A device and method for controlling the etching rate of a magnetron sputtering cathode target.

By designing the magnetron sputtering cathode target etching rate control device in magnetron sputtering coating technology, and adjusting the magnetic field distribution using permanent magnets and magnetic field moving devices, the problems of uneven etching rate of cathode target and fluctuation of discharge parameters are solved. , the stability of coating quality and consistency of etching rate are achieved, and the utilization rate of target materials is improved.

CN114381705BActive Publication Date: 2024-11-08TAIAN DONGDA NEW MATERIAL SURFACE TECH CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111611465.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-27
Publication Date
2024-11-08
Estimated Expiration
2041-12-27

AI Technical Summary

Technical Problem

In magnetron sputtering coating technology, the uneven etching rate of cathode target and fluctuation of discharge parameters make it difficult to ensure the coating quality and target utilization, especially in the precision coating process, there are challenges in properties and uniformity.

Method used

A control device for the etching rate of magnetron sputtering cathode target is designed, including a target module, a constant voltage power supply and a magnetic field module. Using permanent magnets and magnetic field moving devices, the position of magnets and magnetic inductance lines are adjusted to control the real-time control by adjusting the position of magnets and the trajectory of magnets. The magnetic field distribution and ion flow density of the target material achieve uniformity and stability of the etching rate.

Benefits of technology

By precisely controlling the magnetic field distribution and magnetic inductive line trajectory, the ion bombardment energy during the target etching process is ensured, the stability of coating quality and the consistency of etching rate are achieved, and the utilization rate of target materials and the precision of coating process is improved. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114381705B_ABST
    Figure CN114381705B_ABST
Patent Text Reader

Abstract

The present invention relates to a control device and a control method for the etching rate of a cathode target material of a magnetron sputtering device. The control device comprises: a target, a constant voltage power supply, and a magnetic field module arranged behind the target. The magnetic field module comprises a permanent magnet and a control module. The permanent magnet changes its position according to different control parameters input by the control module, that is, changes the distance between the magnet and the target. The cathode target material etching rate control method of the present invention adopts a constant voltage power supply to provide a constant cathode discharge voltage so that the energy of ions bombarding the target surface during the discharge process is constant. The magnetic field distribution is adjusted by changing the position of the permanent magnet to ensure that the ion flow density bombarding the target surface is relatively constant, thereby enhancing the stability of the etching speed and the coating quality during the target material etching process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a magnetron sputtering coating technology, and in particular to a control device and a control method for a magnetron sputtering cathode target material etching rate. Background Art

[0002] Magnetron sputtering coating technology is the main coating technology used in the field of functional films such as semiconductor device films, superconducting films, information display device films, energy-saving glass films, transparent conductive glass films, etc. It is also the main coating technology used in the field of decorative films such as mobile phone and watch shell films, colored glass curtain wall films, and glasses frame surface films. This technology relies on electric field ionization of gas to produce gas ions and electrons, and uses magnetic field to bind electrons within a certain range, so that the local electron density increases, which in turn ionizes more gas ions. At the same time, the cathode with negative potential attracts ions to bombard the target surface to achieve target material etching, bombarding target atoms or atomic groups, and finally depositing them on the substrate surface, so as to obtain a dense film without much temperature rise. Usually, the magnetic field distribution above the cathode target surface is uneven, which will lead to uneven etching of the target material. Specifically, the discharge parameters of the same target material will change in different etching stages, and the etching rate will also change.

[0003] In response to this problem, many experts and scholars have done a lot of research work to enhance the stability of the magnetron sputtering coating process.

[0004] Patent CN211112196U discloses a magnetic source structure for a magnetron sputtering cathode. The patent adopts a method in which transverse magnets and longitudinal magnets are arranged alternately and perpendicular to each other. The magnetic poles of adjacent longitudinal magnets are opposite, and the magnetic poles of adjacent longitudinal magnets and transverse magnets are the same. Compared with the conventional magnet arrangement method, this arrangement of transverse magnets and longitudinal magnets can effectively enhance the magnetic field strength near the cathode target surface; and the position of the transverse magnet is adjustable, and the distribution of the magnetic field on the target surface can be changed according to specific needs, thereby enhancing the uniformity and consistency of the magnetic field distribution, and the target material can be evenly sputtered to improve the utilization rate. However, this structure adopts the method in which adjacent magnetic poles are the same, and the magnets used in magnetron targets are mostly strong magnets. Therefore, the actual installation process will cause great difficulties due to the magnetic pole repulsion; and in the specific process, it is also difficult to adjust the position of the transverse magnet, which is somewhat disconnected from the actual production.

[0005] Patent CN201162043Y discloses a magnetron sputtering target structure and equipment, including: a transmission device, at least two rotating shafts and multiple magnetic target strips; the transmission device is wound around the rotating shaft to form a transmission mechanism; the magnetic target strips are arranged side by side on the transmission device, and the target material is located outside the transmission mechanism. Although this technology uses a transmission device to drive the magnet to perform regular periodic motion to form a parallel uniform magnetic field, avoiding the problem of excessive local loss leading to premature scrapping of the target material, this technology only focuses on the uniformity of the overall etching track of the target material, and does not consider the problem of etching rate changes during the etching process, so it is impossible to achieve the consistency of the etching rate during the etching process of the target material.

[0006] At present, the main research purpose of most scholars is to improve the utilization rate of target materials. However, in fact, for some more precise coating processes, ensuring the properties and uniformity of the thin film itself obtained at each stage of coating is more important than the utilization rate of target materials. Currently, there are few patents involving this issue. Summary of the invention

[0007] The present invention provides a control device and a control method for the etching rate of a magnetron sputtering cathode target material, so as to solve the problems of uneven etching rate of the target material and parameter fluctuation during the discharge process existing in the prior art.

[0008] As a first aspect of the present invention, there is provided a control device for the etching rate of a magnetron sputtering cathode target material, characterized in that the structure includes a target module, a constant voltage power supply, and a magnetic field module arranged behind the target module. The target module includes a target material, a water-cooled back plate, a mounting plate, an outer shell and an upper cover plate. The magnetic field module includes a permanent magnet and a control module, and the control module is mainly composed of a magnetic field moving device. The permanent magnet and the magnetic field moving device are arranged inside the outer shell and bear the weight on the upper cover plate; a yoke is also arranged inside the outer shell, and the position of the yoke is controlled by the magnetic field moving device; the water-cooled back plate is fixed on the mounting plate for water cooling the target material; the target material is fixed on the water-cooled back plate, and the entire cathode is fixed on the vacuum chamber through the mounting plate; a through hole is left on the upper cover plate for installing and connecting the power supply and the water cooling pipe inlet and outlet. After connection, a plastic cover is used to cover the through hole to ensure safety.

[0009] In the device for controlling the etching rate of the magnetron sputtering cathode target material of the present invention, the magnetic field moving device is entirely arranged in the outer shell.

[0010] In the control device for the etching rate of the cathode target material of the magnetron sputtering of the present invention, the upper cover plate is fixed to the outer shell by bolts, and the outer shell is fixed to the mounting plate by bolts. A cylindrical magnet mounting seat and a terminal are also arranged inside the outer shell, and the cylindrical magnet mounting seat and the bottom end of the terminal are fixed to the mounting plate, and the terminal is arranged on the back of the water-cooled back plate and connected to the constant voltage power supply.

[0011] In the control device for the etching rate of the magnetron sputtering cathode target of the present invention, the permanent magnet includes a bar magnet and a cylindrical magnet. The bar magnets are all fixed on the yoke and move synchronously with the yoke; the cylindrical magnet is fixed in the cylindrical magnet mounting seat and can move independently.

[0012] In the control device for the etching rate of the magnetron sputtering cathode target of the present invention, the working principles of the bar magnet and the cylindrical magnet are similar, the bar magnet includes an outer ring bar magnet and a middle bar magnet, the polarity of the outer ring bar magnet is opposite to that of the middle bar magnet and the cylindrical magnet, the bar magnet is moved by a micrometer knob type precision slide, not only the moving distance of the magnet can be understood in real time, but also the distribution of the magnetic field on the target surface and the magnitude of the magnetic field intensity can be controlled, the trajectory of the magnetic flux lines can be controlled, and the ion flow density can be affected. Thus, the ion flow density bombarding the target surface is ensured to be relatively constant.

[0013] Preferably, the outer ring bar magnet is attached to the edge of one side of the yoke, and the middle bar magnet is fixed in the middle position of the yoke and maintained at the same height as the outer ring bar magnet; the outer ring bar magnet, the middle bar magnet and the yoke move as a whole through the linear bearing.

[0014] In the device for controlling the etching rate of the magnetron sputtering cathode target material of the present invention, the magnetic field moving device comprises a linear bearing, a slide bar, a magnet mounting seat and a micrometer knob type precision slide table.

[0015] Furthermore, the linear bearing includes a feed bearing for controlling the reciprocating movement of the bar magnet and the cylindrical magnet respectively; and also includes a load-bearing bearing.

[0016] Furthermore, the micrometer knob type precision slide comprises a first micrometer knob type precision slide for feeding cylindrical magnets and a second micrometer knob type precision slide for feeding bar magnets.

[0017] The feed bearing for controlling the reciprocating movement of the bar magnet is passed through by the feed slide bar, and the top end of the slide bar of the feed bearing passes through the upper cover plate and is connected to the first micrometer knob type precision slide through the clamping plate for feeding the bar magnet, and the other end is connected to the mounting plate through a mounting seat; the cylindrical magnet is arranged in the cylindrical magnet mounting seat, and the feed bearing for controlling the reciprocating movement of the cylindrical magnet is passed through by the feed slide bar, and the top end of the slide bar of the feed bearing passes through the upper cover plate and is connected to the second micrometer knob type precision slide through the clamping plate for feeding the cylindrical magnets at both ends, and the other end is connected to the cylindrical magnet mounting seat through a mounting seat. In the control device for the etching rate of the magnetron sputtering cathode target material of the present invention, the back of the water-cooled back plate is provided with water inlet and outlet pipes; the water circuit design of the water-cooled back plate adopts a water circuit scheme of water inlet from the lower left corner of the water-cooled plate and water outlet from the upper right corner to fully cool the entire target surface.

[0018] In the device for controlling the etching rate of the magnetron sputtering cathode target of the present invention, a wire terminal is provided on the back of the water-cooled back plate for connecting to a constant voltage power supply to realize power supply to the cathode.

[0019] In the device for controlling the etching rate of the magnetron sputtering cathode target of the present invention, the target is fixed on a water-cooled back plate, and different fixing methods such as welding, bolt fixing, etc. can be adopted according to the different materials of the target.

[0020] The present invention controls two cylindrical magnets through two separate linear bearings, plus a linear bearing previously used to control the overall bar magnet. The present invention has a total of three linear bearings, which control the magnets to move back and forth. At the same time, the distance moved is read through the indication of the micrometer knob. Controlling the movement of the magnets also controls the magnetic flux lines, the magnitude and direction of the magnetic induction intensity, and thus controls the movement of the plasma in the cavity during the experiment, and thus controls the etching rate. Among them, the etching rate is also controlled by the size of the current displayed in the device. The voltage is in a constant voltage mode and remains unchanged. The current size is controlled by feedback using the position of the moving magnet.

[0021] As a second aspect of the present invention, a method for controlling the etching rate of a magnetron sputtering cathode target material is also provided, comprising: setting a position magnetic field module behind the target, the magnetic field module comprising a permanent magnet and a control module, adjusting the control parameters input into the control module to change the position of the permanent magnet, that is, the distance between the magnet and the target, adjusting the magnetic field distribution, and thereby achieving control of the target material etching rate.

[0022] In the method for controlling the etching rate of a magnetron sputtering cathode target material of the present invention, the permanent magnets are distributed in an axisymmetric manner, and the two symmetric planes correspond to and overlap with the two symmetric planes of the rectangular target respectively.

[0023] In the method for controlling the etching rate of the magnetron sputtering cathode target material of the present invention, the control strategy inputted by the adjustment control module is: constant discharge voltage, adjustment of the position of the permanent magnet, and stabilization of the discharge current.

[0024] In the method for controlling the etching rate of a magnetron sputtering cathode target material of the present invention, the control module includes a device for manually / electrically controlling the movement of the magnetic field.

[0025] The method for controlling the etching rate of the magnetron sputtering cathode target material comprises the following steps:

[0026] Step 1: Arrange the magnetic field structure using the control device for magnetron sputtering cathode target etching rate provided in Example 1;

[0027] Step 2: Determine the total input power Wa, record the positions Xb and Xc of the bar magnet and the cylindrical magnet and the initial target current I0, and start the experiment;

[0028] Among them, Wa = W0 + UIT, Wa is the expected total input power, which is a known number; W0 is the initial power, which is a known number; U is the constant voltage, I is the current monitored in real time, and T is the etching time;

[0029] Step 3: Check whether the current total input power Wa is less than the expected total input power;

[0030] If yes, then an etching experiment with constant voltage and power is performed;

[0031] If not, end the experiment;

[0032] Step 4: During the etching experiment, check whether the current is within the range of I0±0.5A;

[0033] If yes, record the current data of Xb, Xc, I and Wa, and return to step 2;

[0034] If not, adjust the positions Xb and Xc of the bar magnet and the cylindrical magnet, and then recheck whether the current is within the range of I0±0.5A.

[0035] The above technical solution has at least the following beneficial effects: the method for controlling the etching rate of the magnetron sputtering cathode target of the present invention adopts a constant voltage power supply mode according to the target material, gas type, and specific process requirements, and adjusts the position of the permanent magnet manually or electrically. It can achieve constant energy of ions bombarding the target surface during the target material etching process, stable ion flow bombarding the target surface, and achieve the goal of uniform target material etching during the entire process.

[0036] The invention discloses a method for controlling the etching rate of a magnetron sputtering cathode target material, wherein a bar magnet and a cylindrical magnet are arranged, wherein the bar magnet controls the straight part of the target material etching track, and the cylindrical magnet controls the curved part of the target material etching. The two magnets move independently, thereby ensuring that the etching rates of the straight and curved parts of the target material etching track are relatively consistent, making the energy of ions bombarding the target surface constant during the discharge process, and ensuring the stability of the etching speed and coating quality of the target material during the etching process.

[0037] By adopting the control device and control method of the present invention, the target material etching rate can be controlled very accurately, the cost is low, the discharge parameters are stable, and the consistency of the target material etching rate can be effectively increased. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0039] Figure 1 The overall structure diagram of the control device of the present invention;

[0040] Figure 2 The internal structure diagram of the control device of the present invention after the upper cover plate and the outer shell are hidden;

[0041] Figure 3 The upper cover plate view and AA cross-sectional view of the control device of the present invention, wherein (a) is the upper cover plate view, and (b) is the AA cross-sectional view of (a);

[0042] Figure 4 The waterway board diagram of the control device of the present invention;

[0043] Figure 5 The permanent magnet arrangement diagram of the control device of the present invention;

[0044] Figure 6 It is a schematic diagram of the yoke structure of the present invention;

[0045] Figure 7 Interceptor segment position diagram;

[0046] Figure 8a Variation diagram of horizontal magnetic field on the target surface at different magnet positions;

[0047] Figure 8b Variation diagram of vertical magnetic field on the target surface at different magnet positions;

[0048] Figure 9a Variation diagram of horizontal magnetic field on target surface curve at different magnet positions;

[0049] Figure 9b Variation diagram of vertical magnetic field on target surface curve at different magnet positions;

[0050] Fig.10 Description of magnetic field name;

[0051] Fig.11 Etching experiment flow chart;

[0052] Fig.12 The discharge current changes with the target material etching process.

[0053] Among them: 1-mounting plate; 2-water cooling back plate; 3-outer shell; 4-water inlet pipe; 5-terminal; 6-target material; 7-yoke iron; 9-load-bearing bearing; 11-upper cover plate; 12-load-bearing slide bar, 13-feed slide bar; 14-cylindrical magnet mounting seat; 15-feed bearing; 18-middle bar magnet; 19-cylindrical magnet; 20-baffle; 21-first micrometer knob type precision slide; 22-second micrometer knob type precision slide; 23-anti-electric shield; 24-outer ring bar magnet. DETAILED DESCRIPTION

[0054] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0055] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0056] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0057] Embodiment 1: A device for controlling the etching rate of a cathode target material in magnetron sputtering

[0058] like Figure 1 As shown, the control device for the etching rate of the cathode target material of the magnetron sputtering of the present invention comprises a mounting plate 1, a water-cooled back plate 2, an outer shell 3 and an upper cover plate 11; the mounting plate 1, the outer shell 3 and the upper cover plate 11 form a cube, and the water-cooled back plate 2 is located outside the mounting plate 1; the upper cover plate 11 is provided with two first micrometer knob type precision slides (feed cylindrical magnets) 21 for feeding cylindrical magnets, one second micrometer knob type precision slide 22 for feeding bar magnets, and the second micrometer knob type precision slide 22 for feeding bar magnets. The ruler knob type precision slide 22 is located in the middle of the upper cover plate 11, and the first micrometer knob type precision slide 21 is located at both ends of the upper cover plate 11; a water inlet pipe 4 is arranged on the water-cooled back plate 2, and correspondingly, a water outlet pipe is arranged on the other side of the water-cooled back plate, and the water inlet pipe 4 is diagonally distributed with the water outlet pipe to achieve sufficient cooling; a target material 6 is arranged on the outside of the water-cooled back plate 2, and a baffle 20 is arranged at the bottom of the target material 6, and the target material is fixed on the water-cooled back plate, and the entire cathode is fixed on the vacuum chamber through a mounting plate.

[0059] The upper cover plate is fixed to the outer shell by bolts, and the outer shell is fixed to the mounting plate by bolts.

[0060] like Figure 2 As shown, the outer shell 3 is provided with a load-bearing bearing 9, a feed bearing 15, a cylindrical magnet mounting seat 14 and a terminal 5; the bottom ends of the cylindrical magnet mounting seat 14 and the terminal 5 are fixed on the mounting plate 1;

[0061] In addition, if Figure 3 and Figure 5As shown, the outer shell is provided with a yoke 7, a middle bar magnet 18, a cylindrical magnet 19 and an outer ring bar magnet 24, wherein the outer ring bar magnet has opposite magnetic polarity to the middle bar magnet; the cylindrical magnet 19 is arranged in the cylindrical magnet mounting seat 14; wherein all magnets have the same height and material, and are made of neodymium iron boron material, and the magnetic field size is controlled by adjusting the feeding distance between the bar magnet (including the middle bar magnet 18 and the outer ring bar magnet 24) and the cylindrical magnet 19 to achieve an unbalanced magnetic field or a balanced magnetic field, and when the feeding distances of each magnet are the same, it is a balanced magnetic field; the middle bar magnet 18 and the outer ring bar magnet 24 are fixed on the yoke 7. Specifically, the outer ring bar magnet 24 is attached to the edge of one side of the yoke 7 for one circle, and the middle bar magnet 18 is fixed in the middle position of the yoke 7 and keeps the same height as the outer ring bar magnet 24; the outer ring bar magnet, the middle bar magnet and the yoke move as a whole through the linear bearing.

[0062] The feed bearing is a linear bearing, and its function is to ensure the reciprocating movement of the bar magnet. At the same time, a micrometer knob precision slide is provided at the end of the linear bearing, which can be moved by the micrometer knob to control the feed distance. The load-bearing bearing is a linear bearing, which is used to share the weight of the cathode structure to prevent the cathode structure from being too heavy. If only three feed structure supports are applied, and a knob-type micrometer is installed on the feed structure, on the one hand, it will cause errors in the micrometer readings during feeding, and on the other hand, the weight of the support structure is not enough, resulting in structural instability and failure of the cathode structure. At the same time, in order to ensure the safety of the load-bearing bearing setting, an anti-electric shield is added to the outer shell to avoid electric shock accidents. Other structures can be designed to replace, but insulation measures must be ensured, and the yoke iron part of the cathode structure must be connected and supported with the outer shell to ensure structural stability and support.

[0063] There are 6 load-bearing bearings 9 for bearing the load of the entire magnetic field structure. The load-bearing bearings 9 are sleeved on the load-bearing slide bar 12, and the top end of the slide bar is fixed to the upper cover plate 11, and the bottom end is fixed to the mounting plate 1; a protective electric cover 23 is provided at the connection between the load-bearing bearing 9 and the upper cover plate 11 to insulate the load-bearing bearing 9 from the outside world to avoid electric shock accidents; there are 3 feed bearings 15, one of which is a bar magnet feed bearing for feeding the entire bar magnet, and the other two are cylindrical magnet feed bearings for feeding the cylindrical magnets at both ends; the feed bearing 15 is passed through by the feed slide bar 13, and the top end of the slide bar of the feed bearing passes through the upper cover plate and is connected to the second micrometer knob type precision slide 22 through the clamping plate for feeding the bar magnet, or is connected to the first micrometer knob type precision slide 21 for feeding the cylindrical magnets at both ends, and the other end is connected to the mounting plate 1 or the cylindrical magnet mounting seat 14 through the mounting seat. There are two cylindrical magnet mounting seats 14 for mounting and fixing the cylindrical magnets at both ends; the yoke 7 is used to locate the positions of all bar magnets and to curb the diffusion of magnetic flux lines behind the cathode; the terminal 5 is welded to the cooling water plate, and the lead-out wiring is connected to the constant voltage power supply and connected to the cathode to power the entire cathode, that is, the negative pole of the power supply.

[0064] like Figure 4 As shown, the internal schematic diagram of the water-cooled back plate 2, when working, cooling water enters from the water inlet connected to the water inlet pipe 4 at the bottom, and is discharged from the upper outlet to fully cool the entire target material.

[0065] like Figure 6 As shown, the yoke 7 is provided with a through hole for the load-bearing slide rod 12 of the load-bearing bearing 9 to pass through; the feed slide rod 13 of the bar magnet feed bearing 15 passes through the yoke and is fixedly connected to the yoke 7, thereby driving the yoke to move with the bar magnet feed slide rod; the yoke 7 is also provided with a through hole for the feed slide rod of the cylindrical magnet feed bearing to pass through, so as to ensure that the cylindrical magnet can move freely.

[0066] The working process of etching the magnetron sputtering cathode target material in the present invention is as follows: after the substrate is set and the water cooling system is turned on, the vacuum chamber is evacuated to a gas pressure lower than 3.0×10 -4Pa, then fill with argon gas for discharge, ion clean the substrate, after cleaning, fill with reaction gas, turn on the power and set it to constant voltage mode, start coating after the parameters are stable, as the coating process proceeds, by adjusting the feed amount of the second micrometer knob type precision slide 22, change the position of the entire bar magnet (the middle bar magnet 18 and the outer ring bar magnet 24 are fed simultaneously with the yoke iron), and then adjust the magnetic field strength at the target surface etching straight track, so that the discharge current remains relatively unchanged during the coating process; at the same time, by adjusting the feed amount of the first micrometer knob type precision slide 21, the position of the cylindrical magnet can be changed, and then adjust the magnetic field strength at the target surface etching curve to make it relatively consistent with the straight track, to ensure that the etching rate at the curve is relatively consistent with the straight track, during the adjustment process of the micrometer knob precision slide, manual adjustment can be made by observing the current changes in the experiment, or a feedback signal can be given to the micrometer knob precision slide through the current changes in the experimental process (as the etching current increases), so as to perform automatic adjustment. The magnet position is adjusted by observing and controlling the etching degree, thereby improving the target material utilization.

[0067] The implementation process and effects of the present invention are described below in the form of embodiments.

[0068] Embodiment 2: An application example of magnetic field regulation of the magnetic field structure and control method of the control device of the present invention on a rectangular target with a target size of 698 mm×148 mm.

[0069] Behind a rectangular target made of aluminum and measuring 698 mm × 148 mm, Figure 5 The magnetic field structure is arranged as shown, in which the outer ring magnet and the middle magnet have opposite magnetic polarities. By adjusting the feed amount of the micrometer knob type precision slide 21 and 22, the magnetic field distribution on the target surface can be changed. Here, the position of the magnet is specially explained: the position of the magnet is expressed in mm. Specifically, the overall position of 0 mm represents the position where the upper surface of the magnet (involving the outer ring bar magnet, the middle bar magnet and the cylindrical magnet respectively) coincides with the lower surface of the water-cooled back plate; and the overall position of 10 mm is that the upper surface of the magnet is 10 mm away from the lower surface of the water-cooled back plate.

[0070] In order to further analyze and explain the change of the target surface magnetic field during the overall movement of the magnet, two sectional line segments are established on the target surface, such as Figure 7 As shown, the starting point of section A is the center of the long side of the target material, and the end point is the center of the opposite side. The length of the section is 148 mm, which is used to study the changes in the magnetic field in the straight part; the starting point of section B is the center of the short side of the target material, and the end point is the center of the opposite side. The length of the section is 698 mm, which is used to study the changes in the magnetic field in the curved part.

[0071] Figures 8(a) and 8(b) are the horizontal and vertical magnetic flux density components along the direction of the section line A and the path within the range of 0 to 148 mm from the origin. Figures 9(a) and 9(b) are the horizontal and vertical magnetic flux density components along the direction of the section line B and the path within the range of 0 to 698 mm from the origin.

[0072] It can be seen from Figures 8(a), 8(b) and 9(a), 9(b) that as the magnet position gradually moves away from the target surface, the horizontal magnetic field and vertical magnetic field at the same position of the target surface of the curve and the straight track are reduced; the reduction in magnetic field strength will lead to a reduction in the ability of the magnetic field to bind electrons, causing a decrease in plasma density and weakening the etching behavior of the target material. Here, the term "horizontal magnetic field" is explained. For a magnetic flux line, its tangent direction is the direction of the magnetic field vector B. B is orthogonally decomposed along the direction parallel to the target surface and perpendicular to the target surface, and the vector component parallel to the target surface is called the "horizontal magnetic field"; similarly, the vector component perpendicular to the target surface is called the "vertical magnetic field", as shown in Figure 9.

[0073] Example 3: An application example of the magnetic field structure and control method of the control device of the present invention in controlling the etching rate on a rectangular target with a target size of 698 mm×148 mm.

[0074] The output voltage of the power supply is set to 367V constant. A series of parameter adjustments and explorations are performed in the early stage of target etching. The total etching work of this stage is recorded as 75kW·h, which is the initial work. After 75kW·h, the target current is controlled to be stable at 16±0.5A by adjusting the cathode magnetic field, that is, the discharge power is about 5.87kW, and the upper and lower deviations shall not exceed 3.125%. The target is etched for 150kW·h at a constant voltage U and a relatively unchanged target current I, and the total etching work W accumulated in each stage is recorded. a The corresponding bar magnet position X b and the cylindrical magnet position X c Since the working gas pressure also affects the target current during the discharge process, the working gas pressure must always be maintained at 0.5 Pa during the magnetic field adjustment process.

[0075] The output voltage of the power supply can be selected in the range of 350-420V, which is given according to the specific parameters of the specific equipment. If the voltage is too small, glow discharge cannot be generated and target surface etching cannot be performed. If the voltage is too large, the target surface etching is too severe, which will have a penetration effect and is not conducive to etching.

[0076] 75kW·h is the work done in a series of parameter adjustment and exploration processes before etching in this specific embodiment, mainly studying the voltage, current, inflation pressure (how many ccm of continuous gas flow), the range of magnetic field intensity change, the value of current change, and the discharge stability during the etching process.

[0077] Other magnetic fields are controlled by controlling the movement of magnets to control the size of the magnetic field strength on the target surface. The strength of the magnetic field is reflected by the current on the target surface during the experiment. The stronger the magnetic field, the greater the target current. This experiment is also in the etching process. As the target material is continuously etched, the magnet is getting closer to the etching position of the target material, and then the magnetic field strength increases, causing the current on the target surface to increase. In order to control the current to move within the range of 16±0.5A, it is necessary to control the magnet to move backward to weaken the change in current. This method has certain versatility.

[0078] The current control range is 16±0.5A. ±0.5A indicates that the etching is uniformly controlled within the allowable error range, but it can be further reduced. However, too small an error current is not easy to control. Other data (16A) must also ensure that the target can perform normal glow discharge. If the target current is too small, it will not start glow discharge. Or the target surface is not bright enough and the etching is slow. Too much current will also cause the temperature to be too high. Secondly, the magnetic field strength adjustment is limited. The temperature rises, the etched particles become larger, the coating is uneven, and the density is insufficient, which is not conducive to the experiment.

[0079] The discharge power is calculated according to the formula P=UI.

[0080] Since the size of the horizontal magnetic field on the target surface can be changed by adjusting the position of the bar magnet and the cylindrical magnet, and the horizontal magnetic field can constrain the movement of electrons, thereby controlling the surface Ar + By adjusting the initial positions of the bar magnet and cylindrical magnet, the target current reaches 16A, and the initial positions of the two magnets are determined to be 2mm and 4mm respectively. The specific experimental process is as follows Fig.11 As shown. The total input power is calculated according to the formula W = UIt, and the voltage U is a constant voltage of 367V. However, with continuous etching, the current I will increase, and it is necessary to change the magnetic field by adjusting the micrometer knob to control the current within the range of 16 ± 0.5A. The voltage U, current I and time t are recorded experimentally, and then the total power (calculated by W = UIT) is accumulated and calculated, and then the total input power Wa is calculated.

[0081] The calculation formula is Wa=W0+UIT,

[0082] Wherein, Wa is the expected total input power, which is 225kW·h in this embodiment; W0 is the initial power, which refers to the power done in a series of parameter adjustments and explorations before etching, and is a known number, which is 75kW·h in this embodiment;

[0083] U is a constant voltage, which is 367 V in this embodiment, I is a current monitored in real time, and T is an etching time.

[0084] Step 1: Arrange the magnetic field structure using the control device for the etching rate of the cathode target material of the magnetron sputtering provided in Example 1 and start the experiment;

[0085] Step 2, record the total input power Wa, the positions Xb and Xc of the bar magnet and the cylindrical magnet, and the target current I;

[0086] Step 3: Check whether the current total input power Wa is less than 225kW·h;

[0087] If yes, then an etching experiment with constant voltage and power is conducted, where power P = U*I, and the power is kept constant by controlling the current;

[0088] If not, end the experiment;

[0089] Step 4: During the etching experiment, check whether the current is within the range of 15.5A to 16.5A;

[0090] If yes, record the current data of Xb, Xc, I and Wa, and return to step 2;

[0091] If not, adjust the positions Xb and Xc of the bar magnet and the cylindrical magnet, and then re-check whether the current is within the range of 15.5A to 16.5A.

[0092] according to Fig.11 The process shown is used to control the target etching process, and the data obtained are shown in Table 1. Where I0 represents the target current before the moving magnet.

[0093] Table 1 Control of target current by changing the position of the magnet

[0094]

[0095]

[0096] According to the data in Table 1, the discharge current changes with the target etching process ( Fig.12 ),from Fig.12It can be seen that when using the magnetic field structure and control method of the control device of the present invention, the discharge current can be well stabilized within the range of 16A±0.5A. The results show that the number of ions bombarding the target surface can be stabilized within a relatively small fluctuation range per unit time at different stages of the discharge process; and the bombardment energy of the ions depends on the discharge voltage. The discharge voltage of the device is provided by a constant voltage power supply, so the ion bombardment energy can be guaranteed to remain unchanged. Combining the above two results, it can be obtained that the etching rate of the target material can be stabilized within a certain range using the device and control method of the present invention.

[0097] The above description is only a preferred embodiment of the present invention and is not intended to limit the concept of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for controlling the etching rate of a magnetron sputtering cathode target, characterized in that: The steps include: Step 1: using a magnetron sputtering cathode target etching rate control device to arrange a magnetic field structure; The control device structure of the etching rate of the magnetron sputtering cathode target material comprises a target module, a constant voltage power supply and a magnetic field module arranged behind the target module, wherein the target module comprises a target material, a water-cooled back plate, a mounting plate, an outer shell and an upper cover plate; the magnetic field module comprises a permanent magnet and a control module, and the control module is composed of a magnetic field moving device; the permanent magnet and the magnetic field moving device are arranged inside the outer shell; a yoke is also arranged inside the outer shell, and the position of the yoke is controlled by the magnetic field moving device; the water-cooled back plate is fixed on the mounting plate, and the target material is fixed on the water-cooled back plate; The upper cover is fixed on the outer shell, and the outer shell is fixed on the mounting plate; the back of the water-cooled back plate is provided with water inlet and outlet pipes, and water enters from the lower left corner of the water-cooled back plate and exits from the upper right corner; a cylindrical magnet mounting seat and a terminal are also provided inside the outer shell, and the cylindrical magnet mounting seat and the bottom end of the terminal are fixed on the mounting plate, and the terminal is provided on the back of the water-cooled back plate and connected to a constant voltage power supply; The permanent magnet includes a bar magnet and a cylindrical magnet. The bar magnet includes an outer ring bar magnet and a middle bar magnet. The bar magnets are all fixed on the yoke and move synchronously with the yoke. The cylindrical magnet is fixed in a cylindrical magnet mounting seat. Step 2: Determine the total input power, record the positions Xb and Xc of the bar magnet and the cylindrical magnet and the initial target current I0, and start the experiment; Among them, Wa = W0 + UIT, Wa is the expected total input power, which is a known number; W0 is the initial power, which is a known number; U is the constant voltage, I is the current monitored in real time, and T is the etching time; Step 3: Detect whether the current total input power is less than the expected total input power; If yes, then an etching experiment with constant voltage and power is performed; If not, end the experiment; Step 4: During the etching experiment, check whether the current is within the range of I0±0.5A; If yes, record the current data of Xb, Xc, I and Wa, and return to step 2; If not, adjust the positions Xb and Xc of the bar magnet and the cylindrical magnet, and then recheck whether the current is within the range of I0±0.5A.

2. The control method according to claim 1, characterized in that: The magnetic field moving device comprises a linear bearing, a slide bar, a magnet mounting seat and a micrometer knob type precision slide table.

3. The control method according to claim 2, characterized in that: The linear bearing includes a feed bearing for controlling the reciprocating movement of the bar magnet and a feed bearing for controlling the reciprocating movement of the cylindrical magnet.

4. The control method according to claim 3, characterized in that: The magnetic field moving device also includes a load-bearing bearing.

5. The control method according to claim 4, characterized in that: The micrometer knob type precision slide comprises a first micrometer knob type precision slide for feeding cylindrical magnets and a second micrometer knob type precision slide for feeding bar magnets.

6. The control method according to claim 5, characterized in that: The feed bearing that controls the reciprocating movement of the bar magnet is passed through by the feed slide rod. The top end of the feed slide rod of the feed bearing passes through the upper cover plate and is connected to the first micrometer knob-type precision slide through the clamping plate for feeding the bar magnet. The other end is connected to the mounting plate through a mounting seat.

7. The control method according to claim 6, characterized in that: The feed bearing that controls the reciprocating movement of the cylindrical magnet is passed through by the feed slide rod. The top end of the feed slide rod of the feed bearing passes through the upper cover plate and is connected to the second micrometer knob-type precision slide through the clamping plate. It is used for feeding the cylindrical magnets at both ends, and the other end is connected to the cylindrical magnet mounting seat through the mounting seat.