A catalyst for the reaction of CO2 oxidation of propane to propylene
By preparing Fe-ZrO2 catalyst and adjusting its acid-base and phase state, the problems of unstable activity and low conversion rate of the existing catalyst are solved, and efficient conversion and selectivity of CO2 propane oxide to propylene reaction are achieved, and the preparation process is simplified. , reduces costs and is suitable for industrial applications.
Patent Information
- Application Number
- CN202210036288.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-01-13
AI Technical Summary
The existing CO2 propylene oxide propylene catalyst has unstable activity, low conversion rate, complex preparation method and high cost, resulting in limited industrial applications.
By mixing iron and zirconium sources with oxalic acid, the Fe-ZrO2 catalyst is prepared, the acid-base and phase state of the catalyst are adjusted, and the tetragonal ZrO2 phase of nano-scale particles is formed, which significantly increases the conversion rate of propane and CO2.
The high conversion and selectivity of the CO2 propane oxide-based propylene reaction is achieved, the catalyst activity is stable, the preparation method is simple, the cost is low, and it is suitable for industrial applications.
Smart Images

Figure CN114345343B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalyst preparation, and specifically relates to a catalyst for preparing propylene by oxidizing propane with CO2 and a preparation method thereof. Background Art
[0002] Propylene is an important raw material for the production of chemicals such as acrolein, polypropylene, acetone, acrylonitrile, and propylene oxide. The main industrial sources are steam cracking, catalytic cracking, olefin disproportionation, etc. With the increasing demand, other propylene production routes have attracted attention, such as propane dehydrogenation and methanol to propylene. Due to the limitation of thermodynamic equilibrium, the single-pass conversion rate of propane dehydrogenation process is less than 50%. The CO2 atmosphere oxidation propane dehydrogenation to propylene reaction theoretically has the potential to increase the single-pass conversion rate of propylene. At the same time, this process method helps to convert CO2 into chemicals and promote the recycling of CO2. In addition, CO2 can react with carbon deposits on the surface of the catalyst to achieve carbon removal, thereby extending the life of the catalyst.
[0003] Supported CrO prepared by impregnation method x / SiO2 catalyst at C3H8 / CO2=1 / 3.6, 650 °C, 2800 h -1 and 1atm reaction conditions, the conversion rates of propane and CO2 were 29.1% and 5.5%, respectively, and the selectivity of propylene and methane were 88.7% and 11.3%, respectively (Journal of Inorganic Chemistry, 2000, Vol. 16, pp. 77-782). The Cr / ZrO2 catalyst prepared by hydrothermal and microwave methods had a propane and CO2 conversion rate of 58% and 33%, respectively, and a propylene selectivity of 55%, under the reaction conditions of C3H82.5%, CO26.5%, He91%, 20 mL / min, 550 °C, and 1atm (Applied Catalysis A: General, 2018, Vol. 558). Patent CN109126855B discloses a supported GaN catalyst and its use in CO2 oxidation propane dehydrogenation reaction. The solid gallium source and nitrogen source are mixed with the carrier, dispersed by ultrasonic solvent and dried, and then calcined twice in an inert atmosphere and air atmosphere to obtain the catalyst. At V(C3H8):V(CO2):V(N2)=1:2:7, 9000 mL·h -1 ·g -1 , 600 °C, 0.1 MPa reaction conditions, when the loading is 5%, the propane conversion rate is as high as 31%. nV-MCM-41 catalyst prepared by one-step hydrothermal synthesis, V is doped into the framework of MCM-41, under C3H8 / CO2 / Ar=1 / 4 / 4, 600 °C, 1 h -1Under the reaction conditions of 1 atm, the 6.8V-MCM-41 catalyst showed the highest activity, with an initial propane conversion of 58% and a propylene selectivity of 92%. Due to the reduction changes of the active sites and carbon accumulation on the catalyst surface, the conversion rate dropped to 35% after 2 h of reaction (Journal of Catalysis, 2018, Vol. 39, pp. 1099-1109). x / Al2O3 catalyst has an initial propane conversion rate of 73%. Due to coking on the catalyst surface and covering the active centers, the conversion rate dropped to 25% after 8 hours of reaction (Applied Catalysis B: Environmental, 2020, Vol. 274, p. 119089). From the above analysis, the speed of substances entering and exiting the active sites in the catalyst micropores is usually slow, so the residence time is long, which will increase propylene polymerization and coke formation, and the CO2 oxidation of propane to propylene reaction has problems such as low raw material conversion rate and unstable catalyst activity. In addition, the complicated preparation method is costly and is not conducive to industrial application. Summary of the invention
[0004] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a catalyst for the oxidation of propane to propylene by CO2, which has the characteristics of simple preparation method, environmental friendliness, low cost and high activity.
[0005] The catalyst for preparing propylene by oxidation of propane with CO2 synthesized by the present invention is realized by the following steps:
[0006] (1) mixing an iron source, a zirconium source and alcohol to obtain a solution 1, and mixing oxalic acid and alcohol to obtain a solution 2;
[0007] (2) At a certain temperature, add solution 1 dropwise into solution 2, and continue stirring for aging;
[0008] (3) Drying and calcining the aged uniform gel to obtain the product.
[0009] In the above step (1), n(Fe):n(Zr)=1:1-4, n(Fe+Zr):n(alcohol)=1:20-60, n(oxalic acid):n(alcohol)=1:4-10.
[0010] In the above step (1), the iron source is selected from one of ferric nitrate, ferric sulfate and ferric chloride.
[0011] In the above step (1), the zirconium source is selected from one of zirconium nitrate, zirconyl nitrate and zirconium acetate.
[0012] In the above step (1), the alcohol is selected from one of methanol and anhydrous ethanol.
[0013] In the above step (2), the certain temperature is 50-60°C.
[0014] The aging time in the above step (2) is 4 to 6 h.
[0015] In the above step (3), the drying temperature is 100-120°C and the drying time is 12 h.
[0016] In the above step (3), the calcination temperature is 550-600°C and the calcination time is 4 h.
[0017] The Fe-ZrO2 system catalyst prepared by the present invention is used for the first time in the reaction of CO2 oxidation of propane to propylene. Through the interaction between the iron source and the zirconium source, the acidity and alkalinity of the catalyst are adjusted with the assistance of oxalic acid, and the phase state of ZrO2 can be stabilized as a tetragonal phase, which is beneficial to the adsorption of propane and CO2, and significantly improves the conversion rate of propane and CO2.
[0018] The particle size and acidity of the catalyst in the present invention are well controlled. The catalyst system contains nano-sized particles with a grain size of 3.6 to 5.1 nm. The catalyst provides a suitable acidity for the system by the preparation method and ZrO2, with a weak acid content of 0.046 to 0.087 mmol·g -1 , medium-strong acid content 0.001~0.004 mmol·g -1 , effectively improving the catalytic performance.
[0019] The specific application method of the catalyst for preparing propylene by oxidizing propane with CO2 prepared by the present invention in the reaction is as follows: 1 g of Fe-ZrO2 catalyst is loaded into a micro fixed bed reactor, the temperature is raised to 600 °C in an Ar atmosphere, CO2 and propane are introduced according to n(C3H8) / n(CO2) / n(Ar)=1 / 1 / 1.5, W / F=20 g‧h / mol, 0.1 MPa conditions, and the reaction of preparing propylene by oxidizing propane with CO2 is carried out. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 : Example 1 Preparation of Fe-3ZrO2 sample XRD spectrum.
[0021] Figure 2 :The activity of Fe-ZrO2 catalyst in the oxidation of propane to propylene by CO2. DETAILED DESCRIPTION
[0022] The technical solution of the present invention is further described below by way of embodiments in conjunction with the accompanying drawings:
[0023] Example 1
[0024] According to n(Fe):n(Zr)=1:3, n(Fe+Zr):n(ethanol)=1:40, n(oxalic acid):n(ethanol)=1:8. 4.0430g Fe(NO3)3·9H2O and 12.8791 g Zr(NO3)4·5H2O were dissolved in 60 mL of anhydrous ethanol to obtain solution 1, and 20.1592 g H2C2O4·2H2O was dissolved in 40 mL of anhydrous ethanol to obtain solution 2. Stirring continuously at 50°C, solution 2 was added dropwise to solution 1, and stirring was continued for 4 h after the addition. The uniform gel was dried at 110°C for 12 h, and calcined at 600°C in air atmosphere for 4 h to obtain the catalyst Fe-3ZrO2. The grain size is 3.8 nm, and the weak acid content is 0.067 mmol·g -1 , medium-strong acid content 0.0037mmol·g -1 .
[0025] The inventors used an X-ray diffractometer to characterize the Fe-3ZrO2 catalyst prepared in Example 1. The results are as follows: Figure 1 As shown in the XRD diagram, the diffraction peaks at 30.4°, 35.2°, 50.6°, and 60.3° belong to the tetragonal (t) ZrO2 phase (PDF#29-0997), and there is no α-Fe2O3 diffraction peak, indicating that Fe2O3 is well dispersed on the support surface.
[0026] Example 2
[0027] According to n(Fe):n(Zr)=1:2, n(Fe+Zr):n(ethanol)=1:30, n(oxalic acid):n(ethanol)=1:6. 4.0455g Fe(NO3)3·9H2O and 8.5824 g Zr(NO3)4·5H2O were dissolved in 56 mL of anhydrous ethanol to obtain solution 1, and 12.1251g H2C2O4·2H2O was dissolved in 35 mL of anhydrous ethanol to obtain solution 2. Stirring continuously at 55 °C, solution 2 was added dropwise to solution 1, and stirring was continued for 5 h after the addition. The uniform gel was dried at 110 °C for 12 h and calcined at 600 °C in air atmosphere for 4 h to obtain the catalyst Fe-2ZrO2. The grain size is 3.6 nm, and the weak acid content is 0.073 mmol·g -1 , medium-strong acid content 0.002 mmol·g -1 .
[0028] Example 3
[0029] According to n(Fe):n(Zr)=1:1, n(Fe+Zr):n(ethanol)=1:20, n(oxalic acid):n(ethanol)=1:4. 4.0489g Fe(NO3)3·9H2O and 4.3017 g Zr(NO3)4·5H2O were dissolved in 50 mL of anhydrous ethanol to obtain solution 1, and 10.08 g H2C2O4·2H2O was dissolved in 30 mL of anhydrous ethanol to obtain solution 2. Stirring was continued at 50°C, and solution 2 was added dropwise to solution 1. After the addition, stirring was continued for 4 h. The uniform gel was dried at 110 °C for 12 h and calcined at 600 °C in air atmosphere for 4 h to obtain the catalyst Fe-1ZrO2. The grain size was 4.9 nm and the weak acid content was 0.046 mmol·g -1 , medium-strong acid content 0.0028 mmol·g -1 .
[0030] Example 4
[0031] According to n(Fe):n(Zr)=1:4, n(Fe+Zr):n(ethanol)=1:60, n(oxalic acid):n(ethanol)=1:10. 4.0485g Fe(NO3)3·9H2O and 17.1790 g Zr(NO3)4·5H2O were dissolved in 70 mL of anhydrous ethanol to obtain solution 1, and 25.1275 g H2C2O4·2H2O was dissolved in 45 mL of anhydrous ethanol to obtain solution 2. Stirring was continued at 60°C, and solution 2 was added dropwise to solution 1. After the addition, stirring was continued for 5 h. The uniform gel was dried at 110 °C for 12 h, and calcined at 600 °C in air atmosphere for 4 h to obtain the catalyst Fe-4ZrO2. The grain size is 5.1 nm, and the weak acid content is 0.084 mmol·g -1 , medium-strong acid content 0.001mmol·g -1 .
[0032] Example 5
[0033] According to n(Fe):n(Zr)=1:3, n(Fe+Zr):n(ethanol)=1:40, n(oxalic acid):n(ethanol)=1:8. 4.0430g Fe(NO3)3·9H2O and 12.8791 g Zr(NO3)4·5H2O were dissolved in 60 mL of anhydrous ethanol to obtain solution 1, and 20.1592 g H2C2O4·2H2O was dissolved in 40 mL of anhydrous ethanol to obtain solution 2. Stirring was continued at 60 °C, and solution 2 was added dropwise to solution 1. After the addition was completed, stirring was continued for 5 h. The uniform gel was dried at 100 °C for 12 h and calcined at 550 °C for 4 h in an air atmosphere to obtain the catalyst Fe-3ZrO2. The grain size is 3.9 nm, and the weak acid content is 0.065 mmol·g -1, medium-strong acid content 0.0022mmol·g -1 .
[0034] Example 6
[0035] 1 g of the Fe-3ZrO2 catalyst prepared in Example 1 was loaded into a fixed bed reactor, the Ar atmosphere was heated to 600 °C, CO2 and propane were introduced at n(C3H8) / n(CO2) / n(Ar)=1 / 1 / 1.5, W / F=20 g‧h / mol, 0.1 MPa, and CO2 oxidation propane dehydrogenation reaction was carried out. The results are shown in FIG. Figure 2 The initial propane and CO2 conversions were 56.3% and 47.9%, respectively, and the propylene and CO selectivities were 80.1% and 24.9%, respectively.
[0036] Example 7
[0037] Similar to Example 6, 1 g of the Fe-2ZrO2 catalyst prepared in Example 2 was loaded into a fixed bed reactor. The results of the CO2 oxidation propane dehydrogenation reaction were as follows: Figure 2 The initial propane and CO2 conversions were 55.8% and 45.6%, respectively, and the propylene and CO selectivities were 84.3% and 21.3%, respectively.
[0038] Example 8
[0039] Similar to Example 6, 1 g of the Fe-1ZrO2 catalyst prepared in Example 3 was loaded into a fixed bed reactor to carry out CO2 oxidation propane dehydrogenation reaction. Figure 2 The initial propane and CO2 conversions were 56.3% and 47.9%, respectively, and the propylene and CO selectivities were 85.2% and 19.1%, respectively.
[0040] Example 9
[0041] Similar to Example 6, 1 g of the Fe-4ZrO2 catalyst prepared in Example 4 was loaded into a fixed bed reactor to carry out CO2 oxidation propane dehydrogenation reaction. Figure 2 The initial propane and CO2 conversions were 54.2% and 46.2%, respectively, and the propylene and CO selectivities were 83.2% and 22.1%, respectively.
Claims
1. A catalyst is used for the reaction of CO2 oxidation of propane to propylene, characterized in that The catalyst is applied to CO2 oxidation of propane to propylene, the reaction temperature is 600 °C, CO2 and propane are introduced according to the molar ratio of n(C3H8) / n(CO2) / n(Ar)=1 / 1 / 1.5, W / F=20 g‧h / mol, 0.1 MPa, and the CO2 oxidation of propane to propylene is carried out; the metal elements in the catalyst applied to the CO2 oxidation of propane to propylene reaction include Fe and Zr, and the catalyst includes tetragonal ZrO2; the catalyst is realized by the following steps: (1) Mixing an iron source, a zirconium source and an alcohol at a molar ratio of n(Fe+Zr):n(alcohol)=1:20-60 to obtain a solution 1, and mixing oxalic acid and an alcohol at a molar ratio of n(oxalic acid):n(alcohol)=1:4-10 to obtain a solution 2; (2) At a temperature of 50-60°C, add solution 1 dropwise into solution 2 while stirring continuously for aging; (3) After aging, the product is dried and roasted.
2. The catalyst according to claim 1 is used in the reaction of CO2 oxidation of propane to propylene, characterized in that: In the solution 1 of step (1), n(Fe):n(Zr)=1:1-4.
3. The catalyst according to claim 1 is used in the reaction of CO2 oxidation of propane to propylene, characterized in that: The alcohol in step (1) is selected from one of methanol and anhydrous ethanol.
4. The catalyst according to claim 1 is used in the reaction of CO2 oxidation of propane to propylene, characterized in that: In step (1), the iron source is selected from one of ferric nitrate, ferric sulfate and ferric chloride; the zirconium source is selected from one of zirconium nitrate, zirconyl nitrate and zirconium acetate.
5. The catalyst according to claim 1 is used in the reaction of CO2 oxidation of propane to propylene, characterized in that: The aging time in step (2) is 4 to 6 h; the drying temperature in step (3) is 100 to 120 °C and the drying time is 12 h.
6. The catalyst according to claim 1 is used in the reaction of CO2 oxidation of propane to propylene, characterized in that: In step (3), the calcination temperature is 550-600°C and the calcination time is 4 h.