A carbon-coated current collector and its preparation method and electrochemical device

By mixing carbon materials with fibrotic binder dry method to form a carbon film and combining it with current collector, the problem of solvent introduction in lithium-ion batteries is solved, the performance and stability of the battery is improved, and the cost and environmental impact are reduced.

CN114407263BActive Publication Date: 2024-11-22CHINA AUTOMOTIVE INNOVATION CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210050207.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-17
Publication Date
2024-11-22
Estimated Expiration
2042-01-17

AI Technical Summary

Technical Problem

The existing lithium-ion battery carbon-coated current collector preparation method requires the introduction of solvents, resulting in increased costs, environmental pollution and reduced battery cycle stability.

Method used

The dry method is used to mix carbon materials with fibrotic binder to form a carbon film by rolling pressure, and combine it with the current collector to avoid the use of solvents and improve electrochemical performance.

Benefits of technology

It reduces battery production costs, improves capacity retention and rate performance, reduces environmental pollution, and enhances the cycle stability and energy density of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114407263B_ABST
    Figure CN114407263B_ABST
Patent Text Reader

Abstract

The present invention provides a carbon-coated current collector and a preparation method thereof and an electrochemical device, wherein the preparation method comprises: (1) dry-mixing a carbon material and a first binder to obtain a mixture, and performing a first roll pressing on the mixture to obtain a carbon film; wherein the first binder is a polymer that can be fiberized; (2) placing the carbon film in step (1) on at least one side surface of a current collector, and performing a second roll pressing to obtain a carbon-coated current collector. The present invention prepares a carbon film by dry-mixing a certain proportion of carbon material and a fiberized binder, and roll pressing the carbon-coated current collector with the current collector to form a carbon-coated current collector, thereby avoiding the introduction of solvents, reducing the production cost of the electrochemical device, and improving the capacity retention rate and rate performance of the electrochemical device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to a carbon-coated current collector and a preparation method thereof and an electrochemical device. Background Art

[0002] As one of the most important energy storage devices today, the application scope of lithium-ion batteries has gradually expanded from the fields of electronic products and power tools to emerging fields such as new energy electric vehicles, electric ships, electric aircraft, robots, and distributed energy. These fields generally require lithium-ion batteries to have larger capacity and higher energy density, fast charge and discharge capabilities, and good cycle stability. At present, the research on traditional lithium-ion batteries is mostly focused on positive and negative electrode materials, and there is relatively little research on carbon-coated current collectors.

[0003] CN109888296A discloses a method for preparing a carbon-coated current collector for a lithium-ion battery positive electrode, wherein the current collector is placed in an organic solvent containing nano-carbon powder and nano-titanium powder, subjected to ultrasound, and then the current collector after ultrasound is placed in a vacuum deposition chamber for pre-nucleation treatment, so that a uniform and dense carbon film layer is deposited on the surface of the current collector. This method improves the peeling strength of the carbon layer and the service life of the battery. CN113717595A discloses a carbon-coated current collector coating and a method for preparing the same, wherein a binder, a dispersant, a conductive material and a solvent are mixed to obtain the carbon-coated current collector coating, wherein the selected binder is modified polyacrylic acid, and the use of the carbon-coated current collector coating can reduce the corrosion of the current collector and has a good adhesion effect. CN113394407A provides a current collector for a secondary battery and a method for preparing the same and an application thereof, wherein the conductive liquid comprising a lithium-containing positive electrode material, a conductive agent, a binder and a solvent is coated on the surface of a substrate, and a current collector for a secondary battery is obtained after drying, and the prepared current collector has good adhesion, flexibility and conductivity.

[0004] The prior art uses a variety of methods to prepare carbon-coated current collectors, but the above technical solutions all require the introduction of solvents in the process of preparing the carbon-coated current collectors, which adds an additional drying process, increases the cost, and the evaporated solvent will also have a certain impact on the environment; at the same time, a portion of the solvent remaining in the carbon layer of the current collector will also reduce the cycle stability of the battery and affect the electrochemical performance of the battery. Summary of the invention

[0005] In view of the problems existing in the prior art, the purpose of the present invention is to provide a carbon-coated current collector and a preparation method thereof and an electrochemical device. The present invention prepares a carbon film by dry mixing a certain proportion of carbon material and a fiberizable binder, and rolls the carbon-coated current collector with the current collector to form a carbon-coated current collector, thereby avoiding the introduction of solvents, reducing the production cost of the electrochemical device, and improving the capacity retention rate and rate performance of the electrochemical device.

[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a method for preparing a carbon-coated current collector, the preparation method comprising:

[0008] (1) dry-mixing a carbon material and a first binder to obtain a mixture, and performing a first roll pressing on the mixture to obtain a carbon film;

[0009] Wherein, the first binder is a polymer that can be fiberized;

[0010] (2) Placing the carbon film described in step (1) on at least one side of the current collector and performing a second rolling process to obtain a carbon-coated current collector.

[0011] The present invention prepares a carbon film by dry mixing a certain proportion of carbon material and a fiberizable binder. Under the action of external force, the first binder can form a fiberized network structure and combine with the carbon material to form a carbon film without adding a solvent. The prepared carbon film is then rolled with a current collector to form a carbon-coated current collector. The preparation process of the present invention avoids the introduction of solvents, prevents the solvent from remaining in the carbon film and affecting the electrochemical performance of the electrochemical device, improves the capacity retention rate and rate performance of the electrochemical device, and at the same time eliminates the drying process, and no harmful gas is emitted. The required equipment is simple, the production cost of the electrochemical device is reduced, and the environmental pollution is small.

[0012] As a preferred technical solution of the preparation method of the present invention, the current collector in step (2) is a porous current collector or a non-porous current collector, preferably a porous current collector.

[0013] Using a porous current collector as the current collector of the positive or negative electrode in the battery can reduce the weight of the battery compared to a non-porous current collector, thereby increasing the energy density of the lithium-ion battery. When using a carbon-coated current collector as the current collector of the positive or negative electrode, the carbon film provided on the surface of the carbon-coated current collector can reduce the contact resistance between the electrode material and the carbon-coated current collector, thereby improving the rate performance of the battery. The existing method for preparing a carbon-coated current collector is a wet process, that is, coating a carbon slurry on a current collector substrate and drying it, but the carbon slurry with fluidity cannot be coated on a current collector with a porous structure, so the conventional wet process cannot prepare a carbon-coated porous current collector, and it cannot be applied to lithium-ion batteries. Therefore, developing a preparation method that can combine a carbon film and a porous current collector is a technical difficulty that needs to be solved urgently.

[0014] The present invention preferably adopts a porous current collector combined with a dry process to prepare a carbon-coated current collector. This method can effectively combine the carbon film with the porous current collector, can reduce the contact resistance between the electrode material and the current collector, avoid the problem that the pores of the porous current collector cannot be filled with carbon materials in the conventional preparation process, and improve the rate performance of the battery; compared with the non-porous foil current collector, the unit weight of the carbon-coated current collector is lighter, which can improve the energy density of the battery; at the same time, the dry preparation process also avoids the use of organic solvents, saving the energy consumed by drying. This dry-prepared carbon-coated current collector can not only improve the rate performance and energy density of the battery, reduce the contact resistance, but also reduce the production cost of the battery.

[0015] Preferably, the current collector is an aluminum foil or a copper foil, for example, a porous aluminum foil, a porous copper foil, a non-porous aluminum foil or a non-porous copper foil.

[0016] Preferably, the thickness of the current collector is 6-10 μm, for example, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm or 10 μm.

[0017] Preferably, the mass ratio of the carbon material and the first binder is x:(1-x), where x is 0.5 to 10, for example, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10, and x is further preferably 0.5 to 1. Within this range, the prepared carbon film has better performance.

[0018] Preferably, the carbon material in step (1) comprises any one or a combination of at least two of conductive carbon black, graphene, graphite, acetylene black, carbon nanotubes and graphene-carbon nanotube hybrids, for example, a combination of conductive carbon black and graphene, a combination of graphene and graphite, a combination of acetylene black and carbon nanotubes, or a combination of conductive carbon black, graphene and graphite, etc., preferably conductive carbon black and / or carbon nanotubes.

[0019] The graphene carbon nanotube hybrid in the present invention is a composite of a graphene hybrid and a carbon nanotube hybrid. The present invention has no limitation on the source of the graphene carbon nanotube hybrid. For example, the graphene carbon nanotube hybrid of Beijing North Guoneng Technology Co., Ltd. can be used.

[0020] The carbon material in the present invention is preferably conductive carbon black and / or carbon nanotubes, which are combined with the dry preparation process in the present invention and synergistically act with the porous current collector to obtain a carbon-coated current collector with better performance.

[0021] Preferably, the first binder in step (1) comprises any one of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR) and polyacrylic acid (PAA) or a combination of at least two thereof, for example, a combination of polytetrafluoroethylene and polyvinylidene fluoride, a combination of polyvinylidene fluoride and styrene-butadiene rubber, or a combination of polyvinylidene fluoride, styrene-butadiene rubber and polyacrylic acid, etc., preferably polytetrafluoroethylene.

[0022] The preferred first binder of the present invention is polytetrafluoroethylene. PTFE is easily fibrillated under the action of external force. When combined with the carbon material and dry preparation method of the present invention, it is more conducive to improving the performance of the carbon-coated current collector.

[0023] The present invention does not limit the dry mixing method of step (1). The mixing can be high-speed stirring, air flow crushing, high-energy ball milling or twin-screw extrusion, etc. Any method that can fiberize the polymer is applicable to the present invention, not limited to the listed methods.

[0024] Preferably, the first rolling in step (1) is a first hot rolling.

[0025] Preferably, the temperature of the first hot roller pressing is 80-160°C, for example, it can be 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C or 160°C.

[0026] Preferably, the pressure of the first hot roller pressing is 10-50T, for example, it can be 10T, 15T, 20T, 25T, 30T, 35T, 40T, 45T or 50T.

[0027] The present invention adopts a specific temperature and pressure to perform the first hot rolling, which can make the binder and the carbon material bond together to form a film, so that the carbon film can reach the required thickness.

[0028] Preferably, the carbon film has a thickness of 2 to 10 μm, for example, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm.

[0029] Preferably, the surface loading of the first binder on the carbon film is 0.05-0.2 mg / cm 2 , for example, it can be 0.05 mg / cm 2 , 0.06mg / cm 2 , 0.08mg / cm 2 , 0.1mg / cm 2 , 0.12mg / cm 2 , 0.14mg / cm 2 , 0.16mg / cm 2 、0.18mg / cm 2or 0.2mg / cm 2 wait.

[0030] As a preferred technical solution of the preparation method of the present invention, before the carbon film is placed on at least one side of the current collector in step (2), a second binder is also coated on the side of the carbon film close to the current collector.

[0031] The present invention coats a second binder on the surface of the carbon film, and laminates the side coated with the second binder to the current collector. After subsequent rolling, it is more conducive to improving the bonding force between the carbon layer and the current collector, and is suitable for porous current collectors and non-porous current collectors.

[0032] Exemplarily, the second binder may be applied in the present invention by transferring the carbon film to a coating roller containing the second binder for coating.

[0033] Preferably, the second binder includes any one of polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber and polyacrylic acid, or a combination of at least two thereof;

[0034] Preferably, the surface loading of the second binder on the carbon film is 0.01-0.2 mg / cm 2 , for example, it can be 0.01 mg / cm 2 , 0.02mg / cm 2 , 0.04mg / cm 2 , 0.06mg / cm 2 , 0.08mg / cm 2 , 0.1mg / cm 2 , 0.12mg / cm 2 , 0.14mg / cm 2 , 0.16mg / cm 2 、0.18mg / cm 2 or 0.2mg / cm 2 By regulating the surface loading of the second binder within a suitable range, the electrochemical performance of the carbon-coated current collector can be further improved in combination with the dry preparation method of the present invention.

[0035] As a preferred technical solution of the preparation method of the present invention, the second rolling in step (2) includes integrated rolling and second hot rolling.

[0036] Preferably, the temperature of the integrated rolling is 80-160°C, for example, it can be 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C or 160°C, etc., the purpose is to shape the carbon layer and the collector so that the adhesive can adhere to the surface of the collector.

[0037] Preferably, the integrated rolling pressure is 10-50T, for example, it may be 10T, 15T, 20T, 25T, 30T, 35T, 40T, 45T or 50T.

[0038] In the present invention, it is preferred to pre-press the carbon film and the current collector by integrated rolling to obtain a composite structure current collector (for example, a three-layer composite structure current collector), and then use hot roller pressing to make the composite structure current collector form a carbon-coated current collector, which is beneficial to thermal bonding between the carbon films and between the carbon film and the porous current collector, and at the same time rolling the carbon-coated current collector to a preset thickness.

[0039] Preferably, the temperature of the second hot roller pressing is 80-160°C, for example, it can be 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C or 160°C.

[0040] Preferably, the pressure of the second hot roller pressing is 10-50T, for example, it can be 10T, 15T, 20T, 25T, 30T, 35T, 40T, 45T or 50T.

[0041] In the present invention, during the second hot rolling, a multi-stage rolling method can be adopted, such as using three rolling rollers with the same or different pressures to gradually roll the composite structure current collector obtained by integrated rolling to obtain a carbon-coated current collector, thereby further improving the performance of the carbon-coated current collector.

[0042] In a second aspect, the present invention provides a carbon-coated current collector, which is prepared by the preparation method according to the first aspect, and comprises a current collector and a carbon film disposed on at least one side of the current collector.

[0043] The carbon-coated current collector prepared by the present invention has no solvent residue, is energy-saving and environmentally friendly, has low contact resistance and good stability. The electrochemical device prepared by using the carbon-coated current collector of the present invention has a good capacity retention rate.

[0044] In the present invention, in particular, the carbon-coated current collector prepared by using a porous current collector combined with the dry preparation process of the present invention has a smaller contact resistance, a lighter weight, and a better rate performance. The prepared electrochemical device has excellent rate performance, energy density and cycle stability.

[0045] Preferably, the thickness of the carbon-coated current collector is 8 to 20 μm, for example, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm or 20 μm.

[0046] The carbon-coated current collector with suitable thickness is prepared in the present invention, and its application in electrochemical devices is more conducive to the performance of electrochemical performance.

[0047] In a third aspect, the present invention provides an electrochemical device, wherein the positive electrode and / or the negative electrode of the electrochemical device comprises the carbon-coated current collector according to the second aspect.

[0048] The electrochemical device prepared by the invention has good rate performance, high energy density and good cycle stability.

[0049] Compared with the prior art, the present invention has the following beneficial effects:

[0050] (1) The present invention adopts a dry process to prepare the carbon-coated current collector without using any solvent. Compared with the traditional wet process, it can reduce the influence of residual solvent in the carbon-coated current collector on battery performance and improve the cycle stability of the battery. At the same time, it eliminates the drying process, requires simple equipment, and has no harmful gas emissions, which can reduce battery costs and reduce pollution to the environment.

[0051] (2) The present invention preferably uses a porous current collector in combination with a dry process to prepare a carbon-coated current collector, which can solve the problems of poor coating effect of the traditional wet process, low utilization efficiency of the carbon-coated current collector, and poor conductivity. The prepared current collector is lighter in weight and has a smaller contact resistance with the electrode material, further improving the rate performance, energy density and cycle stability of the electrochemical device. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 It is a flow chart of the preparation of a carbon-coated current collector in a specific embodiment of the present invention.

[0053] Figure 2 It is a schematic diagram of rolling of a carbon-coated current collector in a specific embodiment of the present invention.

[0054] Figure 3 1 is a cross-sectional view and a top view of a carbon-coated current collector in a specific embodiment of the present invention. DETAILED DESCRIPTION

[0055] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0056] The embodiment of the present invention provides a method for preparing a carbon-coated current collector. Figure 1 , the preparation method comprises:

[0057] (1) dry-mixing a carbon material and a first binder to obtain a mixture, and performing a first roll pressing on the mixture to obtain a carbon film;

[0058] Wherein, the first binder is a polymer that can be fiberized;

[0059] (2) Placing the carbon film described in step (1) on at least one side of the current collector and performing a second rolling process to obtain a carbon-coated current collector.

[0060] In some embodiments, the current collector in step (2) is a porous current collector or a non-porous current collector.

[0061] In some embodiments, the current collector in step (2) is a porous current collector.

[0062] In some embodiments, the current collector is aluminum foil or copper foil.

[0063] In some embodiments, the current collector has a thickness of 6 to 10 μm.

[0064] In some embodiments, the mass ratio of the carbon material to the first binder is x:(1-x), where x is 0.5-10.

[0065] In some embodiments, the mass ratio of the carbon material to the first binder is x:(1-x), where x is 0.5-1.

[0066] In some embodiments, the carbon material in step (1) includes any one or a combination of at least two of conductive carbon black, graphene, graphite, acetylene black, carbon nanotubes and graphene-carbon nanotube hybrids, preferably conductive carbon black and / or carbon nanotubes.

[0067] In some embodiments, the first binder in step (1) includes any one of polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber and polyacrylic acid, or a combination of at least two thereof, preferably polytetrafluoroethylene.

[0068] In some embodiments, the first roller pressing in step (1) is a first hot roller pressing.

[0069] In some embodiments, the temperature of the first hot roller pressing is 80-160°C.

[0070] In some embodiments, the pressure of the first hot roller pressing is 10-50T.

[0071] In some embodiments, the thickness of the carbon film in step (1) is 2 to 10 μm.

[0072] In some embodiments, the surface loading of the first binder on the carbon film is 0.05 to 0.2 mg / cm 2 .

[0073] In some embodiments, before the carbon film is placed on at least one side of the current collector in step (2), a second binder is further coated on the side of the carbon film close to the current collector. The second binder can be coated by a coating roller. Figure 2 , connect the carbon film to the glue coating roller, apply the second adhesive and continue to move forward to combine with the current collector.

[0074] In some embodiments, the second binder includes any one of polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber and polyacrylic acid, or a combination of at least two thereof.

[0075] In some embodiments, the surface loading of the second binder on the carbon film is 0.01 to 0.2 mg / cm 2 .

[0076] In some embodiments, the second rolling step (2) comprises an integrated rolling step and a second hot rolling step, see Figure 2 First, the carbon film and the current collector are pressed by integrated rolling to obtain a composite structure current collector, and then a subsequent second hot rolling is performed.

[0077] In some embodiments, the temperature of the integrated rolling is 80-160°C.

[0078] In some embodiments, the integrated rolling pressure is 10-50T.

[0079] In some embodiments, the temperature of the second hot rolling is 80-160°C.

[0080] In some embodiments, the pressure of the second hot roller pressing is 10-50T.

[0081] The second hot rolling of the present invention can be carried out in a multi-stage rolling manner, such as Figure 2 As shown, under the condition of constant temperature, three rolling rollers with the same or different pressures are set, so that the composite structure current collector obtained by integrated rolling passes through three rollers in sequence, and the carbon-coated current collector is obtained by rolling.

[0082] Example 1

[0083] This embodiment provides a carbon-coated current collector and a preparation method thereof. The carbon-coated current collector includes a current collector and a carbon film disposed on both sides of the current collector. The current collector is a porous aluminum foil. The thickness of the carbon-coated current collector is 15 μm. The preparation method is shown in Figure 1 and Figure 2 , the steps are:

[0084] (1) Conductive carbon black (SP) and polytetrafluoroethylene (PTFE) were mixed in a mass ratio of 98:2, added into a stirrer and premixed for 4 hours to obtain a mixture, and the mixture was subjected to a first hot roll pressing at 80° C. and 10F to obtain a carbon film with a thickness of 5 μm;

[0085] (2) The carbon film is introduced onto the rubber coating roller, and the rubber coating roller transfers PTFE onto the surface of the carbon film. The surface loading of PTFE on the surface of the carbon film is 0.2 mg / cm 2 ,like Figure 2 ;

[0086] (3) The two layers of PTFE-coated carbon film and the 10 μm porous aluminum foil were rolled together at a rolling pressure of 15T, and then entered into a 70°C rolling machine, and then entered into 10T, 30T, and 20T rolling machines for a second hot rolling to obtain a carbon-coated current collector. The thickness of the carbon-coated current collector was controlled to be 15 μm. Figure 3 As shown, Figure 3 The left picture in the middle is a cross-sectional view of the carbon-coated current collector, and the right picture is a top view. Figure 3 It can be seen that the carbon film can fill into the pores of the porous current collector.

[0087] A slurry containing 94 parts by mass of NCM523 positive electrode material, 3 parts by mass of conductive agent and 3 parts by mass of binder was coated on the carbon-coated current collector, and the surface capacity was controlled at 3 mA / cm 2 , and obtain the positive electrode.

[0088] Example 2

[0089] This embodiment provides a carbon-coated current collector and a preparation method thereof. The carbon-coated current collector includes a current collector and a carbon film disposed on both sides of the current collector. The current collector is a porous aluminum foil. The thickness of the carbon-coated current collector is 13 μm. The preparation method is shown in Figure 1 and Figure 2 , the steps are:

[0090] (1) carbon nanotubes and polyacrylic acid (PAA) were mixed in a mass ratio of 95:5, added to a stirrer and premixed for 1 hour to obtain a mixture, and the mixture was subjected to a first hot roll pressing at 85° C. and 20° F to obtain a carbon film with a thickness of 3 μm;

[0091] (2) The carbon film was introduced onto a rubber coating roller, which transferred PAA onto the surface of the carbon film. The surface loading of PAA on the carbon film was 0.05 mg / cm 2 ,like Figure 2 ;

[0092] (3) The two layers of PAA-coated carbon film and the 10 μm porous aluminum foil were rolled together at a rolling pressure of 25T, and then entered into a rolling press at 80°C, and then entered into a rolling press at 10T, 30T, and 20T for a second hot rolling to obtain a carbon-coated current collector. The thickness of the carbon-coated current collector was controlled at 13 μm. Figure 3 .

[0093] A slurry containing 90 parts by mass of LiFePO4 positive electrode material, 3 parts by mass of conductive agent and 7 parts by mass of binder is coated on the carbon-coated current collector, and the surface capacity is controlled at 2 mA / cm 2 , and obtain the positive electrode.

[0094] Example 3

[0095] This embodiment provides a carbon-coated current collector and a preparation method thereof. The carbon-coated current collector includes a current collector and a carbon film disposed on both sides of the current collector. The current collector is a porous copper foil. The thickness of the carbon-coated current collector is 20 μm. The preparation method is shown in Figure 1 and Figure 2 , the steps are:

[0096] (1) Graphite and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 99:1, added to a stirrer and premixed for 4 hours to obtain a mixture, and the mixture was subjected to a first hot roll pressing at 90° C. and 10F to obtain a carbon film with a thickness of 10 μm;

[0097] (2) The carbon film is introduced onto the coating roller, and the coating roller transfers PVDF onto the surface of the carbon film. The surface loading of PVDF on the surface of the carbon film is 0.01 mg / cm 2 ,like Figure 2 ;

[0098] (3) The two layers of PVDF-coated carbon film and the 6 μm porous copper foil were rolled together at a rolling pressure of 15T, and then entered into a rolling press at 160°C, and then entered into a rolling press at 10T, 30T, and 20T for a second hot rolling to obtain a carbon-coated current collector. The thickness of the carbon-coated current collector was controlled at 20 μm. Figure 3 .

[0099] A slurry containing 97 parts of artificial graphite negative electrode material, 1.5 parts of conductive agent and 1.5 parts of binder in a mass ratio is coated on the above-mentioned carbon-coated current collector, and the surface capacity is controlled at 2 mA / cm 2 , and obtain the negative electrode sheet.

[0100] Example 4

[0101] This embodiment provides a carbon-coated current collector and a preparation method thereof. The carbon-coated current collector includes a current collector and a carbon film disposed on both sides of the current collector. The current collector is a porous copper foil. The thickness of the carbon-coated current collector is 8 μm. The preparation method is shown in Figure 1 and Figure 2 , the steps are:

[0102] (1) carbon nanotubes and styrene-butadiene rubber (SBR) were mixed in a mass ratio of 99.5:0.5, added into a stirrer and premixed for 8 hours to obtain a mixture, and the mixture was subjected to a first hot roll pressing at 100° C. and 50° F to obtain a carbon film with a thickness of 2 μm;

[0103] (2) The carbon film is introduced onto the rubber coating roller, and the rubber coating roller transfers SBR to the surface of the carbon film. The surface loading of SBR on the surface of the carbon film is 0.05 mg / cm 2 ,like Figure 2 ;

[0104] (3) The two layers of SBR-coated carbon film and the 6 μm porous copper foil were rolled together at a rolling pressure of 30 T, and then entered into a rolling press at 100° C., and then entered into a rolling press at 20 T, 50 T, and 20 T for a second hot rolling to obtain a carbon-coated current collector. The thickness of the carbon-coated porous current collector was controlled at 8 μm, as shown in FIG. Figure 3 .

[0105] A slurry containing 95 parts by mass of silicon-carbon negative electrode material, 2.5 parts by mass of conductive agent and 2.5 parts by mass of binder is coated on the carbon-coated current collector, and the surface capacity is controlled at 3 mA / cm 2 , and obtain the negative electrode sheet.

[0106] Example 5

[0107] This embodiment provides a carbon-coated current collector and a preparation method thereof. The carbon-coated current collector includes a current collector and a carbon film disposed on both sides of the current collector. The current collector is a porous aluminum foil. The thickness of the carbon-coated current collector is 15 μm. The preparation method is shown in Figure 1 and Figure 2 , the steps are:

[0108] (1) Graphene and polytetrafluoroethylene (PTFE) were mixed in a mass ratio of 90:10, added to a stirrer and premixed for 4 hours to obtain a mixture, and the mixture was subjected to a first hot roll pressing at 80° C. and 10F to obtain a carbon film with a thickness of 5 μm;

[0109] (2) The carbon film is introduced onto the rubber coating roller, and the rubber coating roller transfers PTFE onto the surface of the carbon film. The surface loading of PTFE on the surface of the carbon film is 0.2 mg / cm 2 ,like Figure 2 ;

[0110] (3) The two layers of PTFE-coated carbon film and the 10 μm porous aluminum foil were rolled together at a rolling pressure of 15T, and then entered into a 70°C rolling machine, and then entered into 10T, 30T, and 20T rolling machines for a second hot rolling to obtain a carbon-coated current collector. The thickness of the carbon-coated current collector was controlled to be 15 μm. Figure 3 .

[0111] A slurry containing 94 parts by mass of NCM523 positive electrode material, 3 parts by mass of conductive agent and 3 parts by mass of binder was coated on the carbon-coated current collector, and the surface capacity was controlled at 3 mA / cm 2 , and obtain the positive electrode.

[0112] Example 6

[0113] Except that the porous aluminum foil is replaced by a non-porous aluminum foil, the rest is the same as Example 5.

[0114] Example 7

[0115] This embodiment provides a carbon-coated current collector and a preparation method thereof. The carbon-coated current collector includes a current collector and a carbon film disposed on both sides of the current collector. The current collector is a porous copper foil. The thickness of the carbon-coated current collector is 16 μm. The preparation method is shown in Figure 1 and Figure 2 , the steps are:

[0116] (1) Graphene and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 95:5, added to a stirrer and premixed for 4 hours to obtain a mixture, and the mixture was subjected to a first hot roll pressing at 80° C. and 15F to obtain a carbon film with a thickness of 8 μm;

[0117] (2) The carbon film is introduced onto the coating roller, which transfers PVDF onto the surface of the carbon film. The surface loading of PVDF on the carbon film is 0.01 mg / cm 2 ,like Figure 2 ;

[0118] (3) The two layers of PVDF-coated carbon film and 6 μm porous copper foil were rolled together at a rolling pressure of 20T, and then entered into a rolling press at 160°C, and then entered into a rolling press at 10T, 30T, and 20T for a second hot rolling to obtain a carbon-coated current collector. The thickness of the carbon-coated porous current collector was controlled at 16 μm. Figure 2 .

[0119] A slurry containing 97 parts of artificial graphite negative electrode material, 1.5 parts of conductive agent and 1.5 parts of binder in a mass ratio is coated on the above-mentioned carbon-coated current collector, and the surface capacity is controlled at 2 mA / cm 2 , and obtain the negative electrode sheet.

[0120] Example 8

[0121] Except that the porous copper foil is replaced by a non-porous copper foil, the rest is the same as that of Example 7.

[0122] Example 9

[0123] Except that the thickness of the carbon film is 1 μm, the rest is consistent with Example 1.

[0124] Example 10

[0125] Except that the thickness of the carbon film is 11 μm, the rest is consistent with Example 1.

[0126] Embodiment 11

[0127] Except that step (2) is not performed, that is, the carbon film is not coated with the second binder, the rest is consistent with Example 1.

[0128] Example 12

[0129] Except that the surface loading of PTFE in step (2) is 0.3, the rest is consistent with Example 1.

[0130] Example 13

[0131] Except that graphite is replaced by conductive carbon black and carbon nanotubes in a ratio of 1:1, the rest is the same as Example 3.

[0132] Embodiment 14

[0133] Except that the mass ratio of carbon nanotubes to styrene-butadiene rubber (SBR) is 98:2, the rest is consistent with Example 4.

[0134] Embodiment 15

[0135] Except that integrated rolling is not performed in step (3), the rest is consistent with Example 4.

[0136] Comparative Example 1

[0137] This comparative example provides a carbon-coated current collector and a preparation method thereof, wherein the carbon-coated current collector comprises a current collector and a carbon layer disposed on both sides of the current collector, the current collector is a non-porous aluminum foil, the thickness of the carbon-coated current collector is 15 μm, and the preparation method is:

[0138] (1) Conductive carbon black (SP) and polytetrafluoroethylene (PTFE) were mixed in a mass ratio of 98:2, added to a stirrer and premixed for 4 h, and an appropriate amount of deionized water was added to form a carbon slurry;

[0139] (2) coating the carbon slurry on a 10 μm aluminum foil and drying it to obtain a 5 μm carbon film;

[0140] (3) The two layers of carbon film and 10 μm non-porous aluminum foil are integrated by rolling at a rolling pressure of 15T, and then enter into a rolling press at 80°C, and then enter into 10T, 30T, and 20T rolling presses for a second hot rolling to obtain a carbon-coated current collector. The thickness of the carbon-coated current collector is controlled at 15 μm.

[0141] The preparation of the positive electrode sheet in this comparative example is consistent with that in Example 1.

[0142] Comparative Example 2

[0143] This comparative example provides a carbon-coated current collector and a preparation method thereof, wherein the carbon-coated current collector comprises a current collector and a carbon layer disposed on both sides of the current collector, the current collector is a non-porous aluminum foil, the thickness of the carbon-coated current collector is 13 μm, and the preparation method is:

[0144] (1) carbon nanotubes and polyacrylic acid (PAA) were mixed in a mass ratio of 95:5, added to a stirrer and premixed for 1 h, and an appropriate amount of deionized water was added to form a carbon slurry;

[0145] (2) coating the carbon slurry on a 10 μm non-porous aluminum foil and drying it to obtain a 3 μm carbon film;

[0146] (3) The two layers of carbon film and 10 μm non-porous aluminum foil were integrated by rolling at a rolling pressure of 25 T, and then entered into a rolling press at 80°C, and then entered into 10T, 30T, and 20T rolling presses for a second hot rolling to obtain a carbon-coated current collector. The thickness of the carbon-coated current collector was controlled at 13 μm.

[0147] The preparation of the positive electrode sheet in this comparative example is consistent with that in Example 2.

[0148] Comparative Example 3

[0149] This comparative example provides a carbon-coated current collector and a preparation method thereof, wherein the carbon-coated current collector comprises a current collector and a carbon layer disposed on both sides of the current collector, the current collector is a non-porous copper foil, the thickness of the carbon-coated current collector is 20 μm, and the preparation method is:

[0150] (1) Graphite and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 99:1, added to a stirrer and premixed for 4 h, and an appropriate amount of N-methylpyrrolidone was added to form a carbon slurry;

[0151] (2) coating the carbon slurry on a 6 μm non-porous copper foil and drying it to obtain a 10 μm carbon film;

[0152] (3) The two layers of carbon film and the 6 μm non-porous copper foil are integrated by rolling at a rolling pressure of 15 T, and then enter into a rolling press at 160°C, and then enter into 10 T, 30 T, and 20 T rolling presses for a second hot rolling to obtain a carbon-coated current collector. The thickness of the carbon-coated current collector is controlled at 20 μm.

[0153] The preparation of the negative electrode sheet in this comparative example is consistent with that in Example 3.

[0154] Comparative Example 4

[0155] This comparative example provides a carbon-coated current collector and a preparation method thereof, wherein the carbon-coated current collector comprises a current collector and a carbon layer disposed on both sides of the current collector, the current collector is a non-porous copper foil, the thickness of the carbon-coated current collector is 8 μm, and the preparation method is:

[0156] (1) carbon nanotubes and styrene-butadiene rubber (SBR) were mixed in a mass ratio of 99.5:0.5, added to a stirrer for premixing for 8 hours, and an appropriate amount of deionized water was added to form a carbon slurry;

[0157] (2) coating the carbon slurry on a 6 μm non-porous copper foil and drying it to obtain a 2 μm carbon film;

[0158] (3) The two layers of carbon film and the 6 μm non-porous copper foil were integrated by rolling at a rolling pressure of 30 T, and then entered into a rolling press at 160°C, and then entered into 20 T, 50 T, and 20 T rolling presses for a second hot rolling to obtain a carbon-coated current collector. The thickness of the carbon-coated current collector was controlled at 8 μm.

[0159] The preparation of the negative electrode sheet in this comparative example is consistent with that in Example 4.

[0160] Comparative Example 5

[0161] This comparative example provides a carbon-coated current collector and a preparation method thereof, wherein the carbon-coated current collector comprises a current collector and a carbon layer disposed on both sides of the current collector, the current collector is a non-porous aluminum foil, the thickness of the carbon-coated current collector is 15 μm, and the preparation method is:

[0162] (1) Graphene and polytetrafluoroethylene (PTFE) were mixed in a mass ratio of 90:10, added to a stirrer and premixed for 1 h, and an appropriate amount of deionized water was added to form a carbon slurry;

[0163] (2) coating the carbon slurry on a 10 μm non-porous aluminum foil and drying it to obtain a 5 μm carbon film;

[0164] (3) The two layers of carbon film and 10 μm non-porous aluminum foil are integrated by rolling at a rolling pressure of 15T, and then enter into a rolling press at 70°C, and then enter into 10T, 30T, and 20T rolling presses for a second hot rolling to obtain a carbon-coated current collector. The thickness of the carbon-coated current collector is controlled at 15 μm.

[0165] The preparation of the positive electrode sheet in this comparative example is consistent with that in Example 5.

[0166] Comparative Example 6

[0167] This comparative example provides a carbon-coated current collector and a preparation method thereof, wherein the carbon-coated current collector comprises a current collector and a carbon layer disposed on both sides of the current collector, the current collector is a non-porous copper foil, the thickness of the carbon-coated current collector is 15 μm, and the preparation method is:

[0168] (1) Graphene and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 95:5, added to a stirrer and premixed for 1 h, and an appropriate amount of deionized water was added to form a carbon slurry;

[0169] (2) coating the carbon slurry on a 6 μm non-porous copper foil and drying it to obtain an 8 μm carbon film;

[0170] (3) The two layers of carbon film and the 6 μm non-porous copper foil are integrated by rolling at a rolling pressure of 20 T, and then enter into a rolling press at 160°C, and then enter into 10 T, 30 T, and 20 T rolling presses for a second hot rolling to obtain a carbon-coated current collector. The thickness of the carbon-coated current collector is controlled at 16 μm.

[0171] The preparation of the negative electrode sheet in this comparative example is consistent with that in Example 7.

[0172] 1. Preparation of button cells

[0173] Punch the positive electrode sheets or negative electrode sheets of Examples 1-4, Examples 9-15 and Comparative Examples 1-4 to obtain round sheets with a diameter of 10 mm, use them as working electrodes, and assemble button cells with PE diaphragms, metal lithium sheets and 1M LiPF6 electrolyte.

[0174] 2. Electrochemical performance test of button battery

[0175] The prepared button battery was left to stand at room temperature for 8 h to allow the electrolyte to fully infiltrate. After cooling to room temperature, it was formed at 0.05C / 0.05C. Then, the rate test was carried out in the voltage window of 3.0-4.2V. The conditions were: 0.1C / 0.1C, 0.2C / 0.2C, 0.5C / 0.5C, 1C / 1C, 0.2C / 0.2C. The discharge specific capacity at each rate is shown in Table 1.

[0176] Table 1

[0177]

[0178]

[0179] By comparing Example 1 with Examples 9-10 in Table 1, it can be seen that the thickness of the carbon film will affect the performance of the carbon-coated current collector. When the carbon film is thicker, as the integrated rolling and the second hot rolling compact the carbon layer, the flexibility of the carbon film current collector decreases and causes breakage. When the carbon film is thinner, the hole area will collapse when it is bonded to the porous aluminum foil, resulting in an uneven surface of the carbon-coated current collector. What is more serious is that the carbon film breaks at the edge of the hole. Therefore, the discharge specific capacity of Examples 9-10 at different rates is worse than that of Example 1.

[0180] By comparing Example 1 with Examples 10-11 in Table 1, it can be seen that coating the surface of the carbon film with a suitable surface loading of the second binder in the present invention is beneficial to improving the electrochemical properties of the carbon film. In Example 11, no coating was performed, the contact between the carbon film and the aluminum foil was not tight, and the contact resistance increased. In Example 12, the surface loading of the second binder was relatively high, resulting in a tight contact between the carbon film and the aluminum foil, but the insulating property of the binder weakened the ability of electron conduction. Therefore, the large current discharge capability of Examples 11-12 is worse than that of Example 1.

[0181] By comparing Example 3 with Example 13 in Table 1, it can be seen that there is a most suitable choice of carbon material in the present invention, and the conductive carbon black and carbon nanotubes work synergistically with the preparation method and porous current collector of the present invention to further improve the electrochemical properties of the carbon-coated current collector. Therefore, the specific capacity of Example 13 is higher than that of Example 3.

[0182] By comparing Example 4 and Example 14 in Table 1, it can be seen that the contents of the carbon material and the first binder in the present invention exist in a preferred range. When the ratio of the two exceeds the preferred range, the specific capacity of the prepared button battery will be reduced. Therefore, the specific capacity of Example 14 is slightly lower than that of Example 4.

[0183] By comparing Example 4 and Example 15 in Table 1, it can be seen that in the present invention, integrated rolling is arranged before the second hot rolling, which is beneficial to improving the contact between carbon particles in the carbon film and pre-bonding the binder to the current collector. Integrated rolling is not performed in Example 15, so the material performance capacity is worse than that of Example 4.

[0184] By comparing Example 1 and Comparative Example 1, Example 2 and Comparative Example 2, Example 3 and Comparative Example 3, and Example 4 and Comparative Example 4 in Table 1, it can be seen that the carbon-coated current collector prepared by the dry process combined with the porous current collector in the present invention has a higher specific capacity and better rate performance, is suitable for a variety of electrode materials, and can exert good electrochemical performance in both the positive and negative electrodes. At different rates, the corresponding embodiments have higher discharge capacities than their comparative examples.

[0185] 3. Preparation of solid-state batteries

[0186] The positive electrode sheets or negative electrode sheets of Examples 5-8 and Comparative Examples 5 and 6 were punched to obtain squares with a side length of 30 mm*30 mm. The squares were used as working electrodes and assembled into soft-package batteries with solid electrolyte Li6PS5Cl (LPSC) and metallic lithium.

[0187] 2. Electrochemical performance test: The above-mentioned soft-package battery was left to stand at room temperature for 8 hours and then charged at 0.05C / 0.05C. Then, a 0.1C / 0.1C cycle test was performed in a voltage window of 2.8-4.2V. The discharge capacity of the solid-state battery after 50 cycles, 100 cycles and 200 cycles was tested. The discharge capacity after the cycle was divided by the discharge capacity of the first cycle to obtain the retention rate at different cycle numbers.

[0188] Table 2

[0189]

[0190]

[0191] By comparing Examples 5-6 with Comparative Example 5, and comparing Examples 7-8 with Comparative Example 6, it can be seen that the carbon-coated current collector prepared by the dry process in the present invention has better cycle stability, and the dry process and the porous current collector work synergistically to prepare the solid-state battery with the highest capacity retention rate. Therefore, the capacity retention rate of Example 5 at different cycle numbers is not lower than that of Example 6, and that of Example 7 is not lower than that of Example 8. As the cycle number increases, Examples 5 and 7 have the best cycle stability.

[0192] From the above Examples 1-15, it can be seen that the present invention prepares a carbon film by dry mixing a certain proportion of carbon material and a fiberizable binder, and rolls it with a current collector to form a carbon-coated current collector, thereby avoiding the introduction of solvents, reducing the production cost of the electrochemical device, and improving the capacity retention rate and rate performance of the electrochemical device.

[0193] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a carbon-coated current collector, characterized in that: The preparation method comprises: (1) dry-mixing a carbon material and a first binder to obtain a mixture, and performing a first roll pressing on the mixture to obtain a carbon film; Wherein, the first binder is a polymer that can be fiberized; (2) coating a second binder on a surface of the carbon film in step (1) close to the current collector, placing the carbon film coated with the second binder on at least one surface of the current collector, and performing a second rolling process to obtain a carbon-coated current collector; The current collector is a porous current collector; the surface loading of the second binder on the carbon film is 0.01 to 0.2 mg / cm 2 .

2. The preparation method according to claim 1, characterized in that: The current collector is aluminum foil or copper foil.

3. The preparation method according to claim 1, characterized in that: The thickness of the current collector is 6-10 μm.

4. The preparation method according to claim 1, characterized in that: The mass ratio of the carbon material to the first binder is x:(1-x), where x is 0.5-1.

5. The preparation method according to claim 1, characterized in that: The carbon material in step (1) includes any one of conductive carbon black, graphene, graphite, acetylene black, carbon nanotubes and graphene-carbon nanotube hybrids, or a combination of at least two thereof.

6. The preparation method according to claim 1, characterized in that: Step (1) The first binder includes any one of polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber and polyacrylic acid, or a combination of at least two of them.

7. The preparation method according to claim 1, characterized in that: In step (1), the first rolling is a first hot rolling.

8. The preparation method according to claim 7, characterized in that: The temperature of the first hot roller pressing is 80-160°C.

9. The preparation method according to claim 7, characterized in that: The pressure of the first hot roller pressing is 10-50T.

10. The preparation method according to claim 1, characterized in that: The thickness of the carbon film in step (1) is 2 to 10 μm.

11. The preparation method according to claim 1, characterized in that: The surface loading of the first binder on the carbon film is 0.05-0.2 mg / cm 2 .

12. The preparation method according to claim 1, characterized in that: The second binder includes any one of polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber and polyacrylic acid, or a combination of at least two of them.

13. The preparation method according to claim 1, characterized in that: The second rolling process in step (2) includes integrated rolling and second hot rolling.

14. The preparation method according to claim 13, characterized in that: The temperature of the integrated rolling is 80-160°C.

15. The preparation method according to claim 13, characterized in that: The integrated rolling pressure is 10-50T.

16. The preparation method according to claim 13, characterized in that: The temperature of the second hot roller pressing is 80-160°C.

17. The preparation method according to claim 13, characterized in that: The pressure of the second hot roller pressing is 10-50T.

18. A carbon-coated current collector, characterized in that: The carbon-coated current collector is prepared by the preparation method according to any one of claims 1 to 17, and the carbon-coated current collector comprises a current collector and a carbon film disposed on at least one side of the current collector; Wherein, the current collector is a porous current collector; The thickness of the carbon-coated current collector is 9-20 μm.