Negative electrode sheet, lithium metal battery and electronic device containing the negative electrode sheet
By adding a piezoelectric layer to the negative electrode sheet of the lithium metal battery to form an orderly polarization electric field, the dendrite problem caused by uneven lithium ion deposition is solved, and the circulation and safety performance of the lithium metal battery is significantly improved.
Patent Information
- Application Number
- CN202180004984.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-31
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-03-31
AI Technical Summary
During the charging process, the dendrite structure is formed due to uneven lithium ion deposition during lithium-ion, which limits the battery's efficiency, cycle life and safety performance. Sharp dendrites may pierce the diaphragm and cause short-circuit safety problems.
A negative electrode sheet is used, which includes a negative current collector and a piezoelectric layer. The piezoelectric layer has a polarized electric field, and the polarized electric field direction points from the current collector to the surface of the negative electrode. The orderly polarized electric field is formed using piezoelectric polymer, ceramic or single crystal material. , induce the orderly deposition of lithium metal, inhibit dendrites' growth, and control the dispersion of lithium ions through the ratio of conductive material to piezoelectric material.
It effectively improves the circulation and safety performance of lithium metal batteries, prevents sharp dendrites from punctured by the diaphragm, and improves the lithium deposition morphology and the overall performance of the battery.
Smart Images

Figure BDA0003508255240000151 
Figure BDA0003508255240000161 
Figure BDA0003508255240000171
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium metal batteries, and in particular to a negative electrode plate, a lithium metal battery comprising the negative electrode plate, and an electronic device. Background Art
[0002] Lithium metal is the metal with the smallest relative atomic mass (6.94) and the lowest standard electrode potential (-3.045V) among all metal elements, and its theoretical gram capacity can reach 3860mAh / g. Therefore, using lithium metal as the negative electrode of the battery, combined with some high-energy-density positive electrode materials, can greatly improve the energy density of the battery and the operating voltage of the battery. However, if batteries with lithium metal as the negative electrode material are truly commercialized, cycle life and safety issues must be improved: 1) During the charging process of lithium metal batteries, lithium is deposited on the surface of the negative electrode current collector. Due to the weak lithium affinity of the current collector, lithium ions cannot nucleate uniformly and quickly, resulting in uneven lithium ion concentration at the negative electrode / electrolyte interface, making the current density distribution at the interface uneven, causing the deposition rate at the nucleation site to be too fast, forming a dendrite structure, which seriously limits the efficiency, cycle life and energy density of lithium metal batteries; 2) At the interface between the lithium metal negative electrode and the electrolyte, due to the interaction between the applied electric field and the lithium ion flow, an uneven liquid electric convection perpendicular to the negative electrode surface is formed, resulting in the deposition of lithium metal in the direction perpendicular to the current collector faster than in the direction parallel to the current collector, which is also an important factor in the formation of lithium dendrite structure; 3) In the liquid electrolyte system, the consumption rate of lithium ions is far less than the mass transfer rate in the electrolyte, resulting in the accumulation of lithium ions on the dendrite surface, forming a huge space charge layer and deposition barrier, which hinders the deposition of lithium ions at the root of the dendrite and makes the lithium dendrite sharper. Sharp lithium dendrites may pierce the diaphragm and directly contact the positive electrode to form a short circuit, causing serious safety problems.
[0003] Based on the above problems, there is an urgent need to find a method that can improve the lithium affinity of the negative electrode current collector, homogenize the current density distribution at the negative electrode / electrolyte interface, inhibit the generation of a space charge layer on the surface of deposited lithium, and inhibit the growth of lithium dendrites to improve the cycle performance and safety performance of lithium metal batteries. Summary of the invention
[0004] The purpose of the present application is to provide a negative electrode plate, a lithium metal battery and an electronic device comprising the negative electrode plate, so as to improve the cycle performance and safety performance of the lithium metal battery.
[0005] The first aspect of the present application provides a negative electrode plate, which includes a negative electrode current collector and a piezoelectric layer. The piezoelectric layer has a polarization electric field, and the direction of the polarization electric field is from the negative electrode current collector to the surface of the negative electrode. The material of the piezoelectric layer includes at least one of a piezoelectric polymer, a piezoelectric ceramic, a piezoelectric single crystal or an inorganic piezoelectric material.
[0006] In the present application, the piezoelectric layer is polarized so that the direction of the polarization electric field points from the negative electrode current collector to the surface of the negative electrode. The piezoelectric layer that has been subjected to directional polarization treatment has an ordered polarization electric field constructed inside. Macroscopically, the negative electrode surface can be negatively charged, thereby increasing the lithium metal deposition sites, reducing the lithium deposition overpotential, and making the lithium nucleus distribution more uniform; microscopically, the newly deposited lithium metal during charging will cause deformation to the piezoelectric layer. The lithium metal deposition brings strain and produces a piezoelectric effect, which reduces the polarization strength of the piezoelectric layer material, increases the potential at the deposition site, and induces subsequent lithium ions to preferentially deposit in undeposited areas to form planar growth, thereby improving the lithium deposition morphology and inhibiting lithium dendrites. In the present application, the term "strain" refers to the relative deformation of a local object under the action of factors such as external forces or non-uniform temperature fields. In the present application, "deposition overpotential" refers to the overpotential that provides thermodynamic energy for lithium metal nucleation deposition.
[0007] In the present application, the material of the piezoelectric layer includes at least one of a piezoelectric polymer, a piezoelectric ceramic, a piezoelectric single crystal or an inorganic piezoelectric material. By selecting the above materials to prepare a piezoelectric layer with a piezoelectric effect, a polarization electric field is present inside the piezoelectric layer, so as to use the direction of the electric field to induce orderly deposition of lithium metal, thereby preventing the generation of lithium dendrites. The material of the piezoelectric layer can be an elastic material, and the material of the elastic piezoelectric layer can buffer the volume change of the lithium metal negative electrode to a certain extent, thereby protecting the negative electrode. Preferably, the material of the piezoelectric layer includes any one of a piezoelectric polymer, a piezoelectric ceramic, a piezoelectric single crystal or an inorganic piezoelectric material, so that the material of the piezoelectric layer has consistency, and the electric field distribution inside the piezoelectric layer is more uniform, so that the lithium deposition is more uniform, so as to more effectively inhibit the growth of lithium dendrites. In the present application, the term "piezoelectric effect" means that when certain dielectrics are deformed by external forces in a certain direction, polarization will occur inside them, and opposite positive and negative charges will appear on their two opposite surfaces.
[0008] In general, the negative electrode plate provided by the present application includes a negative electrode current collector and a piezoelectric layer, wherein the piezoelectric layer has a polarization electric field, the direction of the polarization electric field is from the negative electrode current collector to the surface of the negative electrode, and the material of the piezoelectric layer includes at least one of a piezoelectric polymer, a piezoelectric ceramic, a piezoelectric single crystal or an inorganic piezoelectric material. The negative electrode plate can increase the lithium metal deposition sites, improve the deposition morphology, effectively inhibit the growth of lithium dendrites, greatly improve the cycle performance of lithium metal batteries, and avoid the presence of sharp lithium dendrites to pierce the isolation membrane and directly contact the positive electrode to form a short circuit, thereby improving the safety performance of lithium metal batteries.
[0009] In some embodiments of the first aspect of the present application, the room temperature coercive field strength Ec of the material of the piezoelectric layer satisfies: 0kV / mm<Ec<100kV / mm. For example, the lower limit of the room temperature coercive field strength Ec may include the following values: 1kV / mm, 10kV / mm, 20kV / mm, 30kV / mm or 40kV / mm; the upper limit of the room temperature coercive field strength Ec may include the following values: 50kV / mm, 60kV / mm, 70kV / mm, 80kV / mm, 90kV / mm or 99kV / mm. Without being limited to any theory, the room temperature coercive field strength Ec of the material of the piezoelectric layer is too high (for example, higher than 100kV / mm), the requirements for the piezoelectric material are too high, the available materials are few, and the polarization voltage of the material is high, the difficulty is great, and it will not significantly further improve the battery performance, and it is not suitable for practical applications. In the present application, the term "room temperature coercive field" refers to the electric field strength at room temperature that causes the polarization of the material to disappear in the electric field.
[0010] In some embodiments of the first aspect of the present application, those skilled in the art can understand that the intensity of the polarization electric field is selected based on the intensity Ec of the coercive field at room temperature of the material of the piezoelectric layer, and the intensity of the polarization electric field is preferably 0.1 to 6 times the intensity Ec of the coercive field at room temperature. For example, the lower limit of the intensity of the polarization electric field may include the following values: 0.1 times, 1 times, 2 times, 2.9 times or 3 times the intensity Ec of the coercive field at room temperature; the upper limit of the intensity of the polarization electric field may include the following values: 4 times, 5 times or 6 times the intensity Ec of the coercive field at room temperature. Without being limited to any theory, if the intensity of the polarization electric field is too low (for example, lower than 0.1 times the intensity Ec of the coercive field at room temperature), the polarization electric field will not be generated inside the piezoelectric layer; if the intensity of the polarization electric field is too high (for example, higher than 6 times the intensity Ec of the coercive field at room temperature), the material of the piezoelectric layer will be broken down and fail. By controlling the intensity of the polarization electric field within the above range, an ordered polarization electric field in a specific direction can be formed inside the piezoelectric layer, so that the surface of the negative electrode is negatively charged, thereby improving the lithium affinity of the negative electrode. At the same time, the piezoelectric effect of the piezoelectric layer is used to increase the potential at the deposition site, inducing lithium ions to deposit in the undeposited area, improving the lithium deposition morphology, and inhibiting the growth of lithium dendrites.
[0011] In some embodiments of the first aspect of the present application, there is no particular restriction on the type of piezoelectric polymer, as long as the purpose of the present application can be achieved. For example, the piezoelectric polymer may include polyvinylidene fluoride (PVDF), vinylidene fluoride / trifluoroethylene copolymer, vinylidene fluoride / tetrafluoroethylene copolymer, vinylidene dicyano / vinyl acetate copolymer (P(VDCN-VAC)), vinylidene dicyano / vinyl benzoate copolymer (P(VDCN-VBz)), vinylidene dicyano / vinyl propionate copolymer (P(VDCN-VPr)), vinylidene dicyano / vinyl neopentanoate copolymer (P(VDCN-VPiv)), vinylidene dicyano / methyl methacrylate copolymer (P(VDCN-MMA)), vinylidene dicyano / isobutylene copolymer (P(VDCN-IB)) or odd-numbered nylon-based piezoelectric polymer-(HN-(CH2) x -CO-) n -, etc., wherein x is an even number from 2 to 10, n is an integer from 90 to 400, when n is greater than 400, -(HN-(CH2) x -CO-) n -If the molecular weight is too large, the processing difficulty will increase sharply. In the present application, there is no particular restriction on the weight average molecular weight of the piezoelectric polymer, and those skilled in the art can select it according to the actual situation, as long as the purpose of the present application can be achieved.
[0012] In some embodiments of the first aspect of the present application, there is no particular limitation on the type of piezoelectric ceramics, as long as the purpose of the present application can be achieved. For example, piezoelectric ceramics may include barium titanate (BaTiO3), lead titanate (PbTiO3), lithium niobate (LiNbO3), lithium tantalate (LiNbO3), lead titanate zirconate (PbZrO3), and lead zirconate (PbZrO3). y Ti 1-y O3, lead magnesium niobate PbMg z Nb 1-z O3, Lead zinc niobate PbZn v Nb 1-v O3, lead manganese antimonate PbMn w Sb 1-w O3 or Pb 1-s M m (Zr t Ti 1-t ) 1-(s / 4) At least one of O3, etc., wherein 0<y<1, 0<z<1, 0<v<1, 0<w<1, 0<s<1, 0<m<1, 0<t<1, M is selected from any one of rare earth elements, and the rare earth elements include Y, La, Ce, Nd, Sm, Eu, Gd or Dy, etc.
[0013] In some embodiments of the first aspect of the present application, there is no particular restriction on the type of piezoelectric single crystal, as long as the purpose of the present application can be achieved. For example, the piezoelectric single crystal may include a quartz single crystal, a tellurium oxide crystal, a bismuth germanate single crystal (Bi 12 GeO 20 ), lithium iodate single crystal (LiIO3), aluminum orthophosphate single crystal (AlPO4), lanthanum gallium silicate single crystal (La3Ga5SiO 14 ), barium titanate single crystal (BaTiO3) or lead zirconate titanate single crystal PbZr e Ti 1-e O3, etc., where 0<e<1.
[0014] In some embodiments of the first aspect of the present application, there is no particular restriction on the type of inorganic piezoelectric material, as long as the purpose of the present application can be achieved. For example, the inorganic piezoelectric material may include at least one of a metal oxide, a nitride, a carbide or an intermetallic compound. Specifically, the inorganic piezoelectric material may include at least one of a metal oxide, a nitride, a carbide or an intermetallic compound having piezoelectric properties, for example, the metal oxide may include zinc oxide, bismuth oxide, cobalt oxide, lead oxide, nickel oxide, chromium oxide or antimony oxide, etc., the nitride may include aluminum nitride (AlN), aluminum gallium nitride (AlGaN), aluminum indium nitride (InAlN), gallium nitride (GaN), gallium indium nitride (InGaN) or indium nitride (InN), etc., the carbide includes silicon carbide (SiC), etc., and the intermetallic compound includes titanium trialuminum (Ti3Al) or titanium aluminum (TiAl) intermetallic compound, etc.
[0015] In some embodiments of the first aspect of the present application, the piezoelectric layer includes a powder piezoelectric layer, and the thickness of the powder piezoelectric layer is 0.1μm to 5μm. For example, the lower limit of the thickness of the powder piezoelectric layer may include the following values: 0.1μm, 0.2μm, 0.5μm, 1μm or 2μm; the upper limit of the thickness of the powder piezoelectric layer may include the following values: 3μm, 4μm, 4.5μm, 4.8μm or 5μm. The inventors found that when the thickness of the powder piezoelectric layer is too small, the powder piezoelectric layer is too thin, its strength is insufficient, it is easy to break, and the safety performance of the lithium metal battery is affected; when the thickness of the powder piezoelectric layer is too large, it will reduce the energy density of the lithium metal battery. The present application can improve the cycle performance and safety performance of the lithium metal battery by controlling the thickness of the powder piezoelectric layer within the above range.
[0016] In some embodiments of the first aspect of the present application, the powder piezoelectric layer is composed of a powder piezoelectric material and a conductive material, the mass percentage of the powder piezoelectric material is 50 to 100%, and the mass percentage of the conductive material is 0 to 50%. The piezoelectric materials in the present application are mostly electronic insulators, which are not conducive to the uniform dispersion of current on the surface of the current collector. Therefore, it is necessary to control the ratio of the piezoelectric material to the conductive material. The present application controls the mass percentage of the powder piezoelectric material and the conductive material in the powder piezoelectric layer within the above range, so as to disperse lithium ions and electrons at the same time, thereby achieving the purpose of inhibiting the growth of lithium dendrites.
[0017] In some embodiments of the first aspect of the present application, the powdered piezoelectric material includes at least one of the powder of the piezoelectric polymer, the powder of the piezoelectric ceramic, or the powder of the piezoelectric single crystal; the conductive material includes at least one of conductive carbon powder or conductive metal powder. The present application does not limit the type of conductive material, as long as the purpose of the present application can be achieved. For example, the conductive material may include at least one of acetylene black (AB), conductive carbon black (Super P), or Ketjen black.
[0018] In some other embodiments of the first aspect of the present application, the piezoelectric layer includes a thin film piezoelectric layer; the thickness of the thin film piezoelectric layer is 5μm to 200μm, preferably 50μm to 100μm. For example, the lower limit of the thickness of the thin film piezoelectric layer may include the following values: 5μm, 10μm, 20μm, 50μm or 100μm; the upper limit of the thickness of the thin film piezoelectric layer may include the following values: 110μm, 130μm, 150μm, 180μm or 200μm. The inventors found that when the thickness of the thin film piezoelectric layer is too small and the thin film piezoelectric layer is too thin, its strength is insufficient and it is easy to break, and the safety performance of the lithium metal battery is affected; when the thickness of the thin film piezoelectric layer is too large, the energy density of the lithium metal battery will be reduced. The present application can improve the cycle performance and safety performance of the lithium metal battery by controlling the thickness of the thin film piezoelectric layer within the above range. The thin film piezoelectric layer with a thickness in the above preferred range has a better effect on improving the cycle performance and safety performance of the lithium metal battery.
[0019] In some other embodiments of the first aspect of the present application, the thin film piezoelectric layer includes a thin film piezoelectric material, and the thin film piezoelectric material includes at least one of a piezoelectric polymer film, a piezoelectric ceramic film, a piezoelectric single crystal film, or an inorganic piezoelectric material film. Among them, the inorganic piezoelectric material film may also include a film or a single crystal sheet made of the above-mentioned piezoelectric ceramics.
[0020] In the present application, there is no particular restriction on the type of piezoelectric layer in the lithium metal battery. Those skilled in the art can choose to use a powder piezoelectric layer or a thin film piezoelectric layer according to actual conditions, as long as the purpose of the present application can be achieved.
[0021] The present application has no particular restrictions on the preparation of the powder piezoelectric layer. In one embodiment, illustratively, PVDF powder and acetylene black can be dispersed in N-methylpyrrolidone (NMP), coated on the surface of the negative electrode current collector using a scraper, and dried at 75 to 85° C. in a vacuum drying oven to obtain a negative electrode sheet, which includes a powder piezoelectric layer located on the surface of the negative electrode current collector.
[0022] The present application has no particular restrictions on the preparation of the thin film piezoelectric layer. In one embodiment, illustratively, PVDF powder is put into 160 to 200 mL of anhydrous ethanol and 110 to 130 mL of NMP mixed solvent, stirred at 65 to 75 ° C for 1.5 to 2.5 hours, then placed in an ultrasonic cleaner, connected to a vacuum pump, ultrasonically evacuated for 8 to 12 minutes, and kept warm at 65 to 75 ° C for 15 to 25 minutes to obtain a transparent and uniform solution, and the solution is introduced into a casting machine equipped with a polyester film tape, and a PVDF film is prepared by casting, and the width of the scraper slit is adjusted. The prepared PVDF film is peeled off from the polyester film tape to obtain a thin film piezoelectric layer.
[0023] In some embodiments of the first aspect of the present application, the piezoelectric layer is located on the surface of the negative electrode collector; or is located between the negative electrode collector and the negative electrode material layer, or is located on the outer surface of the negative electrode material layer; or the piezoelectric layer is mixed with the negative electrode material layer and is located on the surface of the negative electrode collector.
[0024] The negative electrode plate in the present application may include a negative electrode material layer or may not include a negative electrode material layer. It can be understood that when the negative electrode material layer is not included, the piezoelectric layer is located on the surface of the negative electrode collector, and the piezoelectric layer can be evenly covered on the surface of the negative electrode collector, and the negative electrode collector covered with the piezoelectric layer is directly used as the negative electrode plate. When the negative electrode plate in the present application includes a negative electrode material layer, the piezoelectric layer can be evenly covered on the surface of the negative electrode collector, and located between the negative electrode collector and the negative electrode material layer; or the piezoelectric layer can be evenly covered on the outer surface of the negative electrode material layer, and located on the outer surface of the negative electrode material layer, between the negative electrode and the electrolyte; or the piezoelectric layer can be evenly mixed with the negative electrode material layer, and then evenly covered on the surface of the negative electrode collector, and located on the surface of the negative electrode collector.
[0025] The negative electrode plate of the present application includes a negative electrode current collector and a piezoelectric layer. Among them, there is no special restriction on the negative electrode current collector, as long as the purpose of the present application can be achieved, for example, it includes copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, foam nickel, foam copper or composite current collector, etc. When the negative electrode plate in the present application also includes a negative electrode material layer, the negative electrode material layer may include lithium metal or a composite material containing lithium metal. The negative electrode plate in the present application may also include a conductive layer, which is located between the negative electrode current collector and the negative electrode material layer. The composition of the conductive layer is not particularly limited, and it can be a conductive layer commonly used in the art. The conductive layer includes a conductive agent and a binder. The present application has no special restrictions on the conductive agent and the binder, as long as the purpose of the present application can be achieved. When the negative electrode plate of the present application includes a conductive layer, the piezoelectric layer can be uniformly covered on the surface of the negative electrode collector and located between the negative electrode collector and the conductive layer; or the piezoelectric layer is between the conductive layer and the negative electrode material layer; or the piezoelectric layer can be uniformly covered on the outer surface of the negative electrode material layer, located on the outer surface of the negative electrode material layer, between the negative electrode and the electrolyte; or the piezoelectric layer can be uniformly mixed with the negative electrode material layer, and then uniformly covered on the surface of the negative electrode collector, located on the surface of the negative electrode collector.
[0026] The second aspect of the present application provides a lithium metal battery, which includes the negative electrode plate provided in the first aspect of the present application.
[0027] The negative electrode plate in the lithium metal battery of the present application adopts the negative electrode plate provided in the present application, and other components, including the positive electrode plate, isolation membrane and electrolyte, etc., are not particularly limited as long as the purpose of the present application can be achieved.
[0028] There is no particular restriction on the positive electrode sheet in the present application, as long as the purpose of the present application can be achieved. For example, the positive electrode sheet generally includes a positive current collector and a positive electrode material layer. Among them, the positive current collector is not particularly limited, as long as the purpose of the present application can be achieved, for example, it can include aluminum foil, aluminum alloy foil or composite current collector, etc. The positive electrode material layer includes a positive electrode active material. There is no particular restriction on the positive electrode active material, as long as the purpose of the present application can be achieved, for example, it can include lithium nickel cobalt manganese oxide (811, 622, 523, 111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide, lithium manganese oxide, lithium iron manganese phosphate or lithium titanate. In the present application, the thickness of the positive current collector and the positive electrode material layer is not particularly limited, as long as the purpose of the present application can be achieved. For example, the thickness of the positive current collector is 5μm to 20μm, preferably 6μm to 18μm, and more preferably 8μm to 16μm. The thickness of the positive electrode material layer is 30μm to 120μm. Optionally, the positive electrode plate may further include a conductive layer, the conductive layer being located between the positive electrode current collector and the positive electrode material layer. The composition of the conductive layer is not particularly limited, and may be a conductive layer commonly used in the art. The conductive layer includes a conductive agent and a binder.
[0029] The above-mentioned conductive agent is not particularly limited, as long as the purpose of the present application can be achieved. For example, the conductive agent can include at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon nanofibers, flake graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes or graphene, etc. The above-mentioned binder is not particularly limited, and any binder known in the art can be used, as long as the purpose of the present application can be achieved. For example, the binder can include at least one of polypropylene alcohol, sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, polyimide, polyimide, polyamide-imide, styrene-butadiene rubber (SBR), polyvinyl alcohol (PVA), polyvinylidene fluoride, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), water-based acrylic resin, carboxymethyl cellulose (CMC) or sodium carboxymethyl cellulose (CMC-Na), etc.
[0030] The isolation membrane in the present application is not particularly limited, as long as the purpose of the present application can be achieved. For example, polyethylene (PE), polypropylene (PP)-based polyolefin (PO)-based membranes, polyester films (such as polyethylene terephthalate (PET) films), cellulose films, polyimide films (PI), polyamide films (PA), spandex or aramid films, woven films, non-woven films (non-woven fabrics), microporous films, composite films, diaphragm paper, rolled films, spinning films, etc. At least one. For example, the isolation membrane may include a substrate layer and a surface treatment layer. The substrate layer may be a non-woven fabric, a film or a composite film with a porous structure, and the material of the substrate layer may include at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. Optionally, a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite membrane may be used. Optionally, a surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. For example, the inorganic layer includes inorganic particles and a binder, and the inorganic particles are not particularly limited, for example, they can be selected from at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide and barium sulfate. The binder is not particularly limited, for example, it can be selected from one or more combinations of polyvinylidene fluoride, copolymer of vinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene and polyhexafluoropropylene. The polymer layer contains a polymer, and the material of the polymer includes at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride or poly (vinylidene fluoride-hexafluoropropylene) etc.
[0031] The lithium metal battery of the present application also includes an electrolyte, which may be at least one of a gel electrolyte, a solid electrolyte and an electrolyte, and the electrolyte includes a lithium salt and a non-aqueous solvent. In some embodiments of the present application, the lithium salt may include at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, LiBOB, LiTFSI or lithium difluoroborate. For example, the lithium salt may be selected from LiTFSI because it can provide high ionic conductivity and improve cycle characteristics. The non-aqueous solvent may be at least one of a carbonate compound, a carboxylate compound, an ether compound or other organic solvents. The above-mentioned carbonate compound may be a chain carbonate compound, a cyclic carbonate compound, a fluorinated carbonate compound or a combination thereof. Examples of the above-mentioned linear carbonate compounds are dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC) and combinations thereof. Examples of cyclic carbonate compounds are ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC) and combinations thereof. Examples of fluorocarbonate compounds are fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate and combinations thereof. Examples of the above-mentioned carboxylic acid ester compounds are methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolactone, valerolactone, mevalonolactone, caprolactone and combinations thereof. Examples of the above-mentioned ether compounds are dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran and combinations thereof. Examples of the above-mentioned other organic solvents are at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methylcyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate or phosphate.
[0032] The preparation process of lithium metal batteries is well known to those skilled in the art, and this application does not have any particular restrictions. For example, it can be manufactured by the following process: overlap the positive electrode and the negative electrode via a separator, and after stacking, fix the four corners of the entire laminate structure with tape, place it in an aluminum-plastic film, and finally obtain a lithium metal laminate battery after top and side sealing, liquid injection, and packaging. The negative electrode used is the negative electrode provided in this application.
[0033] The third aspect of the present application provides an electronic device, which includes the lithium metal battery provided by the second aspect of the present application.
[0034] The electronic device of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. In some embodiments, the electronic device can include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, and a large household battery.
[0035] The present application provides a negative electrode plate, a lithium metal battery and an electronic device including the negative electrode plate, wherein the negative electrode plate includes a negative electrode current collector and a piezoelectric layer, wherein the piezoelectric layer has a polarization electric field, wherein the direction of the polarization electric field is from the negative electrode current collector to the surface of the negative electrode, and the material of the piezoelectric layer includes at least one of a piezoelectric polymer, a piezoelectric ceramic, a piezoelectric single crystal or an inorganic piezoelectric material. The negative electrode plate can control the lithium deposition site, effectively inhibit the growth of lithium dendrites, and significantly improve the cycle performance and safety performance of the lithium metal battery. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical scheme, and advantages of the present application more clearly understood, the present application is further described in detail with reference to the following embodiments. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by a person of ordinary skill in the art based on the embodiments in the present application belong to the scope of protection of the present application.
[0037] Example
[0038] Hereinafter, the embodiments of the present application will be described in more detail with reference to Examples and Comparative Examples. Various tests and evaluations were performed according to the following methods.
[0039] Test methods and equipment:
[0040] Deposition overpotential test:
[0041] Lithium metal batteries were assembled with lithium metal or current collector with piezoelectric layer as positive electrode and pure lithium metal as negative electrode. The separator and electrolyte were consistent with the battery used for cycling. 2 The lithium metal battery is discharged at a constant current density of , and the curve of voltage changing with time is recorded. The absolute value difference between the peak voltage and the stable voltage is the lithium metal deposition overpotential.
[0042] Cycle performance test:
[0043] The lithium metal battery is charged and discharged at a rate of 0.1C at 25°C for one cycle. Then, at a test temperature of 25°C, it is charged to 4.3V at a constant current of 0.3C, then charged to 0.05C at a constant voltage, and discharged to 2.8V at 1C after standing for 5 minutes. The capacity obtained in this step is taken as the initial capacity, and a cycle test is performed at 0.3C charge / 1C discharge. The capacity at each step is compared with the initial capacity to obtain the capacity decay curve. The number of cycles at 25°C until the capacity retention rate is 80% is recorded as the room temperature cycle performance of the lithium metal battery.
[0044] Example 1
[0045] <Preparation of negative electrode sheet>
[0046] PVDF powder and acetylene black (AB) with a mass ratio of 95:5 were dispersed in NMP to prepare a slurry with a solid content of 12%. The PVDF and AB were mixed evenly by stirring. The slurry was coated on the surface of the negative electrode collector copper foil with a thickness of 10 μm using a scraper, and dried at 80°C in a vacuum drying oven to obtain a negative electrode sheet with a powder piezoelectric layer thickness of 3 μm.
[0047] The negative electrode sheet prepared above was placed in a parallel electric field for air polarization. The polarization electric field was 10 kV / mm, the polarization time was 30 min, the piezoelectric layer faced the negative voltage side, and the negative current collector faced the positive voltage side. After polarization, the negative electrode sheet was cut into 40 mm × 60 mm for standby use. The room temperature coercive field strength Ec of PVDF was 50 kV / mm.
[0048] <Preparation of positive electrode sheet>
[0049] The positive electrode active material lithium iron phosphate (LiFePO4), conductive agent conductive carbon black (Super P), and binder PVDF are mixed in a mass ratio of 97.5:1.0:1.5, and N-methylpyrrolidone (NMP) is added as a solvent to prepare a slurry with a solid content of 75%, and stirred evenly. The slurry is evenly coated on a positive electrode current collector aluminum foil with a thickness of 10μm, and dried at 90°C to obtain a positive electrode sheet with a single-sided positive electrode active material layer coated with a positive electrode active material layer with a thickness of 100μm. After coating, the positive electrode sheet is cut into a specification of 38mm×58mm for standby use.
[0050] <Preparation of Electrolyte>
[0051] In a dry argon atmosphere, dioxolane (DOL) and dimethyl ether (DME) are mixed in a volume ratio of DOL:DME=1:1 to obtain a mixed solvent, and then lithium salt lithium bistrifluoromethanesulfonyl imide (LiTFSI) is added to the mixed solvent to dissolve and mix evenly to obtain an electrolyte with a lithium salt concentration of 1 mol / L.
[0052] <Preparation of lithium metal batteries>
[0053] A polyethylene (PE) with a thickness of 15 μm was selected as the separator, and the negative electrode sheet prepared above was placed in the middle. The upper and lower layers were the positive electrode sheets coated on one side, and the separator was between the positive electrode sheet and the negative electrode sheet. After stacking, the four corners of the entire stacked structure were fixed with tape, and then placed in an aluminum-plastic film. After top and side sealing, liquid injection, and packaging, a lithium metal stacked battery was finally obtained.
[0054] Embodiment 2-8
[0055] The preparation steps of <Preparation of negative electrode sheet>, <Preparation of positive electrode sheet>, <Preparation of electrolyte> and <Preparation of lithium metal battery> are the same as those in Example 1, and the changes in relevant preparation parameters are shown in Table 1.
[0056] Example 9
[0057] <Preparation of negative electrode sheet>
[0058] 80g of PVDF powder was put into a round-bottom flask containing 180mL of anhydrous ethanol and 120mL of NMP mixed solvent, and stirred at 70℃ for 2h. Then it was placed in an ultrasonic cleaner, connected to a vacuum pump, ultrasonically evacuated for 10min, and kept at 70℃ for 20min to obtain a transparent and uniform solution. This solution was introduced into a casting machine equipped with a polyester film tape, and a PVDF film was prepared by casting. The width of the scraper slit was adjusted, and the prepared PVDF film was peeled off from the polyester film tape with a thickness of 10μm.
[0059] The PVDF film is placed in a parallel electric field for air polarization, the polarization electric field is 10 kV / mm, the polarization time is 30 min, and the polarization electric field direction is constant. After completion, the internal positively charged direction of the polarized PVDF film is attached to the negative electrode collector copper foil side to obtain a negative electrode sheet with a film piezoelectric layer thickness of 10 μm, and the negative electrode sheet is cut into a specification of 40 mm × 60 mm for standby use.
[0060] <Preparation of positive electrode sheet>, <Preparation of electrolyte>, and <Preparation of lithium metal battery> are the same as in Example 1.
[0061] Examples 10-15
[0062] The preparation steps of <Preparation of negative electrode sheet>, <Preparation of positive electrode sheet>, <Preparation of electrolyte> and <Preparation of lithium metal battery> are the same as those in Example 9, and the changes in relevant preparation parameters are shown in Table 1.
[0063] Example 16
[0064] <Preparation of negative electrode sheet>
[0065] PVDF powder and acetylene black (AB) with a mass ratio of 95:5 are dispersed in NMP to prepare a slurry with a solid content of 12%. The PVDF and AB are mixed evenly by stirring, and the slurry is coated on the outer surface of the lithium metal of the negative electrode material layer with a scraper. The slurry is dried at 80°C in a vacuum drying oven for use. After drying, a negative electrode sheet with a powder piezoelectric layer thickness of 3 μm is obtained.
[0066] The negative electrode sheet is placed in a parallel electric field for air polarization, the polarization electric field is 50 kV / mm, the polarization time is 30 min, and the piezoelectric layer faces the negative voltage side. After completion, the negative electrode sheet is cut into 40 mm × 60 mm specifications for use.
[0067] <Preparation of positive electrode sheet>, <Preparation of electrolyte>, and <Preparation of lithium metal battery> are the same as in Example 1.
[0068] Embodiment 17
[0069] <Preparation of negative electrode sheet>
[0070] PVDF powder and acetylene black (AB) with a mass ratio of 95:5 are dispersed in NMP to prepare a slurry with a solid content of 12%. The PVDF and AB are mixed evenly by stirring, and the slurry is coated on the surface of the negative electrode current collector copper foil with a scraper, and dried at 80°C in a vacuum drying oven for standby use. After drying, a modified current collector with a powder piezoelectric layer thickness of 3μm is obtained; the lithium metal of the negative electrode material layer is rolled on the modified current collector with a roller press at a pressure of 8t to obtain a negative electrode sheet.
[0071] The negative electrode sheet is placed in a parallel electric field for air polarization, the polarization electric field is 50 kV / mm, the polarization time is 30 min, and the piezoelectric layer faces the negative voltage side. After completion, the negative electrode sheet is cut into 40 mm × 60 mm specifications for use.
[0072] <Preparation of positive electrode sheet>, <Preparation of electrolyte>, and <Preparation of lithium metal battery> are the same as in Example 1.
[0073] Embodiment 18
[0074] <Preparation of negative electrode sheet>
[0075] PVDF powder and acetylene black (AB) with a mass ratio of 95:5 are dispersed in NMP to prepare a slurry with a solid content of 12%. PVDF and AB are mixed evenly by stirring, and coated on the surface of the negative electrode current collector copper foil with a scraper, and dried in a vacuum drying oven at 80°C for standby use. After drying, a modified current collector with a powder piezoelectric layer thickness of 3μm is obtained. Pre-replenishment of lithium is carried out by electrochemical lithium replenishment, and a lithium sheet with a thickness of 0.05mm is used as the lithium source. A 15μm PE diaphragm is selected, and the modified current collector and lithium metal are placed on both sides of the diaphragm, where the piezoelectric layer part and the lithium metal part are facing the diaphragm, and assembled into a lithium replenishment battery for electrochemical lithium replenishment. The electrolyte is the same as the electrolyte in <Preparation of Electrolyte>, and the lithium replenishment equipment is a 5V, 5mA device (brand: Blue Electric, model: CT2001A), and the lithium replenishment current is 0.2mA / cm 2 , discharge 15.5h, lithium replenishment 3.1mAh / cm 2 After the pre-lithium replenishment is completed, a negative electrode sheet containing lithium metal is obtained.
[0076] The negative electrode sheet is placed in a parallel electric field for air polarization, the polarization electric field is 50 kV / mm, the polarization time is 30 min, and the piezoelectric layer faces the negative voltage side. After completion, the negative electrode sheet is cut into 40 mm × 60 mm specifications for use.
[0077] <Preparation of positive electrode sheet>, <Preparation of electrolyte>, and <Preparation of lithium metal battery> are the same as in Example 1.
[0078] The relevant preparation parameters of Examples 16-18 are shown in Table 1.
[0079] Embodiment 19
[0080] <Preparation of negative electrode sheet>
[0081] BaTiO3 piezoelectric ceramic powder and conductive carbon black (SP) with a mass ratio of 95:5 were dispersed in NMP to prepare a slurry with a solid content of 12%. BaTiO3 and SP were mixed evenly by stirring, and the slurry was coated on the surface of the negative electrode collector copper foil with a scraper, and dried at 80°C in a vacuum drying oven for standby use to obtain a negative electrode sheet with a powder piezoelectric layer thickness of 3μm.
[0082] The negative electrode sheet prepared above was placed in a parallel electric field for air polarization, the polarization electric field was 0.1 kV / mm, the polarization time was 30 min, and the piezoelectric layer faced the negative voltage side. After the polarization was completed, the negative electrode sheet was cut into 40 mm × 60 mm specifications for use.
[0083] <Preparation of positive electrode sheet>, <Preparation of electrolyte>, and <Preparation of lithium metal battery> are the same as in Example 1.
[0084] Examples 20-25
[0085] The preparation steps of <Preparation of negative electrode sheet>, <Preparation of positive electrode sheet>, <Preparation of electrolyte> and <Preparation of lithium metal battery> are the same as those in Example 19, and the changes in relevant preparation parameters are shown in Table 1.
[0086] Embodiment 26
[0087] <Preparation of negative electrode sheet>
[0088] PbO, ZrO2, and TiO2 with a molar ratio of 5:3:2 were placed in a high-energy planetary ball mill, 100 ml of ethanol was added as a ball milling aid, and the ball milling was carried out at a speed of 250 r / min for 30 h to obtain lead zirconate titanate PbZr 0.6 Ti 0.4 O3 powder. PbZr 0.6 Ti 0.4 O3 powder is dispersed in NMP and PbZr is stirred 0.6 Ti 0.4 The O3 powder was evenly dispersed to obtain a slurry with a solid content of 12%. The slurry was coated on the surface of the negative electrode current collector copper foil using a scraper and dried in a vacuum drying oven at 80°C for standby use to obtain a negative electrode sheet with a powder piezoelectric layer thickness of 3 μm.
[0089] The negative electrode sheet prepared above was placed in a parallel electric field for air polarization, the polarization electric field was 3 kV / mm, the polarization time was 30 min, and the piezoelectric layer faced the negative voltage side. After the polarization was completed, the negative electrode sheet was cut into 40 mm × 60 mm specifications for use.
[0090] <Preparation of positive electrode sheet>, <Preparation of electrolyte>, and <Preparation of lithium metal battery> are the same as in Example 1.
[0091] Embodiment 27
[0092] <Preparation of negative electrode sheet>
[0093] BaTiO3 single crystals were grown using the solvent method. BaTiO3 powder was evenly mixed with the solvent KF and the oxygen supplement Fe2O3, put into a platinum crucible, heated to 1175°C in a high-temperature furnace, kept warm for 8 hours, slowly cooled to 875°C, then the molten KF was poured out and cooled to room temperature at a rate of 10°C / hour. The remaining KF in the crucible was melted with hot water to obtain a BaTiO3 single crystal.
[0094] The above BaTiO3 single crystal was placed in a parallel electric field for air polarization, the polarization electric field was 0.1 kV / mm, the polarization time was 30 min, and the polarization electric field direction was parallel to the thickness direction of the single crystal and kept constant. After completion, the polarized BaTiO3 single crystal was attached to the negative electrode collector copper foil side with a positive charge direction to obtain a negative electrode sheet with a thin film piezoelectric layer thickness of 10 μm, and the negative electrode sheet was cut into a specification of 40 mm × 60 mm for standby use.
[0095] <Preparation of positive electrode sheet>, <Preparation of electrolyte>, and <Preparation of lithium metal battery> are the same as in Example 1.
[0096] Examples 28-33
[0097] The preparation steps of <Preparation of negative electrode sheet>, <Preparation of positive electrode sheet>, <Preparation of electrolyte> and <Preparation of lithium metal battery> are the same as those in Example 32, and the changes in relevant preparation parameters are shown in Table 1.
[0098] Embodiment 34
[0099] <Preparation of negative electrode sheet>
[0100] A 10 μm thick nylon 7 film (brand: Taiwan Chemical Fiber Co., Ltd., grade: NP4000) was placed in a parallel electric field for air polarization. The polarization electric field was 280 kV / mm, the polarization time was 30 min, and the polarization electric field direction was parallel to the film thickness direction and kept constant. After completion, the polarized nylon 7 film was attached to the negative electrode collector copper foil side with a positive charge direction to obtain a negative electrode sheet with a film piezoelectric layer thickness of 10 μm. The negative electrode sheet was cut into 40 mm × 60 mm specifications for standby use.
[0101] <Preparation of positive electrode sheet>, <Preparation of electrolyte>, and <Preparation of lithium metal battery> are the same as in Example 1.
[0102] Embodiment 35
[0103] <Preparation of negative electrode sheet>
[0104] A tellurium oxide crystal single crystal with a thickness of 10 μm (brand: Beijing Wuke Optoelectronics Technology Co., Ltd., brand: TEO2) was placed in a parallel electric field for air polarization. The polarization electric field was 3 kV / mm, the polarization time was 30 min, and the polarization electric field direction was parallel to the thickness direction of the single crystal and remained constant. After completion, the polarized tellurium oxide crystal single crystal was attached to the negative electrode collector copper foil side with a positive charge direction to obtain a negative electrode sheet with a thin film piezoelectric layer thickness of 10 μm. The negative electrode sheet was cut into a specification of 40 mm × 60 mm for standby use.
[0105] <Preparation of positive electrode sheet>, <Preparation of electrolyte>, and <Preparation of lithium metal battery> are the same as in Example 1.
[0106] Comparative Example 1
[0107] The negative electrode sheet is a negative electrode current collector copper foil, and the preparation steps of <preparation of positive electrode sheet>, <preparation of electrolyte> and <preparation of lithium metal battery> are the same as those in Example 1.
[0108] Comparative Examples 2-5
[0109] The preparation steps of <Preparation of Negative Electrode Plate>, <Preparation of Positive Electrode Plate>, <Preparation of Electrolyte> and <Preparation of Lithium Metal Battery> are the same as those in Example 1.
[0110] Comparative Examples 6-7
[0111] The preparation steps of <Preparation of Negative Electrode Plate>, <Preparation of Positive Electrode Plate>, <Preparation of Electrolyte> and <Preparation of Lithium Metal Battery> are the same as those in Example 9.
[0112] Comparative Examples 8-9
[0113] The preparation steps of <Preparation of negative electrode sheet>, <Preparation of positive electrode sheet>, <Preparation of electrolyte> and <Preparation of lithium metal battery> are the same as those in Example 19.
[0114] Comparative Examples 10-11
[0115] The preparation steps of <Preparation of negative electrode sheet>, <Preparation of positive electrode sheet>, <Preparation of electrolyte> and <Preparation of lithium metal battery> are the same as those in Example 32.
[0116] Comparative Example 12
[0117] The negative electrode plate is lithium metal, and the preparation steps of <Preparation of positive electrode plate>, <Preparation of electrolyte> and <Preparation of lithium metal battery> are the same as those in Example 1.
[0118] The changes of relevant preparation parameters in the above comparative examples are shown in Table 1.
[0119]
[0120]
[0121]
[0122] It can be seen from Examples 1-4, 9-12, 19-22, and 27-30 that when lithium metal batteries using the same type of piezoelectric layer are used, their deposition overpotential and cycle performance change with the change in polarization electric field strength. Among them, after polarizing the negative electrode sheet using the polarization electric field strength and direction within the scope of this application, the deposition overpotential can be effectively reduced and the cycle performance of the lithium metal battery can be improved.
[0123] The thickness of the piezoelectric layer usually also affects the deposition overpotential and cycle performance of the lithium metal battery. From Examples 2, 5-7, 10, 13-15, 21, 23-25, 29, 31-33, it can be seen that when the thickness of the piezoelectric layer is within the range of this application, a lithium metal battery with low deposition overpotential and good cycle performance can be obtained.
[0124] It can be seen from Examples 1-15, 19-25, 27-33 and Comparative Example 1 that the cycle performance of the lithium metal battery including the piezoelectric layer provided in the present application is significantly better than that of the lithium metal battery without the piezoelectric layer. It can be seen from Examples 16-18 and Comparative Example 12 that when the negative electrode plate also includes a negative electrode material layer, the cycle performance of the lithium metal battery including the piezoelectric layer provided in the present application is also significantly better than that of the lithium metal battery without the piezoelectric layer. Providing a piezoelectric layer within the scope of the present application in the negative electrode plate can significantly improve the cycle performance of the lithium metal battery.
[0125] Based on the above analysis, the negative electrode plate provided by the present application includes a negative electrode current collector and a piezoelectric layer with a polarization electric field inside, the direction of the polarization electric field is from the negative electrode current collector to the surface of the negative electrode, and the material of the piezoelectric layer includes at least one of a piezoelectric polymer, a piezoelectric ceramic, a piezoelectric single crystal or an inorganic piezoelectric material. The negative electrode plate can control the lithium deposition site, effectively inhibit the growth of lithium dendrites, and significantly improve the cycle performance and safety performance of lithium metal batteries.
[0126] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A negative electrode plate, comprising a negative electrode current collector and a piezoelectric layer, wherein a polarization electric field exists in the piezoelectric layer, the direction of the polarization electric field is from the negative electrode current collector to the surface of the negative electrode, and the material of the piezoelectric layer comprises at least one of a piezoelectric polymer or an inorganic piezoelectric material; the strength Ec of the room temperature coercive field of the material of the piezoelectric layer satisfies: 10 kV / mm<Ec<100 kV / mm; the strength of the polarization electric field is 0.1 to 6 times the strength Ec of the room temperature coercive field.
2. The negative electrode sheet according to claim 1, wherein: The piezoelectric polymer includes polyvinylidene fluoride, vinylidene fluoride / trifluoroethylene copolymer, vinylidene fluoride / tetrafluoroethylene copolymer, vinylidene dicyano / vinyl acetate copolymer, vinylidene dicyano / vinyl benzoate copolymer, vinylidene dicyano / vinyl propionate copolymer, vinylidene dicyano / vinyl pivalate copolymer, vinylidene dicyano / methyl methacrylate copolymer, vinylidene dicyano / isobutylene copolymer or odd-numbered nylon-based piezoelectric polymer -(HN-(CH2) x -CO-) n -, wherein x is an even number between 2 and 10, and n is a positive integer between 90 and 400; The inorganic piezoelectric material includes barium titanate, lead titanate, lithium niobate, lithium tantalate, lead zirconate titanate PbZr y Ti 1-y O3, lead magnesium niobate PbMg z Nb 1-z O3, Lead zinc niobate PbZn v Nb 1-v O3, lead manganese antimonate PbMn w Sb 1-w O3、Pb 1-s M m (Zr t Ti 1-t ) 1-(s / 4) O3, quartz single crystal, tellurium oxide crystal, bismuth germanate single crystal, lithium iodate single crystal, aluminum orthophosphate single crystal, lanthanum gallium silicate single crystal, barium titanate single crystal, lead zirconate titanate single crystal PbZr e Ti 1-e O3, zinc oxide, bismuth oxide, cobalt oxide, lead oxide, nickel oxide, chromium oxide, antimony oxide, aluminum nitride, gallium aluminum nitride, aluminum indium nitride, gallium nitride, gallium indium nitride, indium nitride, silicon carbide, titanium trialuminum or titanium aluminum based intermetallic compounds, wherein 0<y<1, 0<z<1, 0<v<1, 0<w<1, 0<s<1, 0<m<1, 0<t<1, 0<e<1, and M is selected from any one of the rare earth elements.
3. The negative electrode sheet according to claim 1, wherein: The piezoelectric layer includes a powder piezoelectric layer, and the thickness of the powder piezoelectric layer is 0.1 μm to 5 μm.
4. The negative electrode sheet according to claim 3, wherein: The powder piezoelectric layer is composed of powder piezoelectric material and conductive material. The mass percentage of the powder piezoelectric material is 50% to 100%, and the mass percentage of the conductive material is 0% to 50%.
5. The negative electrode sheet according to claim 4, wherein: The powdered piezoelectric material includes at least one of the powder of the piezoelectric polymer or the powder of the inorganic piezoelectric material; and the conductive material includes at least one of the conductive carbon powder or the conductive metal powder.
6. The negative electrode sheet according to claim 1, wherein: The piezoelectric layer includes a thin film piezoelectric layer; the thickness of the thin film piezoelectric layer is 5 μm to 200 μm.
7. The negative electrode sheet according to claim 6, wherein: The thin film piezoelectric layer includes a thin film piezoelectric material, and the thin film piezoelectric material includes at least one of a piezoelectric polymer film or an inorganic piezoelectric material film.
8. The negative electrode sheet according to claim 1, wherein: The piezoelectric layer is located on the surface of the negative electrode current collector; or located between the negative electrode current collector and the negative electrode material layer, or located on the outer surface of the negative electrode material layer; or the piezoelectric layer is mixed with the negative electrode material layer and located on the surface of the negative electrode current collector.
9. A lithium metal battery comprising the negative electrode sheet according to any one of claims 1 to 8.
10. An electronic device comprising the lithium metal battery according to claim 9.