 2 .
[0114] The performance test of the diamond tool matrix prepared in this embodiment is carried out. The hardness of the diamond tool matrix prepared in this embodiment is 94-102HRB, the tooth resistance strength is 9-12N.M, and the density is 94-96%.
[0115] Meanwhile, the diamond tool matrix prepared in this embodiment is made into a diamond stone saw blade, and the saw blade is used to cut 635# granite. The cutting data of the saw blade is shown in Table 2.
[0116] Embodiment 25
[0117] The FeCuSnP ternary pre-alloyed powder prepared in Example 21 was combined with diamond to form a diamond tool matrix according to the preparation method of the diamond tool matrix in Example 22. The difference from Example 22 is that: 810-820°C, holding time 60-90min, hot pressing pressure 20-70kgf / cm 2 .
[0118] The performance test of the diamond tool matrix prepared in this embodiment is carried out. The hardness of the diamond tool matrix prepared in this embodiment is 75-85HRB, the tooth resistance strength is 7-9N.M, the density is 94-96%, and the deflection is 0.7-1.2mm.
[0119] At the same time, the diamond tool matrix prepared in this embodiment is made into a diamond ceramic saw blade, and the saw blade is used to cut glazed tiles and full ceramic tiles. The cutting data of the saw blade is shown in Table 2.
[0120] Embodiment 26
[0121] The FeCuSnP ternary pre-alloyed powder prepared in Example 21 and diamond were used to prepare a diamond tool matrix according to the preparation method of the diamond tool matrix in Example 22. The difference from Example 22 is that the hot pressing sintering temperature is 750-770°C, the holding time is 90s, and the hot pressing pressure is 250kgf / cm 2 .
[0122] The performance test of the diamond tool matrix prepared in this embodiment is carried out. The hardness of the diamond tool matrix prepared in this embodiment is 90-96HRB, the bending strength is 1200Mpa, and the density is 95-98%.
[0123] Meanwhile, the diamond tool matrix prepared in this embodiment is made into a diamond water drill, and the water drill is used to drill and cut hard pebbles. The cutting data of the water drill is shown in Table 2.
[0124] Test analysis:
[0125] 1. Analysis of the FeCu binary pre-alloyed powder prepared in Example 5
[0126] The FeCu binary pre-alloyed powder prepared in Example 5 was subjected to X-ray energy spectrum analysis (EDS) and the results are as follows: Figure 1 shown.
[0127] The FeCu binary pre-alloyed powder prepared in Example 5 was subjected to scanning electron microscope (SEM) spectrum analysis, and the results are as follows: Figure 2 shown.
[0128] The FeCu binary pre-alloyed powder prepared in Example 5 was subjected to metallographic analysis, and the results are as follows: Figure 3 shown.
[0129] Combination Figure 1-3 The FeCu binary pre-alloyed powder prepared by the method of the present invention was analyzed. Figure 1 EDS analysis is a qualitative analysis. Elements with a mass percentage of less than 1% are usually considered impurities. Figure 1 It can be seen that the FeCu binary pre-alloyed powder prepared by the present invention contains only two elements, iron and copper. In addition, the EDS analysis test is performed at random on one point. Figure 1 It can be seen from the table that the mass fraction of copper in the FeCu binary alloy is 10.11% and the mass fraction of iron is 90.42%, which are close to the mass fractions of copper and iron in the FeCu binary alloy prepared in Example 5. Therefore, it is preliminarily judged that the copper in the FeCu binary pre-alloyed powder is uniformly distributed in the iron powder.
[0130] from Figure 2 It can be seen that some fine particles are adhered to the surface of the iron powder. This is because the melting points of copper and elemental copper are lower than those of iron powder and iron oxide powder. During the eutectic combustion synthesis process, copper is melted and welded to the iron powder. Figure 2 It can be clearly seen from the SEM image that copper is evenly welded on the surface of the iron powder.
[0131] Figure 3The metallographic diagram of the FeCu binary pre-alloyed powder prepared by the present invention after being corroded is shown in FIG. Figure 3 It can be clearly seen that the copper is evenly distributed in the iron powder, which further proves that the copper in the FeCu binary pre-alloyed powder is evenly distributed in the iron powder.
[0132] In summary, from Figure 1-3 It can be concluded that when the FeCu binary pre-alloyed powder is prepared by the method described in the present invention, since the molten copper liquid is directly welded on the iron powder and the copper is evenly distributed in the iron powder, the FeNi binary pre-alloyed powder prepared by the preparation method described in the present invention does not have segregation phenomenon and has a high degree of alloying.
[0133] 2. Analysis of the FeNi binary pre-alloyed powder prepared in Example 8
[0134] The FeNi binary pre-alloyed powder prepared in Example 8 was subjected to X-ray energy spectrum analysis (EDS) and the results are as follows: Figure 4 shown.
[0135] The FeNi binary pre-alloyed powder prepared in Example 8 was subjected to scanning electron microscope (SEM) spectrum analysis, and the results are as follows: Figure 5 shown.
[0136] The FeNi binary pre-alloyed powder prepared in Example 8 was subjected to metallographic spectrum analysis, and the results are as follows: Figure 6 shown.
[0137] Combination Figure 4-6 The FeNi binary pre-alloyed powder prepared by the method of the present invention was analyzed. Figure 4 It is EDS analysis. Figure 4 It can be seen that the FeNi binary pre-alloyed powder prepared by the present invention contains only two elements, iron and nickel. In addition, the EDS analysis test is performed on a certain point at random. Figure 4 It can be seen from the table that the mass fraction of nickel in the FeNi binary alloy is 21.03% and the mass fraction of iron is 78.97%, which are close to the mass fractions of nickel and iron in the FeNi binary alloy prepared in Example 8. Therefore, it is preliminarily judged that the nickel in the FeNi binary pre-alloyed powder is uniformly distributed in the iron powder.
[0138] from Figure 5It can be seen that the iron powder and nickel in the FeNi binary pre-alloyed powder are welded together. This is because iron and nickel belong to the same main group elements and their melting points are relatively close. Therefore, in the process of eutectic combustion synthesis, the surface of the iron powder and the surface of NiO (nickel oxide) formed by high-temperature decomposition of nickel carbonate (NiCO3) melt, thereby welding the iron powder and nickel oxide together, and then successively reducing them with high-temperature carbon powder and hydrogen to obtain the FeNi binary alloy powder in which the iron powder and metallic nickel are welded together.
[0139] Figure 6 The metallographic diagram of the FeNi binary pre-alloy powder prepared by the present invention after corrosion. Since iron and nickel belong to the same main group elements, the two have good mutual solubility. Therefore, there is only a difference in color depth between the two after melting. Figure 6 It can be seen that the color distribution of the metallographic phase diagram of the FeNi binary alloy is uniform, which further proves that nickel is evenly distributed in the iron powder.
[0140] In summary, from Figure 4-6 It can be concluded that when the FeNi binary pre-alloyed powder is prepared by the method described in the present invention, since the iron powder and the metallic nickel are welded together and the metallic nickel is evenly distributed in the iron powder, there is no segregation phenomenon in the FeNi binary pre-alloyed powder prepared by the preparation method described in the present invention.
[0141] 3. Analysis of the FeNiCuSnP alloy powder after phosphating the FeNiCuSn quaternary pre-alloyed powder prepared in Example 15
[0142] The FeNiCuSnP alloy powder after phosphating the FeNiCuSn quaternary pre-alloy powder prepared in Example 15 was subjected to X-ray energy spectrum analysis (EDS) and the results are as follows: Figure 7 shown.
[0143] The FeNiCuSnP alloy powder after phosphating the FeNiCuSn quaternary pre-alloyed powder prepared in Example 15 was subjected to scanning electron microscope (SEM) spectrum analysis, and the results are as follows: Figure 8 shown.
[0144] The FeNiCuSnP alloy powder after phosphating the FeNiCuSn quaternary pre-alloy powder prepared in Example 15 was subjected to metallographic spectrum analysis, and the results are as follows: Fig. 9 shown.
[0145] Combination Figure 7-9 The FeNiCuSnP alloy powder prepared by the method of the present invention was analyzed. Figure 7 It is EDS analysis. Figure 7It can be seen that the FeNiCuSnP alloy powder prepared by the present invention contains only five elements, namely, iron, nickel, copper, tin and phosphorus. In addition, the EDS analysis test is performed at random on a certain point. Figure 7 It can be seen from the table that the mass fraction of phosphorus (P) in the FeNiCuSnP quinary alloy is 1.99%, the mass fraction of iron (Fe) is 58.52%, the mass fraction of nickel (Ni) is 19.38%, the mass fraction of copper (Cu) is 18.2%, and the mass fraction of tin (Sn) is 1.91%. Therefore, it is preliminarily judged that the nickel, copper and tin in the FeNiCuSnP alloy powder are evenly distributed in the iron powder.
[0146] from Figure 8 It can be seen that the average particle size of the FeNiCuSnP alloy powder is small, at the micron level.
[0147] Fig. 9 The metallographic diagram of the FeNiCuSnP alloy powder prepared by the present invention after being corroded is shown in FIG. Fig. 9 It can be seen that copper, nickel and tin in the FeNiCuSnP alloy powder are evenly distributed in the iron powder.
[0148] In summary, from Figure 7-9 It can be concluded that the FeNiCuSnP alloy powder prepared by the preparation method of the present invention does not have the segregation phenomenon.
[0149] 4. The FeCuCo ternary pre-alloyed powder prepared in Example 18 was analyzed. Fig.10 It can be seen that during the eutectic combustion synthesis process of iron powder, copper oxide and cobalt carbonate, it can be clearly seen that the iron powder with an average particle size of less than 30μm is welded on other materials with a larger average particle size.
[0150] 5. The diamond tool matrix prepared in Examples 22-26 was made into different diamond tools and used in different scenarios. The test data of the application is shown in Table 2.
[0151] Table 2 Test data of different diamond tools in different application scenarios
[0152]
[0153]
[0154] The present invention seems simple, but it is not easy to think of. Only by conducting in-depth experiments and research on the characteristics and properties of iron powder with an average particle size of less than 30μm, and on this basis, continuously combining the self-propagating high-temperature synthesis method with practice, can the best solution be obtained, thereby solving a major problem in the industry. The present invention utilizes the extremely strong flammability of iron powder with an average particle size of less than 30μm. After ignition, the iron powder with an average particle size of less than 30μm releases a large amount of iron heat, allowing the iron powder and the additive to undergo eutectic combustion synthesis, so that the iron powder and the additive surface are welded together or the iron powder is coated on the additive surface, thereby obtaining a precursor with a high degree of alloying, uniform composition, no segregation, and containing metal oxides. After the metal oxides in the precursor are fully reduced, a multi-component pre-alloyed powder is obtained, which solves the problems of segregation, large average particle size, and environmental unfriendliness of the multi-component pre-alloyed powder prepared by the prior art.
[0155] Furthermore, when the method of the present invention is used to prepare the precursor, the precursor of the present invention can be obtained by only igniting the alloy system, and no additional heat source is required in the whole process, thereby reducing the preparation cost of the multi-component pre-alloyed powder. In addition, the diamond knife made by combining the multi-component pre-alloyed powder prepared by the present invention with diamond has a longer service life and less wear, and can be used to cut harder pebbles.
[0156] The above descriptions are only some embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing multi-component pre-alloyed powder based on ferrothermal reaction, characterized in that: The following steps are involved: Step S1: prepare an alloy system containing iron powder and additives; the mass of the iron powder is not less than 50% of the mass of the alloy system; the additive is any one or more of metal oxides, metal salts and metal element powders, and the mass of the additive is 1%-50% of the mass of the alloy system; when the additive is metal oxide or metal element powder, the average particle size is less than 200 mesh or less than or equal to 30μm, and the metal element powder is any one or more of copper, zinc, cobalt, nickel and aluminum, and the metal oxide is any one or more of CuO, ZnO, CoO, Co2O3, Co3O4, NiO and Ni2O3; when the additive is a metal salt, the metal salt is any one or more of NiCO3, CoCO3, CuCO3, Cu2(OH)2CO3, Ni2(OH)2CO3, Co2(OH)2CO3, CoC2O4, CuC2O4 and NiC2O4; Step S2: After fully mixing the alloy system material and the reducing agent, perform eutectic combustion synthesis to weld the iron powder and the additive surface together to obtain a precursor containing metal oxides; wherein the igniter is high-purity iron powder contained in the iron powder, the mass of the high-purity iron powder is not less than 10% of the mass of the alloy system material, and the average particle size is less than 30 μm; the reducing agent is used to reduce part of the metal oxides in the precursor; in this step, the mass of the reducing agent is 15%-66.7% of the mass of the iron powder, and the reducing agent is selected from any one or more of carbon powder, charcoal powder and coke powder with an average particle size of 325-500 mesh; Step S3: reducing the metal oxides in the precursor using a reducing gas at a reduction temperature of 350-750° C. to obtain a multi-element pre-alloyed powder.
2. The method for preparing multi-component pre-alloyed powder based on ferrothermal reaction according to claim 1, characterized in that: In the step S2, the alloy system undergoes eutectic combustion synthesis in a burner with a stirring function.
3. The method for preparing multi-component pre-alloyed powder based on ferrothermal reaction according to claim 2, characterized in that: The reduction time in step S3 is 6-8 hours, and the precursor is first crushed before reduction, and the processing time is 30-60 minutes.
4. A method for preparing multi-component pre-alloyed powder based on ferrothermal reaction according to any one of claims 1 to 3, characterized in that: In the step S2, a combustion aid is added to increase the rate of eutectic combustion synthesis of iron powder and additives; the mass of the combustion aid is 1%-5% of the mass of the alloy system.
5. A method for preparing a diamond tool matrix, characterized in that: The multi-element pre-alloyed powder prepared by the method according to any one of claims 1 to 4 is mixed with diamond and then sintered to form a diamond tool matrix.
Citation Information
Patent Citations
Method for preparing nano aluminum-copper-iron quasicrystal powder
CN101758237A
Preparation method of prealloying powder for dispersion strengthening metal by low-temperature combustion synthesis method
CN101956119A