A method for preparing nickel-germanium-silver electrode for gallium arsenide solar cells

The nickel layer is prepared by electroplating and the germanium and silver layers are prepared by evaporation or magnetron sputtering. The problem of nickel alloy formation in vacuum evaporation is solved, and the low-cost preparation of high-purity nickel-germanium silver electrodes is achieved, reducing the cost of reducing the It has production costs and environmental pollution, and is suitable for large-scale production.

CN114300548BActive Publication Date: 2024-12-03CHINA ELECTRONIC TECH GRP CORP NO 18 RES INST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111580055.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-22
Publication Date
2024-12-03
Estimated Expiration
2041-12-22

AI Technical Summary

Technical Problem

When the existing vacuum evaporation method is used to prepare nickel-germanium silver electrodes, nickel and crucible sleeve material form an alloy at low temperature, which affects the purity and reliability of the electrodes. Magnetic sputtering method may cause metal nickel to contaminate other cavitys. Increased production costs and environmental pollution.

Method used

The nickel layer is prepared by electroplating or electrochemical plating, and the germanium and silver layers are prepared by evaporation or magnetron sputtering. The silver layer is thickened in combination with the electroplating process to avoid the eutectic phenomenon of crucible sleeves and magnetism in vacuum evaporation. Control the pollution problem in the sputtering method, reduce production costs and improve the utilization rate of metal materials.

Benefits of technology

It realizes high purity preparation of nickel layers, reduces production costs, avoids waste of metal materials and environmental pollution, improves battery performance and reliability, simplifies process equipment and maintenance costs, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114300548B_ABST
    Figure CN114300548B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a nickel-germanium-silver electrode for a gallium arsenide solar cell, wherein a nickel layer is prepared by electroplating or chemical plating, a germanium layer and a part of a silver layer are prepared by evaporation or magnetron sputtering, and then the silver layer is thickened by electroplating. The nickel-germanium-silver electrode is prepared, wherein the nickel layer and the germanium layer are prepared by different preparation methods respectively, and the electroplating process and the evaporation process are combined to reduce the production cost to the greatest extent, while ensuring the quality of the nickel layer, avoiding the phenomenon of nickel and crucible sleeve eutectic in the vacuum evaporation method, and also avoiding the problem of metal nickel contaminating other cavities in the magnetron sputtering method; in addition, the invention prepares the nickel layer by electroplating or chemical plating, which makes maximum use of metal materials and reduces the waste of metal materials; the electroplating process equipment is simple, the maintenance cost is low, the large-scale production cost is low, and the emission of chemicals is very small; the electroplating can be produced synchronously in batches, and the working hours are shorter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of physical power sources, and in particular relates to a method for preparing a nickel-germanium-silver electrode of a gallium arsenide solar cell. Background Art

[0002] Gallium arsenide solar cells have the characteristics of high conversion efficiency, good radiation resistance, and high efficiency at high temperatures. They are currently the most efficient solar cells used in domestic aerospace engineering. Gallium arsenide solar cells are made of upper and lower metal electrodes on the upper and lower surfaces of epitaxial wafers with PN junctions. When the cell is exposed to light, the photocurrent generated is collected and exported by the metal electrodes. Therefore, the quality of the electrodes plays a very important role in the electrical performance and reliability of the cell.

[0003] For existing III-V single-junction or multi-junction solar cells for space use, metal electrodes are often prepared by vacuum evaporation to meet the requirements of space use. The metal electrodes prepared by this method have been verified to meet the requirements of space use. For nickel-germanium-silver metal electrodes, since metal nickel is easily dissolved with crucible cover materials such as molybdenum and tungsten at a temperature lower than the melting point of nickel during the evaporation process, that is, the crucible cover material will dissolve into nickel and tungsten or nickel and molybdenum alloys during the process of heating and melting metal nickel by electron beam, thus affecting the purity of the metal and further affecting the reliability of the electrode. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for preparing a nickel-germanium-silver electrode for a gallium arsenide solar cell.

[0005] The technical solution adopted by the present invention is: a method for preparing a nickel-germanium-silver electrode for a gallium arsenide solar cell, preparing a nickel layer by electroplating or chemical plating, and preparing a germanium layer and a silver layer by evaporation or magnetron sputtering.

[0006] Preferably, after the silver layer is evaporated, electroplating is performed to thicken the silver layer.

[0007] Preferably, the 30nm-100nm germanium layer and the 50nm-500nm silver layer are prepared by evaporation or magnetron sputtering.

[0008] Preferably, before nickel electroplating, the light-receiving surface of the battery is subjected to glue etching.

[0009] Preferably, the specific steps are as follows:

[0010] Gluing: Gluing the light-receiving surface of the battery;

[0011] Corrosion, to corrode and activate the surface of the lower electrode to be evaporated;

[0012] Preparation of nickel layer: preparing a nickel layer on the outer side of the epitaxial wafer by electroplating or chemical plating;

[0013] Preparation of germanium-silver layer: a germanium layer and a silver layer are sequentially prepared on the outer side of the nickel layer by evaporation or magnetron sputtering;

[0014] Preparation of thickened silver layer: electroplating thickened silver layer on the lower electrode of the battery.

[0015] The advantages and positive effects of the present invention are: preparing a nickel-germanium-silver electrode, wherein the nickel layer and the germanium-silver layer are prepared by different methods respectively, combining the electroplating process with the evaporation process, reducing the production cost to the greatest extent, while ensuring the quality of the nickel layer, avoiding the phenomenon of nickel and the crucible sleeve being eutectic in the vacuum evaporation method, and avoiding the problem of metal nickel contaminating other cavities in the magnetron sputtering method;

[0016] In addition, the present invention prepares the nickel layer through electroplating process or chemical plating, which maximizes the use of metal materials and reduces the waste of metal materials; the electroplating process equipment is simple, the maintenance cost is low, the large-scale production cost is low, and the emission of chemicals is very small; electroplating can be produced synchronously in batches, and the working hours are shorter. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 Schematic diagram of the lower electrode structure according to an embodiment of the present invention. DETAILED DESCRIPTION

[0018] The embodiments of the present invention are described below with reference to the accompanying drawings.

[0019] The present invention discloses a method for preparing a nickel-germanium-silver electrode for a gallium arsenide solar cell. In order to prevent other metals in a crucible sleeve from affecting the purity of the nickel layer during the evaporation method, the nickel layer is prepared by electroplating or chemical plating, and then the germanium layer and the silver layer are prepared by evaporation or magnetron sputtering. The prepared electrode structure is as follows: Figure 1 As shown. Electroplating is a common method for preparing metal films. The nickel electroplating process is widely used in the machinery industry and is a very mature and low-cost metal film preparation process. The electroplating method of the present invention is used to prepare the nickel layer, which can not only achieve the high-purity preparation of nickel metal electrodes, but also reduce the process cost and achieve low-cost battery electrodes. The various metal layers of the nickel-germanium-silver electrode are prepared in layers by different methods to maximize the purity of each metal layer and ensure battery performance. Before electroplating nickel, the light-receiving surface of the battery is subjected to glue corrosion; after evaporating the silver layer, the silver layer is electroplated to thicken it.

[0020] The specific steps include:

[0021] Gluing: Gluing the light-receiving surface of the battery, and baking to fix the shape after gluing;

[0022] Etching: the surface of the lower electrode to be evaporated is corroded and activated. It is divided into two steps: the epitaxial wafer is corroded and removed in the etching solution a, and then washed with deionized water and immersed in the acid solution b for activation;

[0023] Preparation of nickel layer: preparing a nickel layer on the outer side of the epitaxial wafer by electroplating or chemical plating;

[0024] Preparation of germanium-silver layer: a germanium layer and a part of the silver layer protecting the germanium layer are prepared on the outer side of the nickel layer by evaporation or magnetron sputtering, wherein the germanium layer is 30nm-100nm and the silver layer is 50nm-500nm;

[0025] The thickened silver layer is prepared by thickening the silver layer of the lower electrode of the battery prepared in the previous step, and the silver layer is thickened by electroplating, and finally the silver layer is 3μm-8μm.

[0026] The method of combining the electroplating process with the evaporation process can avoid the phenomenon of nickel and crucible sleeve eutectic in the vacuum evaporation method, and can also avoid the problem of metal nickel contaminating other cavities in the magnetron sputtering method; the electroplating process maximizes the use of metal materials, and its utilization rate is close to 100%, which reduces the waste of metal materials and minimizes production costs.

[0027] The scheme of the present invention is described below in conjunction with the accompanying drawings, wherein the experimental methods without specific operating steps are all carried out in accordance with the corresponding product instructions, and the instruments, reagents, and consumables used in the examples can all be purchased from commercial companies unless otherwise specified.

[0028] Embodiment 1:

[0029] 1. Glue coating: Glue corrosion is performed on the light-receiving surface of the battery.

[0030] Apply glue and spread it at a speed of 500r / min-1500r / min; bake at 95℃-110℃ for 7 minutes-15 minutes to set the shape;

[0031] Apply glue to the light-receiving surface of the cell, bake the epitaxial wafer in an oven at 130-150°C for 30 minutes, and perform photolithography exposure for 20s-30s; bake the epitaxial wafer at 95°C-110°C for 7 minutes-15 minutes, and then place it in the corresponding developer for development for 30s-60s;

[0032] The etching is carried out alternately in a sulfuric acid and hydrogen peroxide mixture, hydrochloric acid, a sulfuric acid and hydrogen peroxide mixture and a hydrofluoric acid solution. After etching with each solution, the etching is rinsed with water 6 to 8 times; finally, the glue is removed by immersion in an acetone solution.

[0033] 2. Corrosion: Corrosion activation of the lower electrode surface to be evaporated

[0034] Alternately perform etching and bottom removal in sulfuric acid and hydrogen peroxide mixture, hydrochloric acid, sulfuric acid and hydrogen peroxide mixture and hydrofluoric acid solution; wash with deionized water; soak in dilute sulfuric acid solution for 5s-15s for activation;

[0035] 3. Nickel plating:

[0036] The process of electroplating nickel electrodes includes: (1) placing the activated sample on the electroplating tool with the surface to be electroplated facing outward and the electrode leads in contact with the surface to be electroplated, and immersing the device in the nickel electroplating solution; (2) connecting the anode and cathode of the power supply to the nickel plate and the battery tool leads respectively; (3) turning on the power switch to start electroplating, with a current density of 1A / dm 2 -10A / dm 2 After a certain period of electroplating, when the coating thickness reaches 20nm-100nm, turn off the power, take out the sample, rinse it and dry it;

[0037] 4. Evaporation of Germanium Silver:

[0038] The process of evaporating germanium-silver on the lower electrode of the battery includes: (1) placing the sample into a vacuum coating machine and -4 Under the condition of Pa, plasma is used to bombard the surface to be evaporated to clean the surface; (2) 80nm germanium is evaporated at a rate of 0.5nm / s-2nm / s; (3) 300nm silver is evaporated at a rate of 0.5nm / s-5nm / s; (4) Cool for 5min, fill with nitrogen, and take out the sample;

[0039] 5. Electroplating thickened silver layer:

[0040] The process of electroplating a thick silver layer on the lower electrode of the battery includes: (1) placing the sample on the electroplating tool with the surface to be electroplated facing outward and the electrode lead in contact with the surface to be electroplated, and immersing the device in the silver electroplating solution; (2) connecting the anode and cathode of the power supply to the nickel plate and the battery tool lead respectively; (3) turning on the power switch to start electroplating, with a current density of 2A / dm 2 -20A / dm 2 After electroplating for a certain period of time, when the silver layer reaches a coating thickness of 4 μm, turn off the power supply, take out the sample, rinse it, and immerse it in an acetone solution to remove the glue. After completion, rinse it with deionized water and dry it.

[0041] Embodiment 2:

[0042] 1. Glue coating: Glue corrosion is performed on the light-receiving surface of the battery.

[0043] Apply glue and spread it at a speed of 500r / min-1500r / min; bake at 95℃-110℃ for 7 minutes-15 minutes to set the shape;

[0044] Apply glue to the light-receiving surface of the cell, bake the epitaxial wafer in an oven at 130-150°C for 30 minutes, and perform photolithography exposure for 20s-30s; bake the epitaxial wafer at 95°C-110°C for 7 minutes-15 minutes, and then place it in the corresponding developer for development for 30s-60s;

[0045] The etching is carried out alternately in a sulfuric acid and hydrogen peroxide mixture, hydrochloric acid, a sulfuric acid and hydrogen peroxide mixture and a hydrofluoric acid solution. After etching with each solution, the etching is rinsed with water 6 to 8 times; finally, the glue is removed by immersion in an acetone solution.

[0046] 2. Corrosion: Corrosion activation of the lower electrode surface to be evaporated

[0047] Alternately perform etching and bottom removal in sulfuric acid and hydrogen peroxide mixture, hydrochloric acid, sulfuric acid and hydrogen peroxide mixture and hydrofluoric acid solution; wash with deionized water; soak in dilute sulfuric acid solution for 5s-15s for activation;

[0048] 3. Chemical nickel plating:

[0049] The process of chemically plating nickel electrodes includes: (1) placing the activated sample on a fixture with the surface to be plated facing outward, and immersing the device in a nickel plating solution; (2) after a certain period of time, when the set plating thickness is reached, taking out the sample, rinsing it, and drying it;

[0050] 4 Magnetron sputtering germanium silver:

[0051] The process of magnetron sputtering germanium and silver on the lower electrode of the battery includes: (1) placing the sample in a magnetron sputtering device and pre-evacuating the sample; (2) transferring the sample to a vacuum chamber and sputtering 80nm of germanium at a rate of 0.5nm / s-2nm / s; and sputtering 300nm of silver at a rate of 0.5nm / s-5nm / s at a certain power; (3) filling with nitrogen and taking out the sample;

[0052] 5. Electroplating thickened silver layer:

[0053] The process of electroplating a thick silver layer on the lower electrode of the battery includes: (1) placing the sample on the electroplating tool with the surface to be electroplated facing outward and the electrode lead in contact with the surface to be electroplated, and immersing the device in the silver electroplating solution; (2) connecting the anode and cathode of the power supply to the nickel plate and the battery tool lead respectively; (3) turning on the power switch to start electroplating, with a current density of 2A / dm 2 -20A / dm 2 After electroplating for a certain period of time and reaching a coating thickness of 5 μm, turn off the power supply, take out the sample, rinse it, and immerse it in an acetone solution to remove the glue. After completion, rinse it with deionized water and dry it.

[0054] The above method can be used to prepare a triple-junction gallium arsenide solar cell with a nickel-germanium-silver lower electrode. This process reduces the use time of high-priced equipment, among which the use time of the electron gun in the evaporation process is reduced by more than half, thereby improving production capacity; the utilization rate of metals in the evaporation method is less than 5%, while the utilization rate of metals in the electroplating method is close to 100%, thereby improving the material utilization rate of nickel and silver metals and reducing production costs; it can avoid the problem of reduced material purity caused by crucible eutectic in the vacuum evaporation process of nickel; the electroplating solution can be reused, and the electroplating process produces almost no waste of raw materials, reducing the waste generated in the process, and is environmentally friendly.

[0055] The embodiments of the present invention are described in detail above, but the contents described are only preferred embodiments of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for preparing a nickel-germanium-silver electrode for a gallium arsenide solar cell, characterized in that: The specific steps are as follows: Step 1: Apply glue to the light-receiving surface of the battery; Step 2: Corrosion, corroding and activating the surface of the lower electrode to be evaporated; Step 3: preparing a nickel layer, preparing a nickel layer on the outer side of the epitaxial wafer by electroplating or chemical plating; Step 4: Preparation of germanium-silver layer: a 30nm-100nm germanium layer and a 50nm-500nm silver layer are prepared on the outside of the nickel layer by evaporation or magnetron sputtering; Step 5: Preparation of thickened silver layer: electroplating a thickened silver layer on the lower electrode of the battery.