Copper-ceramic joint body and insulating circuit substrate

By controlling the concentration of impurity elements at the joint interface of the copper-ceramic joint body and suppressing the precipitation of intermetallic compounds, the problem of ceramic substrate cracking under hot and cold cycles is solved, and high-reliability copper-ceramic joint bodies and insulating circuit substrates are realized .

CN114342573BActive Publication Date: 2024-10-15MITSUBISHI MATERIALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080061015.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-06
Filing Date
2020-08-19
Publication Date
2024-10-15
Estimated Expiration
2040-08-19

AI Technical Summary

Technical Problem

The joint between the existing ceramic substrate and the copper plate is prone to cracking under hot and cold cycles, and the Cu-Mg-Ti solder will precipitate intermetallic compounds during the joint, affecting the reliability of the joint interface.

Method used

By performing energy dispersive X-ray analysis at a position 1000nm away from the joint interface of the copper-ceramic joint, the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is controlled to 100 atomic % and limited The concentration of Al, Si, Zn and Mn is 3 atomic % or less to suppress the precipitation of impurity elements and fine intermetallic compounds.

Benefits of technology

It effectively inhibits the cracking of ceramic components, improves the reliability of hot and cold cycles, and ensures the stable bonding of ceramic substrates and copper plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114342573B_ABST
    Figure CN114342573B_ABST
Patent Text Reader

Abstract

The present invention provides a copper-ceramic joint (10), which is formed by joining a copper component (12, 13) and a ceramic component (11), wherein the copper component is made of copper or a copper alloy, and when the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is set to 100 atomic %, the total concentration of Al, Si, Zn and Mn is less than 3 atomic % at a position 1000 nm away from the joining interface between the copper component (12, 13) and the ceramic component (11) toward the copper component (12, 13) side, the concentration is measured by energy dispersion X-ray analysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a copper-ceramic joint body formed by joining a copper component made of copper or a copper alloy and a ceramic component, and an insulating circuit substrate formed by joining a copper plate made of copper or a copper alloy to the surface of a ceramic substrate.

[0002] This application claims priority based on Patent Application No. 2019-159566 filed in Japan on September 2, 2019, and Patent Application No. 2020-134070 filed in Japan on August 6, 2020, and the contents of which are incorporated herein by reference. Background Art

[0003] The power module, LED module and thermoelectric module have a structure in which a power semiconductor element, an LED element and a thermoelectric element are bonded to an insulating circuit substrate having a circuit layer made of a conductive material formed on one surface of an insulating layer.

[0004] In order to control the power semiconductor elements for high power control used in wind power generation, electric vehicles, hybrid vehicles, etc., a large amount of heat is generated during operation. Therefore, as a substrate for mounting the power semiconductor elements, the following insulating circuit substrate has been widely used: a ceramic substrate and a circuit layer formed by bonding a metal plate with excellent conductivity to one surface of the ceramic substrate. As an insulating circuit substrate, there is also provided an insulating circuit substrate in which a metal layer is formed by bonding a metal plate to the other surface of the ceramic substrate.

[0005] Patent Document 1 proposes an insulating circuit substrate in which a circuit layer and a metal layer are formed by bonding a copper plate to one surface and the other surface of a ceramic substrate. In Patent Document 1, a copper plate is arranged on one surface and the other surface of a ceramic substrate via an Ag-Cu-Ti brazing material, and the copper plates are bonded by performing a heat treatment (so-called active metal brazing method). In the active metal brazing method, a brazing material containing Ti as an active metal is used, so that the wettability of the molten brazing material and the ceramic substrate is improved, and the ceramic substrate and the copper plate can be well bonded.

[0006] When a ceramic substrate and a copper plate are joined by the active metal brazing method described in Patent Document 1, a TiN layer is formed at the joint interface between the ceramic substrate and the copper plate. This TiN layer is hard and brittle, so cracks may occur in the ceramic substrate during thermal cycling.

[0007] Patent Document 2 proposes an insulating circuit substrate in which a ceramic substrate and a copper plate are bonded together using a Cu-Mg-Ti based brazing filler metal.

[0008] In Patent Document 2, the Cu-Mg-Ti alloy is joined by heating at 560 to 800° C. in a nitrogen atmosphere, and Mg in the Cu-Mg-Ti alloy is sublimated and does not remain at the joining interface, and titanium nitride (TiN) is not substantially formed.

[0009] Patent Document 1: Japanese Patent No. 3211856

[0010] Patent Document 2: Japanese Patent No. 4375730

[0011] Recently, the heat generation temperature of semiconductor elements mounted on insulating circuit boards has tended to be higher, and insulating circuit boards are required to have higher thermal cycle reliability than ever before, which allows them to withstand severe thermal cycles.

[0012] As described in Patent Document 2, when a Cu-Mg-Ti solder is used, a liquid phase of Cu and Mg is generated at the bonding interface. Here, when there are many impurity elements at the bonding interface, when the liquid phase at the bonding interface solidifies, an intermetallic compound is precipitated, and precipitation and solidification are precipitated near the bonding interface between the ceramic substrate and the copper plate. Therefore, when subjected to severe cold and hot cycles, cracks may occur in the ceramic substrate. Summary of the invention

[0013] The present invention has been completed in view of the above situation, and its purpose is to provide a copper-ceramic joint body that can suppress the occurrence of cracks in ceramic parts even when subjected to severe thermal cycles and has excellent thermal cycle reliability, and an insulating circuit substrate composed of the copper-ceramic joint body.

[0014] In order to solve the above-mentioned problems, a copper-ceramic joint body of one embodiment of the present invention (hereinafter referred to as "the copper-ceramic joint body of the present invention") is a copper-ceramic joint body formed by joining a copper part and a ceramic part composed of copper or a copper alloy, and is characterized in that, at a position 1000 nm away from the joining interface between the copper part and the ceramic part toward the copper part side, concentration measurement is performed by energy dispersive X-ray analysis, and when the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is set to 100 atomic %, the total concentration of Al, Si, Zn and Mn is less than 3 atomic %.

[0015] According to the copper-ceramic joint body of the present invention, the concentration of impurity elements (Al, Si, Zn and Mn) at the joint interface is sufficiently low, which can inhibit the precipitation of fine intermetallic compounds at the joint interface, thereby inhibiting precipitation and solidification near the joint interface between the ceramic component and the copper component. Therefore, even when subjected to severe thermal cycles, the occurrence of cracks in the ceramic component can be inhibited.

[0016] In the copper-ceramic joint body of the present invention, preferably, when the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is set to 100 atomic %, the concentration of Al is less than 2 atomic % at a position 1000 nm away from the bonding interface between the copper part and the ceramic part toward the copper part by energy dispersive X-ray analysis.

[0017] In this case, since the concentration of Al as an impurity element at the bonding interface is limited as described above, it is possible to further suppress the occurrence of precipitation solidification near the bonding interface between the ceramic member and the copper member.

[0018] In the copper-ceramic joint body of the present invention, preferably, when the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is set to 100 atomic %, the concentration of Si is less than 2 atomic % at a position 1000 nm away from the bonding interface between the copper part and the ceramic part toward the copper part by energy dispersive X-ray analysis.

[0019] In this case, since the concentration of Si as an impurity element at the bonding interface is limited as described above, precipitation and solidification near the bonding interface between the ceramic member and the copper member can be further suppressed.

[0020] In the copper-ceramic joint body of the present invention, preferably, when the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is set to 100 atomic %, the total concentration of Zn and Mn is less than 2 atomic % at a position 1000 nm away from the bonding interface between the copper part and the ceramic part toward the copper part side by concentration measurement by energy dispersive X-ray analysis.

[0021] In this case, since the total concentration of Zn and Mn as impurity elements at the bonding interface is limited as described above, precipitation solidification near the bonding interface between the ceramic member and the copper member can be further suppressed.

[0022] Another embodiment of an insulating circuit substrate of the present invention (hereinafter referred to as "the insulating circuit substrate of the present invention") is an insulating circuit substrate formed by joining a copper plate made of copper or a copper alloy to the surface of a ceramic substrate, and is characterized in that, when the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is set to 100 atomic %, the total concentration of Al, Si, Zn and Mn is less than 3 atomic % by measuring the concentration at a position 1000 nm away from the bonding interface between the copper plate and the ceramic substrate toward the copper plate side by energy dispersive X-ray analysis.

[0023] According to the insulating circuit substrate of the present invention, the concentration of impurity elements (Al, Si, Zn and Mn) at the bonding interface is sufficiently low, which can inhibit the precipitation of fine intermetallic compounds at the bonding interface, thereby inhibiting precipitation and solidification near the bonding interface between the ceramic substrate and the copper plate. Therefore, even when subjected to severe thermal cycles, the occurrence of cracks in the ceramic substrate can be inhibited, and the thermal cycle reliability is excellent.

[0024] In the insulating circuit substrate of the present invention, preferably, when the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is set to 100 atomic %, the concentration of Al is less than 2 atomic % at a position 1000 nm away from the bonding interface between the copper plate and the ceramic substrate toward the copper plate side by energy dispersion X-ray analysis.

[0025] In this case, since the concentration of Al as an impurity element at the bonding interface is limited as described above, it is possible to further suppress the occurrence of precipitation solidification near the bonding interface between the ceramic substrate and the copper plate.

[0026] In the insulating circuit substrate of the present invention, preferably, when the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is set to 100 atomic %, the concentration of Si is less than 2 atomic % at a position 1000 nm away from the bonding interface between the copper plate and the ceramic substrate toward the copper plate side by performing concentration measurement by energy dispersive X-ray analysis.

[0027] In this case, since the concentration of Si as an impurity element at the bonding interface is limited as described above, it is possible to further suppress the occurrence of precipitation solidification near the bonding interface between the ceramic substrate and the copper plate.

[0028] In the insulating circuit substrate of the present invention, preferably, when the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is set to 100 atomic %, the total concentration of Zn and Mn is less than 2 atomic % at a position 1000 nm away from the bonding interface between the copper plate and the ceramic substrate toward the copper plate side by performing concentration measurement by energy dispersive X-ray analysis.

[0029] In this case, since the total concentration of Zn and Mn as impurity elements at the bonding interface is limited as described above, the occurrence of precipitation solidification near the bonding interface between the ceramic substrate and the copper plate can be further suppressed.

[0030] According to the present invention, it is possible to provide a copper-ceramic bonded body which can suppress the occurrence of cracks in a ceramic component even when subjected to severe thermal cycles and has excellent thermal cycle reliability, and an insulating circuit board composed of the copper-ceramic bonded body. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic explanatory diagram of a power module using an insulating circuit substrate according to an embodiment of the present invention.

[0032] Figure 2 It is an enlarged explanatory diagram of a bonding interface between a circuit layer (metal layer) and a ceramic substrate of an insulating circuit board according to an embodiment of the present invention.

[0033] Figure 3 This is a flowchart of a method for manufacturing an insulating circuit board according to an embodiment of the present invention.

[0034] Figure 4 It is a schematic explanatory diagram of a method for manufacturing an insulating circuit board according to an embodiment of the present invention. DETAILED DESCRIPTION

[0035] Hereinafter, embodiments of the present invention will be described with reference to the drawings.

[0036] The copper-ceramic bonded body according to the present embodiment is an insulating circuit substrate 10 formed by bonding a ceramic substrate 11 as a ceramic component made of ceramic, a copper plate 22 (circuit layer 12) as a copper component made of copper or a copper alloy, and a copper plate 23 (metal layer 13). Figure 1 A power module 1 including an insulating circuit substrate 10 according to the present embodiment is shown.

[0037] The power module 1 includes an insulating circuit substrate 10 on which a circuit layer 12 and a metal layer 13 are arranged, and a Figure 1 The semiconductor element 3 is bonded via the bonding layer 2, and the other side of the metal layer 13 is arranged (on the Figure 1 The heat sink 30 is shown in FIG.

[0038] The semiconductor element 3 is made of a semiconductor material such as Si, and is bonded to the circuit layer 12 via the bonding layer 2 .

[0039] The bonding layer 2 is made of, for example, Sn—Ag-based, Sn—In-based, or Sn—Ag—Cu-based solder.

[0040] The heat sink 30 diffuses the heat from the insulating circuit substrate 10. The heat sink 30 is made of copper or a copper alloy, and in this embodiment, is made of phosphorus deoxidized copper. The heat sink 30 is provided with a flow path 31 for flowing a cooling fluid.

[0041] In the present embodiment, the heat sink 30 and the metal layer 13 are bonded to each other via a solder layer 32. The solder layer 32 is made of, for example, a Sn-Ag-based, Sn-In-based, or Sn-Ag-Cu-based solder.

[0042] like Figure 1 As shown, the insulating circuit substrate 10 of this embodiment includes a ceramic substrate 11, and a circuit board 12 disposed on one surface (at the Figure 1 The circuit layer 12 is disposed on the other side of the ceramic substrate 11 (in the Figure 1 The metal layer 13 is shown below.

[0043] The ceramic substrate 11 is made of ceramics such as silicon nitride (Si3N4), aluminum nitride (AlN), and aluminum oxide (Al2O3) that have excellent insulation and heat dissipation properties. In the present embodiment, the ceramic substrate 11 is made of aluminum nitride (AlN) that has particularly excellent heat dissipation properties. The thickness of the ceramic substrate 11 is set, for example, within a range of 0.2 mm to 1.5 mm, and in the present embodiment, is set to 0.635 mm.

[0044] like Figure 4 As shown, the circuit layer 12 is formed on one side of the ceramic substrate 11 (on Figure 4 The upper surface is joined to a copper plate 22 made of copper or a copper alloy.

[0045] In the present embodiment, the circuit layer 12 is formed by bonding a rolled plate of oxygen-free copper to the ceramic substrate 11 .

[0046] The thickness of the copper plate 22 that becomes the circuit layer 12 is set within a range of 0.1 mm to 2.0 mm, and in the present embodiment, is set to 0.6 mm.

[0047] The total concentration of impurities (Al, Si, Zn, and Mn) in the copper plate 22 is preferably 0.1 mass % or less, and more preferably 0.04 mass % or less.

[0048] As the copper plate 22 , tough pitch copper can also be used.

[0049] like Figure 4 As shown, the metal layer 13 is formed on the other side of the ceramic substrate 11 (on the Figure 4 The bottom is formed by joining a copper plate 23 made of copper or a copper alloy.

[0050] In the present embodiment, the metal layer 13 is formed by bonding a rolled plate of oxygen-free copper to the ceramic substrate 11 .

[0051] The thickness of the copper plate 23 that becomes the metal layer 13 is set within a range of 0.1 mm to 2.0 mm, and in the present embodiment, is set to 0.6 mm.

[0052] The total concentration of impurities (Al, Si, Zn, and Mn) in the copper plate 23 is preferably 0.1 mass % or less, and more preferably 0.04 mass % or less.

[0053] As the copper plate 23 , tough pitch copper can also be used.

[0054] At the bonding interface between the ceramic substrate 11 and the circuit layer 12 (metal layer 13), Figure 2 As shown, at a position 1000 nm away from the bonding interface between the ceramic substrate 11 and the circuit layer 12 (and the metal layer 13) toward the circuit layer 12 (and the metal layer 13), the concentration was measured by energy dispersion X-ray analysis. When the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn was set to 100 atomic %, the total concentration of Al, Si, Zn and Mn was less than 3 atomic %.

[0055] This can suppress the precipitation of fine intermetallic compounds at the bonding interface, suppress precipitation and solidification near the bonding interface between the ceramic substrate 11 and the circuit layer 12 (and the metal layer 13), and suppress the occurrence of cracks in the ceramic substrate 11 during thermal cycle loads.

[0056] In order to suppress the occurrence of cracks in the ceramic substrate 11 even in a more severe environment, the total concentration of Al, Si, Zn, and Mn is preferably 2 atomic % or less.

[0057] In the present embodiment, the concentration of Al measured as described above is preferably 2 atomic % or less, and more preferably 1.5 atomic % or less.

[0058] The Si concentration measured as described above is preferably 2 atomic % or less, and more preferably 1.5 atomic % or less.

[0059] The total concentration of Zn and Mn measured as described above is preferably 2 atomic % or less, and more preferably 1 atomic % or less.

[0060] Below, reference Figure 3 and Figure 4 A method for manufacturing the insulating circuit board 10 according to the present embodiment will be described.

[0061] (Ceramic substrate cleaning process S01)

[0062] First, a ceramic substrate 11 is prepared and the bonding surface of the ceramic substrate 11 is cleaned. Figure 4 As shown, the surface of the ceramic substrate 11 is cleaned using the treatment liquid 51. The surface of the ceramic substrate 11 may be cleaned by immersing it in the treatment liquid 51. The treatment conditions are preferably set according to the treatment liquid 51 used. The following shows the treatment conditions when using various treatment liquids.

[0063] When hydrochloric acid is used, the concentration of HCl is set to 8 mass % or more and 20 mass % or less, the treatment temperature is set to 28° C. or more and 40° C. or less, and the treatment time is set to 3 minutes or more and 10 minutes or less.

[0064] When nitric acid is used, the concentration of HNO 3 is set to an aqueous solution of 5 mass % to 30 mass %, the treatment temperature is set to 28° C. to 40° C., and the treatment time is set to 3 minutes to 10 minutes.

[0065] When using a sodium hydroxide aqueous solution, the concentration of NaOH is set to 1 mass % to 4 mass %, the treatment temperature is set to 28° C. to 40° C., and the treatment time is set to 1 minute to 5 minutes.

[0066] When using a sodium bicarbonate aqueous solution, the concentration of NaHCO 3 is set to 1 mass % to 4 mass %, the treatment temperature is set to 28° C. to 40° C., and the treatment time is set to 1 minute to 5 minutes.

[0067] (Jointing Material Arrangement Step S02)

[0068] Then, if Figure 4 As shown, bonding materials are disposed between the copper plate 22 that becomes the circuit layer 12 and the ceramic substrate 11 , and between the copper plate 23 that becomes the metal layer 13 and the ceramic substrate 11 .

[0069] As the bonding material, Mg alone, a combination of Mg and an active metal (one or two or more selected from Ti, Zr, Hf, and Nb), or a combination of Mg and Cu can be used.

[0070] The bonding material can be arranged between the copper plate and the ceramic substrate as a slurry or a foil. When using a slurry, Mg (Mg powder) or an active metal (active metal powder) can be used as a filler of the slurry. As a filler, their hydrides can also be used.

[0071] When using foil materials, Mg foil and active metal foil can be arranged to overlap each other.

[0072] Furthermore, an alloy foil of Mg and an active metal can also be used. Furthermore, Mg foil and an active metal foil can also be used as a clad.

[0073] A Mg vapor-deposited film or a vapor-deposited film of Mg and an active metal may be arranged between the copper plate and the ceramic substrate, or the vapor-deposited film may be used as a bonding material. The vapor-deposited film may be arranged on at least one of the copper plate or the ceramic substrate, or may be arranged on both. When the vapor-deposited film of Mg and an active metal is set, co-vapor deposition may be performed, or Mg and an active metal may be vapor-deposited separately as a laminated film. The vapor-deposited film may be formed, for example, by a sputtering method or a vapor deposition method.

[0074] When an active metal is used as a bonding material, the amount of the active metal may be set to 0.4 μmol / cm 2 Above 18.8 μmol / cm 2 At this time, the amount of Mg can be set to 14 μmol / cm 2 Above 86 μmol / cm 2 the following.

[0075] When active metal is disposed, the Al concentration and Si concentration at the bonding interface may increase due to the reaction with the ceramic substrate. Therefore, it is necessary to fully control the cleanliness of the ceramic substrate and the impurity amounts of the disposed Mg, active metal, and Cu.

[0076] The purity of the disposed Mg is preferably 99.0% or more, and the total concentration of impurities (Al, Si, Zn, and Mn) is preferably 1.0% by mass or less, and more preferably 0.3% by mass or less.

[0077] The purity of the disposed active metal is preferably 99.2% or more, and the total concentration of impurities (Al, Si, Zn, and Mn) is preferably 0.5% by mass or less, and more preferably 0.3% by mass or less.

[0078] The concentration and purity of these impurities can be measured by ICP (inductively coupled plasma) emission spectrometry.

[0079] When a bonding material of a combination of Mg and Cu is used, it can be used in the same manner as when an active metal is used.

[0080] In the present embodiment, Mg foil 25 is disposed between the copper plate 22 and the ceramic substrate 11 and between the copper plate 23 and the ceramic substrate 11 .

[0081] In the Mg foil 25 , the total concentration of Al, Si, Zn, and Mn is limited to 1 mass % or less.

[0082] In the bonding material placement step S02, the amount of Mg to be placed was set to 7 μmol / cm 2 Above 143 μmol / cm 2 Within the following range.

[0083] (Lamination process S03)

[0084] Next, the copper plate 22 and the ceramic substrate 11 are stacked with the Mg foil 25 interposed therebetween, and the ceramic substrate 11 and the copper plate 23 are stacked with the Mg foil 25 interposed therebetween.

[0085] (Joining Step S04)

[0086] Next, the laminated copper plate 22 , Mg foil 25 , ceramic substrate 11 , Mg foil 25 , and copper plate 23 are pressed in the lamination direction and placed in a vacuum furnace for heating to bond the copper plate 22 , ceramic substrate 11 , and copper plate 23 .

[0087] The pressurizing load in the bonding step S04 is preferably set within a range of 0.049 MPa to 3.4 MPa.

[0088] The heating temperature in the bonding step S04 is preferably set in the range of 500° C. to 850° C. The holding time of the heating temperature is preferably set in the range of 5 min. to 180 min.

[0089] The vacuum degree in the bonding step S04 is preferably set at 1×10 -6 Pa or more and 5×10 -2 Within the range below Pa.

[0090] As described above, the insulating circuit substrate 10 of the present embodiment is manufactured through the ceramic substrate cleaning step S01 , the bonding material placement step S02 , the lamination step S03 , and the bonding step S04 .

[0091] (Heat sink bonding process S05)

[0092] Next, the heat sink 30 is bonded to the other surface of the metal layer 13 of the insulating circuit substrate 10 .

[0093] The insulating circuit substrate 10 and the heat sink 30 are stacked with solder interposed therebetween, and then placed in a heating furnace, whereby the insulating circuit substrate 10 and the heat sink 30 are solder-joined with each other via the solder layer 32 .

[0094] (Semiconductor element bonding step S06)

[0095] Next, the semiconductor element 3 is bonded to one surface of the circuit layer 12 of the insulating circuit substrate 10 by soldering.

[0096] Through the above process, Figure 1 The power module 1 is shown.

[0097] According to the insulating circuit substrate 10 (copper-ceramic joint body) of the present embodiment constructed as above, when the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is 100 atomic %, the total concentration of Al, Si, Zn and Mn is 3 atomic % or less when the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is 100 atomic %, so that the concentration of impurity elements (Al, Si, Zn and Mn) at the bonding interface is sufficiently low, and the precipitation of fine intermetallic compounds at the bonding interface can be suppressed, thereby suppressing the precipitation and solidification near the bonding interface between the ceramic substrate 11 and the circuit layer 12 (and the metal layer 13). Therefore, even when a severe thermal cycle is applied, the occurrence of cracks in the ceramic substrate 11 can be suppressed, and the insulating circuit substrate 10 with excellent thermal cycle reliability can be obtained.

[0098] In this embodiment, when the concentration of Al at the above-mentioned bonding interface is limited to less than 2 atomic %, or when the concentration of Si at the above-mentioned bonding interface is limited to less than 2 atomic %, and when the combined concentration of the above-mentioned Zn and Mn is limited to less than 2 atomic %, precipitation solidification near the bonding interface between the ceramic substrate 11 and the circuit layer 12 (and the metal layer 13) can be further suppressed.

[0099] In the present embodiment, in the ceramic substrate cleaning step S01, the bonding surface of the ceramic substrate 11 is cleaned, and in the bonding material configuration step S02, the total concentration of the impurities (Al, Si, Zn and Mn) of the provided Mg is limited to less than 1 mass %, thereby being able to limit the total concentration of the impurities (Al, Si, Zn and Mn) at the above-mentioned bonding interface to less than 3 atomic %.

[0100] In this embodiment, in the bonding material arrangement step S02, the amount of Mg is set to 7 μmol / cm 2 Above 143 μmol / cm 2 The following range is therefore possible to obtain a sufficient liquid phase required for the interface reaction.

[0101] Therefore, the insulating circuit substrate 10 (copper-ceramic bonded body) in which the copper plates 22 and 23 and the ceramic substrate 11 are reliably bonded can be obtained.

[0102] As mentioned above, although embodiment of this invention was described, this invention is not limited to this, It can change suitably within the range which does not deviate from the technical idea of ​​this invention.

[0103] For example, in this embodiment, a case where a semiconductor element is mounted on an insulating circuit substrate to form a power module is described, but the present invention is not limited thereto. For example, an LED element may be mounted on a circuit layer of an insulating circuit substrate to form an LED module, or a thermoelectric element may be mounted on a circuit layer of an insulating circuit substrate to form a thermoelectric module.

[0104] In the insulating circuit board of the present embodiment, the case where both the circuit layer and the metal layer are formed of a copper plate made of copper or a copper alloy has been described, but the present invention is not limited to this.

[0105] For example, when the circuit layer and the ceramic substrate are composed of the copper-ceramic joint body of the present invention, there is no limitation on the material or joining method of the metal layer. There may be no metal layer, the metal layer may be composed of aluminum or aluminum alloy, or may be composed of a laminate of copper and aluminum.

[0106] On the other hand, when the metal layer and the ceramic substrate are formed by the copper-ceramic joint body of the present invention, there is no limitation on the material or joining method of the circuit layer. The circuit layer can be formed by aluminum or aluminum alloy, or by a laminate of copper and aluminum.

[0107] In the insulating circuit substrate of this embodiment, an example of a ceramic substrate composed of aluminum nitride (AlN) is cited as an example for explanation, but it is not limited to this, and other ceramic substrates such as aluminum oxide (Al2O3) and silicon nitride (Si3N4) can also be used.

[0108] Example

[0109] Hereinafter, the results of confirmation experiments conducted to confirm the effects of the present invention will be described.

[0110] First, the ceramic substrates (40 mm×40 mm) listed in Tables 1 and 2 were prepared.

[0111] Regarding thickness, AlN and Al2O3 are 0.635 mm, and Si3N4 is 0.32 mm.

[0112] Then, the surface of the ceramic substrate was cleaned using the treatment liquids shown in Tables 1 and 2 under the following conditions.

[0113] In Tables 1 and 2, "HCl" means that hydrochloric acid having an HCl concentration of 12 mass % was used and the treatment was carried out at a treatment temperature of 35° C. and a treatment time of 5 minutes.

[0114] In Tables 1 and 2, "HNO 3 " means that an aqueous solution having a HNO 3 concentration of 10 mass % was used and the treatment was carried out at a treatment temperature of 35° C. and a treatment time of 7 minutes.

[0115] In Tables 1 and 2, "NaOH" means that an aqueous solution having a NaOH concentration of 1 mass % was used, and the treatment was carried out at a treatment temperature of 30° C. and a treatment time of 1 minute.

[0116] In Tables 1 and 2, "NaHCO 3 " means that an aqueous solution having a NaHCO 3 concentration of 1.5 mass % was used and the treatment was carried out at a treatment temperature of 30° C. and a treatment time of 1 minute.

[0117] In Comparative Examples 1, 3, 11, and 13, the cleaning process of the ceramic substrate was not performed.

[0118] In Comparative Examples 2 and 12, an aqueous solution having a HNO 3 concentration of 2 mass % was used, and the treatment was carried out at a treatment temperature of 35° C. and a treatment time of 20 minutes.

[0119] In Comparative Example 4, an aqueous solution having a NaOH concentration of 8% by mass was used, and the treatment was carried out at a treatment temperature of 30° C. and a treatment time of 3 minutes.

[0120] In Comparative Examples 5 and 14, hydrochloric acid having a HCl concentration of 3% by mass was used, and the treatment was carried out at a treatment temperature of 35° C. and a treatment time of 1 minute.

[0121] In Comparative Example 15, an aqueous solution having a NaHCO 3 concentration of 0.5 mass % was used, and the treatment was carried out at a treatment temperature of 30° C. and a treatment time of 3 minutes.

[0122] As described above, on both sides of the ceramic substrate subjected to the cleaning treatment, a copper plate (37 mm × 37 mm × 0.3 mm thick) made of oxygen-free copper was bonded to the ceramic substrate using the bonding materials shown in Tables 1 and 2 to obtain an insulating circuit substrate (copper-ceramic bonded body). The vacuum degree of the vacuum furnace during bonding was 3 × 10 -3 Pa, the bonding temperature was 800°C, the holding time was 60 minutes, and the press load was 0.98 MPa.

[0123] The purity of the raw materials of the respective elements used as the bonding material is shown in Tables 1 and 2. A foil material was used as the bonding material.

[0124] The obtained insulating circuit substrate (copper-ceramic bonded body) was evaluated as follows with respect to the impurity concentration near the bonding interface and the cracking of the ceramic substrate after thermal cycling.

[0125] (Impurity concentration at the bonding interface)

[0126] The concentration near the bonding interface between the copper plate and the ceramic substrate was measured using a scanning transmission electron microscope (Titan ChemiSTEM manufactured by FEI Corporation) and an EDS detector (NSS7 manufactured by ThermoScientific Corporation).

[0127] At an accelerating voltage of 200 kV, the concentration was measured by energy dispersive X-ray analysis at a position 1000 nm away from the bonding interface to the copper plate side, and the concentrations of active metals (Ti, Zr, Nb, Hf), Al, Si, Zn and Mn were measured when the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn was set to 100 atomic %. The measurement was performed at 5 locations, and the average value of the 5 measured locations was taken as the concentration of each element at the bonding interface. The evaluation results are shown in Tables 1 and 2.

[0128] (Cracks in ceramic substrate after thermal cycling)

[0129] According to the material of the ceramic substrate, after passing the furnace through the following atmosphere, the bonding interface between the copper plate and the ceramic substrate was inspected by SAT (scanning ultrasonic microscope) to determine whether the ceramic substrate was cracked.

[0130] Table 1 shows the evaluation results.

[0131] For AlN and Al2O3: 10 cycles of -78℃×2min←→350℃×2min

[0132] For Si3N4: 20 hot and cold cycles of -78℃×2min←→350℃×2min

[0133] [Table 1]

[0134]

[0135] *1The atomic ratio of each element when the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is taken as 100 atomic % by measuring the concentration by energy dispersive X-ray analysis at a position 1000 nm away from the bonding interface toward the copper plate side.

[0136] [Table 2]

[0137]

[0138] *1The atomic ratio of each element when the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is taken as 100 atomic % by measuring the concentration by energy dispersive X-ray analysis at a position 1000 nm away from the bonding interface toward the copper plate side.

[0139] In Comparative Examples 1 to 5 and Comparative Examples 11 to 15 in which the total concentration of Al, Si, Zn, and Mn exceeded 3 atomic % at the bonding interface, cracks in the ceramic substrate were observed after thermal cycling.

[0140] In Comparative Examples 1, 3, 11 and 13, the surface cleaning of the ceramic substrate was not performed, and the purity of the elements in the bonding material was low. Therefore, the total concentration of Al, Si, Zn and Mn at the bonding interface exceeded 3 atomic %, and cracks in the ceramic substrate were confirmed after hot and cold cycle loading.

[0141] In Comparative Examples 2, 4, 5, 12, 14 and 15, although surface treatment of the ceramic substrate was performed, the purity of the element (Mg) in the bonding material was low, so the total concentration of Al, Si, Zn and Mn exceeded 3 atomic % at the bonding interface, and cracks in the ceramic substrate were confirmed after hot and cold cycle loads.

[0142] On the other hand, in Inventive Examples 1 to 8 and Inventive Examples 11 to 18 in which the total concentration of Al, Si, Zn and Mn at the bonding interface was limited to 3 atomic % or less, no cracking of the ceramic substrate was confirmed after thermal cycle loading.

[0143] As shown in the above results, according to the present example, it is confirmed that a copper-ceramic bonded body having excellent thermal cycle reliability and capable of suppressing the occurrence of cracks in ceramic components even when subjected to severe thermal cycles can be provided, and an insulating circuit substrate composed of the copper-ceramic bonded body can be provided.

[0144] Industrial Applicability

[0145] According to the present invention, it is possible to provide a copper-ceramic bonded body which can suppress the occurrence of cracks in a ceramic component even when subjected to severe thermal cycles and has excellent thermal cycle reliability, and an insulating circuit board composed of the copper-ceramic bonded body.

[0146] Explanation of symbols

[0147] 10- insulating circuit substrate (copper-ceramic joint body), 11- ceramic substrate (ceramic component), 12- circuit layer (copper component), 13- metal layer (copper component).

Claims

1. A copper-ceramic joint body, wherein a copper component and a ceramic component are joined by a joint material including Mg alone or a combination of Mg and an active metal, wherein the copper component is made of copper or a copper alloy, wherein: When the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is set to 100 atomic %, the total concentration of Al, Si, Zn and Mn is 3 atomic % or less at a position 1000 nm away from the bonding interface between the copper component and the ceramic component toward the copper component side by energy dispersive X-ray analysis, The bonding is achieved by an interfacial reaction involving the generation of a liquid phase containing Mg.

2. The copper-ceramic joint body according to claim 1, characterized in that: The concentration was measured by energy dispersive X-ray analysis at a position 1000 nm away from the joining interface between the copper component and the ceramic component toward the copper component. When the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn was set to 100 atomic %, the concentration of Al was less than 2 atomic %.

3. The copper-ceramic joint body according to claim 1 or 2, characterized in that: The concentration was measured by energy dispersive X-ray analysis at a position 1000 nm away from the joining interface between the copper component and the ceramic component toward the copper component. When the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn was set to 100 atomic %, the concentration of Si was less than 2 atomic %.

4. The copper-ceramic joint body according to claim 1 or 2, characterized in that: The concentration was measured by energy dispersive X-ray analysis at a position 1000 nm away from the joining interface between the copper part and the ceramic part toward the copper part. When the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn was set to 100 atomic %, the total concentration of Zn and Mn was less than 2 atomic %.

5. An insulating circuit substrate, comprising a copper plate bonded to the surface of a ceramic substrate by a bonding material comprising Mg alone or a combination of Mg and an active metal, wherein the copper plate is made of copper or a copper alloy, wherein: When the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn is set to 100 atomic %, the total concentration of Al, Si, Zn and Mn is less than 3 atomic % at a position 1000 nm away from the bonding interface between the copper plate and the ceramic substrate toward the copper plate side by energy dispersive X-ray analysis, The bonding is achieved by an interfacial reaction involving the generation of a liquid phase containing Mg.

6. The insulating circuit substrate according to claim 5, characterized in that: The concentration was measured by energy dispersive X-ray analysis at a position 1000 nm away from the bonding interface between the copper plate and the ceramic substrate toward the copper plate side. When the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn was set to 100 atomic %, the concentration of Al was less than 2 atomic %.

7. The insulating circuit substrate according to claim 5 or 6, characterized in that: The concentration was measured by energy dispersive X-ray analysis at a position 1000 nm away from the bonding interface between the copper plate and the ceramic substrate toward the copper plate side. When the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn was set to 100 atomic %, the concentration of Si was less than 2 atomic %.

8. The insulating circuit substrate according to claim 5 or 6, characterized in that: The concentration was measured by energy dispersive X-ray analysis at a position 1000 nm away from the bonding interface between the copper plate and the ceramic substrate toward the copper plate side. When the total value of Cu, Mg, Ti, Zr, Nb, Hf, Al, Si, Zn and Mn was set to 100 atomic %, the total concentration of Zn and Mn was less than 2 atomic %.