Copper-molybdenum metal film etching liquid, application method thereof and display panel

By using hydrogen peroxide, inorganic acid, ethylenediaminetetrapropionic acid and potassium chromate in the copper-molybdenum metal film etching solution to balance the etching rates of copper and molybdenum, the problems of molybdenum residue and uneven etching in the existing technology are solved. , achieving high-precision copper-molybdenum metal film etching.

CN114411151BActive Publication Date: 2024-10-11FUJIAN ZHONGAN HIGH-TECH MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210057992.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-19
Publication Date
2024-10-11
Estimated Expiration
2042-01-19

AI Technical Summary

Technical Problem

The existing etching solution has an uneven etching effect on molybdenum and copper, resulting in problems of molybdenum residue and uneven etching, making it difficult to achieve high-precision etching of copper-molybdenum metal films.

Method used

Use a copper-molybdenum metal film etching solution containing hydrogen peroxide, inorganic acid, ethylenediaminetetrapropionic acid and potassium chromate to balance the etching rates of copper and molybdenum and reduce molybdenum through etching under acidic conditions and the formation of an inorganic passivation film. residue and improve etching accuracy.

Benefits of technology

It achieves balanced etching of the copper-molybdenum metal film, reduces molybdenum residue, improves etching accuracy and product yield, and ensures high-precision copper-molybdenum metal film etching effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114411151B_ABST
    Figure CN114411151B_ABST
Patent Text Reader

Abstract

The present application provides a copper-molybdenum metal film etching solution and its application method and display panel, the etching solution includes the following components in percentage by mass: hydrogen peroxide: 10% to 30%; inorganic acid: 5% to 20%; etching regulator: 0.5% to 2%; water: 60% to 80%; wherein the etching regulator includes ethylenediaminetetrapropionic acid and potassium chromate. The copper-molybdenum metal film etching solution not only has good stability, but also has a relatively balanced etching rate for metal copper and metal molybdenum. Using the etching solution to etch the copper-molybdenum metal film can eliminate the molybdenum residue and achieve a good etching effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of etching liquid, and in particular to a copper-molybdenum metal film etching liquid, an application method thereof, and a display panel. Background Art

[0002] Liquid crystal display (LCD) includes a liquid crystal display panel and a backlight module. The liquid crystal display panel generally includes a CF (color filter) substrate, a TFT (thin film transistor) array substrate and a liquid crystal (liquid crystal). The direction of the liquid crystal molecules can be controlled by supplying power to the TFT array substrate, so that the light of the backlight module is projected onto the CF substrate to produce a picture. The preparation of the microcircuit in the TFT array substrate is to first form a conductive metal layer on the substrate, then apply a photoresist on the metal layer, and develop the microcircuit on the photoresist, and then use an etching liquid to etch the metal layer not covered by the photoresist to form the microcircuit. At present, copper (Cu) and molybdenum (Mo) are widely used as metal layers in electronic circuits in TFT array substrates. However, the etching effects of existing etching solutions on molybdenum and copper are quite different, and the etching rate of molybdenum is much lower than that of copper, resulting in problems of molybdenum residue and uneven etching. Summary of the invention

[0003] In view of this, the present application provides a copper-molybdenum metal film etching solution, which not only has good stability, but also has a relatively balanced etching rate for metallic copper and metallic molybdenum. Using this etching solution to etch the copper-molybdenum metal film is beneficial to reducing molybdenum residue and achieving a good etching effect.

[0004] The first aspect of the present application provides a copper-molybdenum metal film etching solution, comprising the following components in percentage by mass:

[0005] Hydrogen peroxide: 10% to 30%;

[0006] Inorganic acid: 5% to 20%;

[0007] Etching regulator: 0.5% to 2%;

[0008] Water: 60%-80%;

[0009] The etching conditioner includes ethylenediaminetetrapropionic acid and potassium chromate.

[0010] In the copper-molybdenum metal film etching solution of the present application, hydrogen peroxide can convert metallic copper and metallic molybdenum into water-soluble metal ions under acidic conditions, thereby removing the metal layer not covered by the photoresist; the etching regulator is used to balance the etching rate of the etching solution on metallic copper and metallic molybdenum, wherein ethylenediaminetetrapropionic acid has good affinity for metallic copper, can be adsorbed on the surface of metallic copper to form an organic molecular film, inhibits direct contact between the etching solution and metallic copper, thereby slowing down the etching of metallic copper by the etching solution, and during the etching process, ethylenediaminetetrapropionic acid will also complex with the released copper ions, reduce the free metal ion content in the etching solution, and improve the stability of hydrogen peroxide in the etching solution; potassium chromate can form an inorganic passivation film on the surface of the metal layer, the inorganic passivation film can not only reduce the etching rate of the etching solution on metallic copper, but also the inorganic passivation film can cooperate with the organic molecular film to make the etching solution form a moderate etching angle (Taper angle) and a lower critical dimension loss (CD loss) at the edge of the metal layer, thereby achieving high-precision etching. Under the synergistic effect of the above-mentioned specific mass percentage components, the copper-molybdenum metal film etching solution has a relatively balanced etching rate for metallic copper and metallic molybdenum, can achieve uniform etching of the metal layer, and the array substrate obtained after etching is free of molybdenum residue, meeting the requirements for high-precision etching of the copper-molybdenum metal film.

[0011] Optionally, the mass ratio of the ethylenediaminetetrapropionic acid to the potassium chromate is 1:(0.1-5).

[0012] Optionally, the etching regulator further includes o-phenanthroline.

[0013] Optionally, the mass ratio of the ethylenediaminetetrapropionic acid to the o-phenanthroline is 1:(0.1-2).

[0014] Optionally, the inorganic acid includes one or more of nitric acid, sulfuric acid and hydrochloric acid, and the mass ratio of nitrate ions in the copper-molybdenum metal film etching solution to the ethylenediaminetetrapropionic acid is less than or equal to 0.01.

[0015] Optionally, the inorganic acid includes one or more of nitric acid, sulfuric acid and hydrochloric acid, and the ratio of the mass of nitrate ions in the copper-molybdenum metal film etching solution to the sum of the masses of the ethylenediaminetetrapropionic acid and the 1,1-diazole.

[0016] Optionally, the copper-molybdenum metal film etching solution also includes a hydrogen peroxide stabilizer with a mass percentage of 0.05%-0.5%, and the hydrogen peroxide stabilizer includes one or more of triethanolamine, triethylenetetramine, diphenylamino urea and 8-hydroxyquinoline.

[0017] Optionally, the mass ratio of the hydrogen peroxide stabilizer to the hydrogen peroxide is 1:(20-100).

[0018] Optionally, the copper-molybdenum metal film etching solution also includes an organic acid with a mass percentage of 5% to 18%, and the organic acid includes one or more of oxalic acid, tartaric acid, citric acid and sulfosalicylic acid.

[0019] Optionally, the inorganic acid includes one or more of nitric acid, sulfuric acid and hydrochloric acid.

[0020] Optionally, the pH value of the copper-molybdenum metal film etching solution is 3-4.

[0021] Optionally, the copper-molybdenum metal film etching solution includes the following components in percentage by mass:

[0022] Hydrogen peroxide: 10% to 30%;

[0023] Inorganic acid: 5% to 20%;

[0024] Water: 60%~80%;

[0025] Ethylenediaminetetrapropionic acid: 0.01%~1%;

[0026] Potassium chromate: 0.01% to 1%;

[0027] Phthalophenanthroline: 0.01%~1%.

[0028] In a second aspect, the present application provides an application method of a copper-molybdenum metal film etching liquid, comprising the following steps: contacting the copper-molybdenum metal film etching liquid as described in the first aspect with a substrate having a copper-molybdenum metal film on its surface to etch the copper-molybdenum metal film.

[0029] Optionally, the etching time is 80s to 160s, and the etching temperature is 25°C to 40°C.

[0030] In a third aspect, the present application provides a display panel, which includes a metal layer, and the metal layer is produced by the application method of the copper-molybdenum metal film etching solution as described in the second aspect.

[0031] Optionally, a critical dimension loss of the metal layer is less than or equal to 0.9 μm, and an etching angle of the metal layer is 35° to 75°. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 A schematic structural diagram of a TFT substrate precursor provided in one embodiment of the present application;

[0033] Figure 2 A schematic diagram of a sample structure after etching provided in one embodiment of the present application;

[0034] Figure 3 This is an electron microscope characterization image of the sample after etching provided in Example 7 of the present application;

[0035] Figure 4 This is the electron microscope characterization image of the sample after etching provided in Comparative Example 1 of this application. Figure 4 (a) is a morphology characterization diagram of the left side of the sample after etching in Comparative Example 1. Figure 4 (b) is a morphology characterization diagram of the right side of the sample after etching in Comparative Example 1. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0037] Existing TFT-LCD devices mostly use copper metal with low resistivity as wiring material, and add molybdenum metal to improve the bonding strength between the metal layer and the substrate. Therefore, the copper-molybdenum metal film is the main structure of the metal wire in the TFT array substrate. In the preparation process of the TFT array substrate, the copper-molybdenum metal film needs to be etched to obtain a microcircuit. However, the existing etchant is prone to produce molybdenum residue during the etching process, which is not conducive to forming a high-precision wiring structure. The present application provides a copper-molybdenum metal film etching solution. Using the etching solution to etch the copper-molybdenum metal film is conducive to eliminating molybdenum residue, improving etching accuracy, and achieving a good etching effect.

[0038] It should be noted that the copper-molybdenum metal film in the present application refers to a multilayer film in which one or more copper films and one or more molybdenum films and / or molybdenum alloy films are stacked on top of each other. The copper-molybdenum metal film can be, for example, a copper film / molybdenum film double-layer film, a copper film / molybdenum alloy film double-layer film, or a molybdenum film / copper film / molybdenum film triple-layer film.

[0039] In the implementation manner of the present application, the copper-molybdenum metal film etching solution includes the following components in percentage by mass:

[0040] Hydrogen peroxide: 10% to 30%;

[0041] Inorganic acid: 5% to 20%;

[0042] Etching regulator: 0.5% to 2%;

[0043] Water: 60%-80%;

[0044] Etch conditioners include ethylenediaminetetrapropionic acid and potassium chromate.

[0045] In the present application, the inorganic acid can provide hydrogen ions, and hydrogen peroxide can etch the copper-molybdenum metal film in an acidic environment to remove the copper-molybdenum metal film that is not covered by the photoresist. The etching regulator is used to reduce the etching rate of the etching solution on the metal copper, so that the etching solution has a relatively balanced etching rate on the metal copper and the metal molybdenum, suppresses the residual molybdenum, and improves the production efficiency. Specifically, the polar groups in ethylenediaminetetrapropionic acid give it a good affinity for metal copper, and it can adhere to the surface of the metal copper and form an organic molecular film; potassium chromate will form an inorganic passivation film on the metal surface during the etching process. The inorganic passivation film and the organic molecular film can synergistically reduce the etching rate of the etching solution on the metal copper, suppress the residual molybdenum, and optimize the etching morphology, ensuring that the obtained product has a moderate etching angle and a low critical dimension loss, meeting the requirements of high-precision etching of the copper-molybdenum metal film.

[0046] In the present application, ethylenediaminetetrapropionic acid contains polar groups, which can be adsorbed by the surface charge of the metal to form an organic molecular film on the surface of the metal copper, inhibiting the etching of the metal copper by the etching solution; during the etching process, copper ions are released from the metal surface, and ethylenediaminetetrapropionic acid can complex the released copper ions to reduce the copper ion concentration around the metal layer, inhibit the reaction of copper ions catalyzing the decomposition of hydrogen peroxide, and improve the stability of the etching solution and the uniformity of etching. The inventors of the present application have found that the carbon chain length of ethylenediaminetetrapropionic acid is moderate, and its adsorption capacity for metals and its complexing capacity for metal ions are relatively balanced, so ethylenediaminetetrapropionic acid can be gathered on the metal surface, which can reduce the etching rate of metal copper and inhibit the increase of copper ion concentration. In some embodiments of the present application, the mass percentage of ethylenediaminetetrapropionic acid in the copper-molybdenum metal film etching solution is 0.01% to 1.5%. The mass percentage of EDTA in the copper-molybdenum metal film etching solution can be, but is not limited to, 0.01%, 0.08%, 0.1%, 0.3%, 0.5%, 0.8%, 1% or 1.5%. When the mass percentage of EDTA in the copper-molybdenum metal film etching solution is within the above range, the etching rate of the etching solution on the metal copper can be effectively slowed down.

[0047] Since ethylenediaminetetrapropionic acid will complex with copper ions, resulting in the continuous reconstruction of the formed organic molecular film, the addition of potassium chromate in the etching solution of the present application can make up for the deficiency of ethylenediaminetetrapropionic acid, inhibit the etching solution from over-etching the areas with higher reaction activity in the metal film, form a moderate etching angle, and improve the uniformity of etching. Specifically, during the dissolution of the metal layer, the pH value around the metal layer increases, and potassium chromate can form a chromate passivation film on the surface of the metal layer, thereby inhibiting the etching reaction in the areas with higher reaction activity in the metal layer and reducing the etching rate of the etching solution on the metal copper. In some embodiments of the present application, the mass percentage of potassium chromate in the copper-molybdenum metal film etching solution is 0.01% to 1%. The mass percentage of potassium chromate in the copper-molybdenum metal film etching solution can be specifically but not limited to 0.01%, 0.08%, 0.1%, 0.3%, 0.5%, 0.8% or 1%.

[0048] In some embodiments of the present application, the mass ratio of ethylenediaminetetrapropionic acid to potassium chromate is 1:(0.1-5). The mass ratio of ethylenediaminetetrapropionic acid to potassium chromate may be, but is not limited to, 1:0.1, 1:0.4, 1:0.8, 1:1, 1:2, 1:3 or 1:5. When the mass ratio of ethylenediaminetetrapropionic acid to potassium chromate is controlled within the above range, ethylenediaminetetrapropionic acid and potassium chromate can play a good synergistic role, reduce the etching rate of the etching solution on metallic copper, eliminate molybdenum residues, reduce the deviation of the etching angle, and improve the etching accuracy.

[0049] In some embodiments of the present application, the etching regulator also includes o-phenanthroline. O-phenanthroline has a weak adsorption force on metallic copper, but has a strong complexing ability for copper ions. Adding o-phenanthroline can reduce the concentration of copper ions around the metal layer, improve the stability of the ethylenediaminetetrapropionic acid organic molecular film, and help slow down the etching of metallic copper by the etching solution. In some embodiments of the present application, the mass percentage of o-phenanthroline in the copper-molybdenum metal film etching solution is 0.01% to 1%. The mass percentage of o-phenanthroline in the copper-molybdenum metal film etching solution can be, but not limited to, 0.01%, 0.08%, 0.1%, 0.3%, 0.5%, 0.8% or 1%. In some embodiments of the present application, the mass ratio of ethylenediaminetetrapropionic acid to o-phenanthroline is 1: (0.1 to 2). The mass ratio of ethylenediaminetetrapropionic acid to o-phenanthroline can be, but not limited to, 1: 0.1, 1: 0.4, 1: 0.8, 1: 1 or 1: 2. When the mass ratio of ethylenediaminetetrapropionic acid to o-phenanthroline is controlled within the above range, not only can the etching rate of the etching solution on metallic copper be effectively slowed down, but also the copper ion concentration around the metal layer can be reduced, the decomposition of hydrogen peroxide can be inhibited, the stability of the etching solution can be improved, and uniform etching can be achieved.

[0050] In some embodiments of the present application, the copper-molybdenum metal film etching solution also includes a hydrogen peroxide stabilizer, and the hydrogen peroxide stabilizer includes one or more of triethanolamine, triethylenetetramine, diphenylaminourea and 8-hydroxyquinoline. The above substances not only do not interfere with the formation of organic molecular films and inorganic passivation films, but also can stabilize hydrogen peroxide ions, inhibit the formation of hydrogen peroxide free radicals, slow down the decomposition rate of hydrogen peroxide, improve the uniformity of etching, and extend the service life of the etching solution. In some embodiments of the present application, the mass percentage of the hydrogen peroxide stabilizer in the copper-molybdenum metal film etching solution is 0.05%-0.5%. The mass percentage of the hydrogen peroxide stabilizer in the copper-molybdenum metal film etching solution can be, but is not limited to, 0.05%, 0.08%, 0.1%, 0.2%, 0.3% or 0.5%.

[0051] In some embodiments of the present application, the copper-molybdenum metal film etching solution also includes an organic acid, and the organic acid includes one or more of oxalic acid, tartaric acid, citric acid and sulfosalicylic acid. The organic acid can effectively adjust the concentration of hydrogen ions in the solution, improve the stability of the etching process, and facilitate the uniform etching of the copper-molybdenum metal film. In some embodiments of the present application, the mass percentage of the organic acid in the copper-molybdenum metal film etching solution is 5% to 18%. The mass percentage of the organic acid in the copper-molybdenum metal film etching solution can be, but is not limited to, 5%, 8%, 10%, 12%, 15% or 18%.

[0052] In some embodiments of the present application, the inorganic acid includes one or more of nitric acid, sulfuric acid and hydrochloric acid.

[0053] In some embodiments of the present application, the inorganic acid includes one or more of sulfuric acid and hydrochloric acid. Sulfuric acid and hydrochloric acid have good compatibility with the etching conditioner of the present application, which is conducive to the etching conditioner to fully exert its effect.

[0054] In some embodiments of the present application, the mass ratio of nitrate ions to ethylenediaminetetrapropionic acid in the copper-molybdenum metal film etching solution is less than or equal to 0.01. In some embodiments of the present application, the ratio of the mass of nitrate ions in the copper-molybdenum metal film etching solution to the sum of the masses of ethylenediaminetetrapropionic acid and 1,2-phenanthroline is less than or equal to 0.01. Controlling the content of nitrate ions can ensure that ethylenediaminetetrapropionic acid and 1,2-phenanthroline can effectively complex free copper ions in the etching solution, inhibit the decomposition of hydrogen peroxide, and extend the service life of the etching solution.

[0055] The copper-molybdenum metal film etching solution provided in the present application can not only balance the etching rates of the etching solution on metal copper and metal molybdenum and eliminate molybdenum residues through the mutual synergy between components, but also the metal layer after etching has a moderate etching angle (Taper angle) and a low critical dimension loss (CD loss), which can achieve high-precision etching and effectively improve the yield of the product.

[0056] The present application also provides a method for preparing the copper-molybdenum metal film etching solution, which comprises: uniformly mixing the following raw materials in percentage by mass to obtain the copper-molybdenum metal film etching solution:

[0057] Hydrogen peroxide: 10% to 30%;

[0058] Inorganic acid: 5% to 20%;

[0059] Etching regulator: 1% to 2%;

[0060] Water: 60%~80%;

[0061] Etch conditioners include ethylenediaminetetrapropionic acid and potassium chromate.

[0062] The preparation method of the copper-molybdenum metal film etching solution provided in the present application is simple to operate and has high production efficiency, and is suitable for large-scale industrial production.

[0063] The present application also provides an application method of the copper-molybdenum metal film etching solution, comprising:

[0064] A TFT substrate precursor is provided, wherein the TFT substrate precursor comprises a substrate and a copper-molybdenum metal film arranged on a surface of the substrate; a copper-molybdenum metal film etching liquid is brought into contact with the TFT substrate precursor to etch the copper-molybdenum metal film.

[0065] In some embodiments of the present application, contacting the copper-molybdenum metal film etching liquid with the TFT substrate precursor includes immersing the TFT substrate precursor in the copper-molybdenum metal film etching liquid, or spraying / rinsing the copper-molybdenum metal film etching liquid on the surface of the copper-molybdenum metal film in the TFT substrate precursor. The specific selection can be made according to actual production conditions.

[0066] In some embodiments of the present application, the etching time is 80s to 160s. The etching time can be, but is not limited to, 80s, 100s, 120s, 150s or 160s. Controlling the etching time can ensure that there is no residue after etching, and the etched product has high precision. In some embodiments of the present application, the etching temperature is 25°C to 40°C. The etching temperature can be, but is not limited to, 25°C, 28°C, 30°C, 32°C, 35°C or 40°C. The appropriate temperature can ensure the etching accuracy and etching speed.

[0067] The application method of the copper-molybdenum metal film etching solution provided in the present application can complete the etching of the copper film and the molybdenum film in the copper-molybdenum metal film through one etching, and this method has no molybdenum residue, good etching uniformity, smooth etching angle, and high precision, which greatly improves the etching efficiency and has good application prospects.

[0068] The present application also provides a display panel, which is manufactured by the application method of the copper-molybdenum metal film etching solution.

[0069] The implementation of the present application is further described below with reference to a number of embodiments.

[0070] Example 1

[0071] A copper-molybdenum metal film etching solution comprises the following components in percentage by mass:

[0072] Hydrogen peroxide: 20%; sulfuric acid: 10%; water: 69%; ethylenediaminetetrapropionic acid: 0.8%; potassium chromate: 0.2%.

[0073] A method for applying a copper-molybdenum metal film etching solution, comprising:

[0074] Provide TFT substrate precursors, please refer to Figure 1 , Figure 1 A structural schematic diagram of a TFT substrate precursor provided for an embodiment of the present application, the TFT substrate precursor includes a substrate 10, a copper-molybdenum metal film 20 arranged on the surface of the substrate 10 and a photoresist 30 arranged on the surface of the copper-molybdenum metal film 20, the copper-molybdenum metal film includes a molybdenum layer 21 close to the substrate 10, a molybdenum layer 23 close to the photoresist 30 and a copper layer 22 located between the molybdenum layer 21 and the molybdenum layer 23.

[0075] At 31° C., the TFT substrate precursor was immersed in a copper-molybdenum metal film etching solution for 100 seconds, and then cleaned and dried with nitrogen to obtain an etched sample S1.

[0076] See also Figure 2 , Figure 2 A schematic diagram of the sample structure after etching is provided for an embodiment of the present application. Due to the isotropy of chemical etching, the etching solution will cause certain side etching to the copper-molybdenum metal film. The maximum distance between the side wall boundary of the copper-molybdenum metal film and the side wall of the photoresist caused by the side etching is the critical dimension loss, and the angle between the side wall of the copper-molybdenum metal film and the substrate is the etching angle.

[0077] Example 2

[0078] A copper-molybdenum metal film etching solution comprises the following components in percentage by mass:

[0079] Hydrogen peroxide: 20%; sulfuric acid: 10%; water: 68.1%; ethylenediaminetetrapropionic acid: 0.2%; potassium chromate: 1.7%.

[0080] The copper-molybdenum metal film etching solution of Example 2 is used to etch the TFT substrate precursor. The etching conditions are the same as those of Example 1, and the etched sample S2 is obtained.

[0081] Example 3

[0082] A copper-molybdenum metal film etching solution comprises the following components in percentage by mass:

[0083] Hydrogen peroxide: 20%; Hydrochloric acid: 10%; Water: 68.4%; Ethylenediaminetetrapropionic acid: 1.5%; Potassium chromate: 0.1%.

[0084] The copper-molybdenum metal film etching solution of Example 3 is used to etch the TFT substrate precursor. The etching conditions are the same as those of Example 1, and the etched sample S3 is obtained.

[0085] Example 4

[0086] A copper-molybdenum metal film etching solution comprises the following components in percentage by mass:

[0087] Hydrogen peroxide: 20%; hydrochloric acid: 5%; sulfuric acid: 5%; water: 68.2%; ethylenediaminetetrapropionic acid: 0.4%; potassium chromate: 0.4%; o-phenanthroline: 1%.

[0088] The TFT substrate precursor was etched using the copper-molybdenum metal film etching solution of Example 4, and the etching conditions were the same as those of Example 1 to obtain the etched sample S4.

[0089] Example 5

[0090] A copper-molybdenum metal film etching solution, comprising the following components in percentage by weight:

[0091] Hydrogen peroxide: 20%; hydrochloric acid: 5%; sulfuric acid: 5%; water: 69%; ethylenediaminetetrapropionic acid: 0.4%; potassium chromate: 0.4%; o-phenanthroline: 0.2%.

[0092] The TFT substrate precursor is etched using the copper-molybdenum metal film etching solution of Example 5, and the etching conditions are the same as those of Example 1, to obtain the etched sample S5.

[0093] Example 6

[0094] A copper-molybdenum metal film etching solution comprises the following components in percentage by mass:

[0095] Hydrogen peroxide: 20%; hydrochloric acid: 5%; sulfuric acid: 5%; water: 68.7%; ethylenediaminetetrapropionic acid: 0.8%; potassium chromate: 0.2%; o-phenanthroline: 0.2%; 8-hydroxyquinoline: 0.05%; triethanolamine: 0.05%.

[0096] The TFT substrate precursor is etched using the copper-molybdenum metal film etching solution of Example 5, and the etching conditions are the same as those of Example 1 to obtain the etched sample S6.

[0097] Example 7

[0098] A copper-molybdenum metal film etching solution comprises the following components in percentage by mass:

[0099] Hydrogen peroxide: 20%; hydrochloric acid: 5%; sulfuric acid: 3%; water: 65.7%; ethylenediaminetetrapropionic acid: 0.8%; potassium chromate: 0.2%; o-phenanthroline: 0.2%; 8-hydroxyquinoline: 0.1%; tartaric acid: 5%.

[0100] The TFT substrate precursor is etched using the copper-molybdenum metal film etching solution of Example 7, and the etching conditions are the same as those of Example 1 to obtain the etched sample S7.

[0101] Example 8

[0102] A copper-molybdenum metal film etching solution comprises the following components in percentage by mass:

[0103] Hydrogen peroxide: 20%; nitric acid: 0.1%; sulfuric acid: 1.9%; hydrochloric acid: 5%; water: 65.7%; ethylenediaminetetrapropionic acid: 0.8%; potassium chromate: 0.2%; o-phenanthroline: 0.2%; 8-hydroxyquinoline: 0.1%; tartaric acid: 5%.

[0104] The TFT substrate precursor is etched using the copper-molybdenum metal film etching solution of Example 8, and the etching conditions are the same as those of Example 1 to obtain the etched sample S8.

[0105] Comparative Example 1

[0106] An etching solution comprises the following components in percentage by weight:

[0107] Hydrogen peroxide: 20%; sulfuric acid: 10%; water: 69%; EDTA: 1%.

[0108] The TFT substrate precursor was etched using the etching solution of Comparative Example 1 under the same etching conditions as those of Example 1, to obtain an etched sample D1.

[0109] Comparative Example 2

[0110] An etching solution comprises the following components in percentage by weight:

[0111] Hydrogen peroxide: 20%; Sulfuric acid: 10%; Water: 69%; Potassium chromate: 1%.

[0112] The TFT substrate precursor was etched using the etching solution of Comparative Example 2 under the same etching conditions as those of Example 1, to obtain an etched sample D2.

[0113] Comparative Example 3

[0114] An etching solution comprises the following components in percentage by weight:

[0115] Hydrogen peroxide: 20%; sulfuric acid: 10%; water: 69.9%; ethylenediaminetetrapropionic acid: 0.1%; potassium chromate: 0.1%.

[0116] The TFT substrate precursor was etched using the etching solution of Comparative Example 3 under the same etching conditions as in Example 1, to obtain an etched sample D3.

[0117] Effect Example

[0118] In order to verify the properties and effects of the copper-molybdenum metal film etching solution of the present application, the present application also provides an effect embodiment.

[0119] The samples prepared in the above embodiments and comparative examples were placed under a scanning electron microscope to characterize the residual copper-molybdenum metal film on the substrate surface. Figure 3 , Figure 3 The electron microscope characterization image of the sample after etching provided in Example 7 of the present application is Figure 3 It can be seen that when the copper-molybdenum metal film etching solution of Example 1 is used for etching, there is basically no molybdenum residue on the surface of the substrate in the obtained sample, the critical dimension loss of the copper-molybdenum metal film is 0.3539μm, and the etching angle of the copper-molybdenum metal film is 48°, wherein the critical dimension loss of the copper-molybdenum metal film is equal to half of the difference between the lengths of line segment 1 and line segment 3, and the etching angle is equal to the average of angle 4 and angle 5. Figure 4 , Figure 4 This is an electron microscope characterization image of the sample after etching provided in Comparative Example 1 of the present application, wherein: Figure 4 (a) is a morphology characterization diagram of the left side of the sample after etching in Comparative Example 1. Figure 4 (b) is a morphology characterization diagram of the right side of the sample after etching in Comparative Example 1. Figure 4 It can be seen that when the etching solution of Comparative Example 1 is used for etching, there is still molybdenum residue in the substrate of the sample obtained after etching, such as the circled area in the characterization figure, there are a lot of granular molybdenum residues on the surface of the substrate, and the structure of the copper-molybdenum metal film after etching is not uniform, the surface of the metal film is very rough, the critical dimension loss of the copper-molybdenum metal film is 0.281μm, and the etching angle of the copper-molybdenum metal film is 41°. The samples of other embodiments and comparative examples are characterized, and the characterization results are shown in Table 1.

[0120] Table 1 Test results of samples etched from Examples 1-8 and Comparative Examples 1-3

[0121]

[0122]

[0123] It can be seen from Table 1 that the copper-molybdenum metal film etching solution of the present application has a good etching effect on the copper-molybdenum metal film, there is no molybdenum residue after etching, the etching angle is within a reasonable range, the key dimension loss is less than 0.9μm, and high-precision etching can be achieved.

[0124] The above is a preferred embodiment of the present application, but it should not be understood as limiting the scope of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.

Claims

1. A copper-molybdenum metal film etching solution, characterized in that: Includes the following components in percentage by mass: Hydrogen peroxide: 10% to 30%; Inorganic acid: 5% to 20%; Etching regulator: 0.5% to 2%; Water: 60%-80%; The etching conditioner includes ethylenediaminetetrapropionic acid and potassium chromate, and the mass ratio of the ethylenediaminetetrapropionic acid to the potassium chromate is 1:(0.1-5); the etching conditioner also includes o-phenanthroline, and the mass ratio of the ethylenediaminetetrapropionic acid to the o-phenanthroline is 1:(0.1-2); The inorganic acid includes one or more of nitric acid, sulfuric acid and hydrochloric acid, and the ratio of the mass of nitrate ions in the copper-molybdenum metal film etching solution to the sum of the masses of the ethylenediaminetetrapropionic acid and the 1,1-diphenylamine is less than or equal to 0.

01.

2. The copper-molybdenum metal film etching solution according to claim 1, characterized in that: The copper-molybdenum metal film etching solution also includes a hydrogen peroxide stabilizer with a mass percentage of 0.05%-0.5%, and the hydrogen peroxide stabilizer includes one or more of triethanolamine, triethylenetetramine, diphenylaminourea and 8-hydroxyquinoline.

3. The copper-molybdenum metal film etching solution according to claim 1 or 2, characterized in that: The copper-molybdenum metal film etching solution also includes an organic acid with a mass percentage of 5% to 18%, and the organic acid includes one or more of oxalic acid, tartaric acid, citric acid and sulfosalicylic acid.

4. A method for applying a copper-molybdenum metal film etching solution, characterized in that: The following steps are involved: The copper-molybdenum metal film etching solution as described in any one of claims 1 to 3 is brought into contact with a substrate having a copper-molybdenum metal film on its surface to etch the copper-molybdenum metal film.

5. A display panel, characterized in that: The display panel includes a metal layer, and the metal layer is made by the application method of the copper-molybdenum metal film etching solution as described in claim 4.