A large-size silicon carbide single crystal growth device and a silicon carbide single crystal preparation method

Through the combined resistance heating structure and the temperature field adjustment controlled by the pull rod, the problem of insufficient temperature gradient in the traditional silicon carbide single crystal growth device is solved, and the growth of large-size and high-quality silicon carbide single crystal is achieved, ensuring the powder Efficient utilization and inhibition of crystal defects.

CN114411254BActive Publication Date: 2024-11-12XIANSHU (XIAMEN) TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111543071.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-16
Publication Date
2024-11-12
Estimated Expiration
2041-12-16

AI Technical Summary

Technical Problem

In traditional silicon carbide single crystal growth devices, a single axial temperature gradient is not conducive to the efficient use of powder, making it difficult to prepare large-size and high-quality single crystals. The highest temperature zone in the growth crucible is usually located at the bottom of the powder, affecting the powder. The mass transfer process is prone to produce amorphous or polycrystalline SiC particles.

Method used

Using a combined resistive heating structure, including the main heater and the auxiliary heater, the position of the growth crucible and the power of the heater are controlled by lifting rods, and the precise control of the temperature field in the crucible is achieved, ensuring the highest temperature point near the powder surface and avoiding The bottom of the powder is overheated, improving the mass transfer efficiency of the powder and the quality of the single crystal.

Benefits of technology

Achieve high-quality growth of large-size silicon carbide single crystals. By precisely controlling the temperature field, crystal defects are reduced, powder utilization efficiency is improved, and the thickness and size of single crystals are ensured. For example, it can be prepared ≥6 inches and ≥2cm. Thick silicon carbide single crystal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114411254B_ABST
    Figure CN114411254B_ABST
Patent Text Reader

Abstract

The present invention discloses a large-size silicon carbide single crystal growth device and a preparation method thereof. By utilizing the cooperation of a main heater and an auxiliary heater and moving the position of a crucible up and down, localized adjustment of the temperature field in the growth crucible can be achieved, and the position of the highest temperature zone inside the crucible raw material can be accurately controlled to always be close to the surface area of ​​the powder material, thereby avoiding graphitization of the raw material surface and damage to the single crystal growth quality caused by raw material carbon or silicon carbide amorphous particles due to excessively high internal temperature of the powder material and excessively low surface temperature during the growth process, thereby obtaining large-size, high-quality silicon carbide single crystals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor material growth, and in particular to a large-size silicon carbide single crystal growth device and a silicon carbide single crystal preparation method. Background Art

[0002] Silicon carbide is a third-generation semiconductor material with properties such as wide bandgap, high thermal conductivity, high electron saturation mobility and high breakdown electric field. It has significant advantages over first-generation semiconductor materials such as silicon and second-generation semiconductor materials such as gallium arsenide. At the same time, silicon carbide, as a third-generation semiconductor high-power power electronic device, is currently one of the fastest-growing power semiconductor devices in the field of power electronics. As a typical representative of the third-generation semiconductor materials, silicon carbide is one of the wide-bandgap semiconductor materials with the most mature crystal production technology and device manufacturing level and the most widely used. It is an extremely ideal semiconductor material for high-temperature, high-frequency, radiation-resistant and high-power applications. Therefore, it is very important to prepare large-size, high-quality silicon carbide single crystals.

[0003] At present, the main methods for growing silicon carbide single crystals include physical vapor transport (PVT), chemical vapor deposition (CVD) and liquid phase epitaxy (LPE). Among them, the PVT method is the most mature method and the most widely used method for growing silicon carbide single crystals commercially. The growth device for growing silicon carbide single crystals by the PVT method generally adopts medium-frequency induction heating. The growth crucible is coaxially placed with the coil. When the coil is loaded with medium-frequency alternating current, the growth crucible is induced to heat, and then the powder is heated by heat conduction. The powder in the high-temperature zone sublimates the atmosphere, and the gas phase components rise to the seed crystal in the low-temperature zone under the temperature gradient to crystallize and grow.

[0004] However, the traditional single axial temperature trend from low to high from the single crystal growth surface to the powder area has disadvantages in growing large-size, high-quality single crystals: on the one hand, the highest temperature zone in the crucible is usually located at the bottom of the crucible powder, which is not conducive to the mass transfer process of the powder. The reaction precursors such as SiC2 and Si2C at the bottom are not easily effectively transferred to the seed crystal growth surface, and the lower temperature on the powder surface easily leads to more amorphous or polycrystalline SiC, or C particles being transported to the growth surface, resulting in the generation of crystal defects; on the other hand, the single axial temperature gradient field is not conducive to the efficient utilization of the powder grade, which makes it difficult to prepare a thicker single crystal layer. Summary of the invention

[0005] In order to solve the above-mentioned technical problems of large-size silicon carbide single crystal growth, the present invention proposes a large-size silicon carbide single crystal growth device and a single crystal preparation method. The proposed device can accurately control the temperature field inside the growth crucible and adjust the position of the high-temperature zone of the powder inside the powder to achieve the purpose of improving the powder consumption process and inhibiting growth defects. The combined resistance heating structure used can also ensure the extremely small radial temperature difference and specific axial gradient temperature required for large-size single crystals.

[0006] To achieve the above-mentioned objectives, the first aspect of the present invention provides a large-size silicon carbide single crystal growth device, comprising a growth crucible, an insulation layer, a main heater and an auxiliary heater arranged in a PVT growth chamber; the lower part of the growth crucible is used to fill powder, and the upper part is used to install seed crystals; the insulation layer is wrapped around the outer periphery of the growth crucible and temperature measuring holes are opened corresponding to the top and bottom of the growth crucible; the main heater and the auxiliary heater are arranged between the growth crucible and the insulation layer; the main heater and the auxiliary heater are both cylindrical resistance heaters, and the main heater is located below the auxiliary heater, wherein the main heater corresponds to the powder area, and the auxiliary heater corresponds to the seed crystal area; a lifting rod is connected to the top of the growth crucible, and the lifting rod is used to control the up and down movement of the growth crucible so that the highest temperature point in the growth crucible during the growth process is located 2 to 10 cm below the powder surface.

[0007] Furthermore, it also includes furnace walls, vacuum systems, water cooling devices and other components required to assist in constructing the PVT growth chamber.

[0008] Optionally, the height of the main heater and the auxiliary heater is 5 to 15 cm; the material of the main heater and the auxiliary heater is graphite, tungsten, molybdenum or tantalum, and the thickness of the tube wall is 2 to 20 mm; the main heater and the auxiliary heater are respectively coaxially arranged with the crucible. The cylindrical main and auxiliary heaters are placed up and down, located between the growth crucible and the insulation layer, and are isolated by a vacuum or atmosphere gas layer in the middle. The main heater is located in the lower area of ​​the crucible close to the crucible powder position. The main function of the main heater is to use its lower height to achieve the height localization of the heating area along the axial direction of the crucible, so that the highest temperature point in the crucible is always close to the surface area of ​​the powder, avoiding the highest temperature point obtained by conventional growth equipment or heating devices close to the inside or bottom of the powder, which is not conducive to the efficient use of the powder gradient and the controllable mass transfer process; the auxiliary heater is located in the upper area of ​​the crucible close to the crucible cover seed crystal position, and its height is consistent with the requirements of the main heater. The main function of the auxiliary heater is to assist in maintaining a small radial temperature difference in the seed crystal area and the required growth temperature.

[0009] Optionally, the diameter of the temperature measuring hole is 5 to 20 mm, which is convenient for collecting the temperature of the top and bottom of the growth crucible.

[0010] To achieve the above-mentioned purpose, the second aspect of the present invention also provides a method for preparing a single crystal using the large-size silicon carbide single crystal growth device as described above, comprising the following steps: loading silicon carbide powder into the lower part of a growth crucible, installing a silicon carbide seed crystal at the top of the crucible, independently controlling a main heater and an auxiliary heater to heat the growth crucible, and when the growth crucible is heated to the silicon carbide growth temperature, collecting temperature data at the top and bottom of the growth crucible through a temperature measuring hole; controlling the position of the growth crucible relative to the main heater by a lifting rod and / or controlling the power of the main heater and the auxiliary heater to adjust the temperature gradient inside the growth crucible, so that the highest temperature point in the growth crucible is always located 2 to 10 cm below the surface of the powder, the silicon carbide powder is heated and sublimated to form a gas phase component, and the gas phase component rises to the surface of the seed crystal and crystallizes under the drive of the temperature gradient to grow a silicon carbide single crystal.

[0011] By using the localized area heating of the main heater in combination with the auxiliary heater and the lifting of the crucible, the powder in the crucible can be consumed during the growth process, and the highest temperature point can always be kept close to the surface area of ​​the powder.

[0012] Furthermore, the filling height of the powder is greater than the height of the main heater, and its smaller height is utilized to realize highly localized heating area along the axial direction of the crucible, that is, the highest temperature point of the powder zone of the crucible can be adjusted to a certain extent by moving the crucible up and down.

[0013] Furthermore, the crucible thermal field during the growth process is characterized by a peak-shaped temperature distribution along the axial direction of the crucible, that is, the temperature of the crystal growth surface area is relatively low, with a temperature range of 1950 to 2350°C, the temperature of the area below the powder surface is the highest, with a typical range of 2000 to 2400°C, and the temperature near the bottom of the powder is slightly lower. When the powder is exhausted, the highest temperature point may be the surface of the powder.

[0014] Furthermore, the large-sized silicon carbide single crystal that can be prepared has a size of ≥6 inches and a thickness of ≥2 cm.

[0015] The beneficial effects of the present invention are:

[0016] The present invention compares the temperature difference between the top and bottom of the growth crucible with the silicon carbide growth temperature, adopts a resistive main heater and an auxiliary heater to heat the growth crucible, and simultaneously combines a lifting rod to control the position of the growth crucible relative to the heater to adjust the crucible thermal field. The advantages of the present invention are uniform heating, reduced temperature gradient on the surface of the seed crystal, and precise control of the temperature field. In particular, the position of the high-temperature zone of the powder can be precisely adjusted in the longitudinal direction of the entire powder filling area, which is beneficial to the efficient use of the powder and the suppression of single crystal growth defects, thereby obtaining large-sized, high-quality silicon carbide single crystals. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a cross-sectional view of a large-size silicon carbide single crystal growth device in one embodiment of the present invention;

[0018] Figure 2 Schematic diagram of the comparison between the axis gradient temperature distribution characteristics (2-B) of a large-size silicon carbide single crystal growth device in one embodiment of the present invention and the axis gradient temperature characteristics (2-A) obtained by a conventional structure;

[0019] Figure 3 Schematic diagram of the location of the high temperature zone inside the raw material under three conditions in one embodiment of the present invention. DETAILED DESCRIPTION

[0020] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments.

[0021] like Figure 1 As shown, a large-size silicon carbide single crystal growth device 10 includes a growth crucible 3, an insulation layer 2, a main heater 6 and an auxiliary heater 7 arranged in a PVT growth chamber. As is known, the PVT growth chamber is constructed by a furnace wall, a vacuum system, a water cooling device, etc. The lower part of the growth crucible 3 is used to load silicon carbide raw material powder 5, and the upper part is used to install silicon carbide seed crystals 4. The insulation layer 2 is made of thermal insulation material, wrapped around the outer periphery of the growth crucible 3 and provided with temperature measuring holes 21 corresponding to the top and bottom of the growth crucible 3. The main heater 6 and the auxiliary heater 7 are arranged between the growth crucible 3 and the insulation layer 2, and are isolated by a vacuum or atmosphere gas layer in the middle; the main heater 6 and the auxiliary heater 7 are both cylindrical resistance heaters, and the main heater 6 is located below the auxiliary heater 7, wherein the main heater 6 corresponds to the powder 5 area, and the auxiliary heater 7 corresponds to the seed crystal 4 area. A lifting rod 1 is connected to the top of the growth crucible 3, and the lifting rod 1 is used to control the growth crucible 3 to move up and down so that the highest temperature point in the growth crucible 3 is located 2 to 10 cm below the surface of the powder 5 during the growth process.

[0022] In this embodiment, the growth crucible 3 is coaxially arranged with the main heater 6 and the auxiliary heater 7, and all three are cylindrical, wherein the main heater 6 is the main heating source, the auxiliary heater 7 has a relatively small power and can be turned off, and the insulation layer 2 has 5-10 mm temperature measuring holes 21 at both ends, which is convenient for collecting the top and bottom temperature data of the growth crucible 3, and is also conducive to the construction of the temperature field. When measuring the temperature, an infrared thermometer can be aligned with the temperature measuring hole, and the internal infrared radiation can be used to determine the internal temperature. As such, the temperature field distribution inside the growth crucible 3 during heating is characterized by a higher temperature at the bottom and a lower temperature at the top, and the overall temperature field distribution is uniform and stable. The heating method of the resistance heater includes but is not limited to constant voltage DC heating.

[0023] The height of the main heater 6 and the auxiliary heater 7 is 5 to 15 cm. The material of the main heater 6 and the auxiliary heater 7 is graphite, tungsten, molybdenum or tantalum, and the thickness of the tube wall is 2 to 20 mm. The main function of the main heater is to use its small height to realize the high localization of the heating area along the axial direction of the crucible, that is, the highest temperature point of the crucible powder area can be adjusted to a certain extent by moving the crucible up and down. The typical application feature when preparing single crystals is to make its highest temperature point always close to the surface area of ​​the powder, avoiding the highest temperature point obtained by conventional growth equipment or heating devices close to the inside or bottom of the powder, which leads to the drawback that the efficient use of the powder and the controllable mass transfer process cannot be achieved. The main heater 6 mainly heats, and the auxiliary heater 7 assists in heating, so as to achieve a uniform temperature field inside the growth crucible 3, reduce the temperature gradient on the growth surface of the seed crystal 4, independently control the heating power of the main and auxiliary heating, realize the precise adjustment of the axial temperature, obtain the ideal crystal interface, and prepare large-sized, high-quality silicon carbide single crystals.

[0024] Compared with the traditional single gradient change of axial temperature, such as Figure 2 -A, the growth device of the present invention can be used to adjust (move) the highest temperature point of the powder area in the crucible, as shown in FIG. Figure 2 -B indicates.

[0025] The method for preparing a silicon carbide single crystal using the large-size silicon carbide single crystal growth device as described above comprises the following steps:

[0026] The silicon carbide powder is loaded into the bottom of the growth crucible, and the silicon carbide seed crystal is installed on the top of the crucible cover; wherein the powder loading height is greater than the height of the main heater;

[0027] Control the main heater and the auxiliary heater to heat the growth crucible. When the growth crucible is heated to the silicon carbide growth temperature, collect the temperature data of the top and bottom of the growth crucible. Adjust the position of the growth crucible relative to the heater by controlling the lifting rod connected to the top of the growth crucible, or independently control the heating power of the main heater and the auxiliary heater at the same time to adjust the temperature gradient inside the growth crucible and the position of the high temperature zone of the powder;

[0028] The silicon carbide powder is heated and sublimated into gas phase components, and the gas phase components rise to the surface of the silicon carbide seed crystal driven by the temperature gradient to crystallize, thereby growing the silicon carbide single crystal.

[0029] By localized area heating of the main heater, combined with the auxiliary heater and the pulling of the crucible, the powder in the crucible can be consumed during the growth process, and the highest temperature point is always kept close to the surface area of ​​the powder. However, the highest point is not on the surface of the powder, and is typically located 2 to 10 cm below the surface of the powder.

[0030] The characteristic of the crucible thermal field during the growth process is that the temperature distribution along the axial direction of the crucible is in the shape of a peak, that is, the temperature in the crystal growth surface area is relatively low, with a temperature range of 1950-2350°C, the temperature in the area below the powder surface is the highest, with a typical range of 2000-2400°C, and the temperature near the bottom of the powder is slightly lower. When the powder is exhausted, the highest temperature point may be the powder surface.

[0031] The temperature data collected from the top and bottom of the growth crucible are compared with the expected temperature field inside the growth crucible, and the relative position of the growth crucible is moved and / or the heating power of the main heater and the auxiliary heater is controlled according to the comparison results. For example, if the temperature at the bottom of the growth crucible is too high and the heating time is too long, the powder at the bottom of the growth crucible will be severely graphitized. By slowly moving the position of the growth crucible upward or adjusting the power of the main heater downward, the position of the high temperature area of ​​the powder can be adjusted to shift upward to achieve the expected temperature field inside the growth crucible; vice versa.

[0032] In order to verify the effect of adjusting the position of the high temperature zone of the powder inside the growth crucible in the embodiment of the present invention, the present invention respectively statistically analyzes the cross-sectional temperature of the high temperature zone of the powder at different positions of the growth crucible relative to the heater under the following three conditions. The temperature inside the growth crucible is higher as the color becomes darker. Specifically, Figure 3 As shown in A, B, and C.

[0033] in, Figure 3 A, B, and C in the figure are for the following three situations respectively:

[0034] A. In the large-scale silicon carbide single crystal growth device of this embodiment, the height position of the surface of the silicon carbide powder inside the growth crucible is above the height position of the top of the main heater, and the cross-sectional view of the high-temperature area of ​​the silicon carbide powder in the growth crucible formed by high-power heating of the main heater;

[0035] B. The large-size silicon carbide single crystal growth device in this embodiment controls the lifting rod to move the growth crucible so that the height position of the silicon carbide powder surface is flush with the height position of the top of the main heater. The cross-sectional view of the high-temperature area of ​​the silicon carbide powder in the growth crucible formed by high-power heating of the main heater;

[0036] C. The large-size silicon carbide single crystal growth device in this embodiment controls the lifting rod to move the growth crucible so that the surface height of the silicon carbide powder is below the top height of the main heater. The cross-sectional view of the high-temperature zone of the silicon carbide powder in the growth crucible formed by high-power heating of the main heater.

[0037] contrast Figure 3From the position of the high-temperature zone of the silicon carbide powder, it can be seen that the high-temperature area of ​​the powder has an obvious offset. The high-temperature zone of the powder in A is concentrated at the bottom corner of the growth crucible, the high-temperature zone of the powder in B moves upward and is located at the center of the powder, and the high-temperature zone of the powder in C moves upward and is located at a higher position above the center. This shows that the effect of adjusting the position of the high-temperature zone of the powder inside the growth crucible in this embodiment is obvious, so that the temperature field change can be accurately controlled, thereby preparing large-size, high-quality silicon carbide single crystals.

[0038] The above embodiments are only used to further illustrate a large-size silicon carbide single crystal growth device and a silicon carbide single crystal preparation method of the present invention, but the present invention is not limited to the embodiments. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention fall within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a large-size silicon carbide single crystal, characterized in that: The large-sized silicon carbide single crystal has a size of ≥6 inches and a thickness of ≥2 cm; The preparation method adopts a large-size silicon carbide single crystal growth device, which includes a growth crucible, an insulation layer, a main heater and an auxiliary heater arranged in a PVT growth chamber; the lower part of the growth crucible is used to fill powder, and the upper part is used to install seed crystals; the insulation layer is wrapped around the outer periphery of the growth crucible and temperature measuring holes are opened corresponding to the top and bottom of the growth crucible; the main heater and the auxiliary heater are arranged between the growth crucible and the insulation layer; the main heater and the auxiliary heater are both cylindrical resistance heaters, and the main heater is located below the auxiliary heater, wherein the main heater corresponds to the powder area, and the auxiliary heater corresponds to the seed crystal area; a lifting rod is connected to the top of the growth crucible, and the lifting rod is used to control the growth crucible to move up and down; The preparation method comprises the following steps: loading silicon carbide powder into the lower part of a growth crucible, installing a silicon carbide seed crystal at the top of the crucible, independently controlling a main heater and an auxiliary heater to heat the growth crucible, and collecting temperature data of the top and bottom of the growth crucible through a temperature measuring hole when the growth crucible is heated to a silicon carbide growth temperature; controlling the position of the growth crucible relative to the main heater and / or controlling the power of the main heater and the auxiliary heater through a lifting rod to adjust the temperature gradient inside the growth crucible, so that the highest temperature point in the growth crucible is always located at a position 2 to 10 cm below the surface of the powder; heating and sublimating the silicon carbide powder to form a gas phase component, and the gas phase component rises to the surface of the seed crystal to crystallize under the drive of the temperature gradient, thereby growing a silicon carbide single crystal.

2. The method for preparing a large-size silicon carbide single crystal according to claim 1, characterized in that: The height of the main heater and the auxiliary heater is 5-15 cm.

3. The method for preparing a large-size silicon carbide single crystal according to claim 1, characterized in that: The main heater and the auxiliary heater are made of graphite, tungsten, molybdenum or tantalum, and the thickness of the cylinder wall is 2-20 mm.

4. The method for preparing a large-size silicon carbide single crystal according to claim 1, characterized in that: The diameter of the temperature measuring hole is 5-20 mm.

5. The method for preparing a large-size silicon carbide single crystal according to claim 1, characterized in that: The main heater and the auxiliary heater are respectively arranged coaxially with the crucible.

6. The method for preparing a large-size silicon carbide single crystal according to claim 1, characterized in that: The filling height of the powder is greater than the height of the main heater.

7. The method for preparing a large-size silicon carbide single crystal according to claim 1, characterized in that: The temperature distribution in the growth crucible along the axial direction is in a peak shape.

8. The method for preparing a large-size silicon carbide single crystal according to claim 7, characterized in that: The temperature of the crystal growth surface area of ​​the seed crystal is 1950-2350°C, and the temperature of the highest temperature point area of ​​the powder is 2000-2400°C.