A back film structure for improving the back efficiency of bifacial PERC and its preparation method and application

By depositing aluminum oxide, silicon nitride and silicon oxynitride films on the back of the P-type double-sided PERC solar cell, ensuring that their refractive index product and optical path are equal, the problems of complex structure and low efficiency of the back film in the prior art are solved, and the problem of the structure of the back film in the prior art is realized. The back efficiency is significantly improved and the front efficiency is improved.

CN114420766BActive Publication Date: 2024-11-26CSI CELLS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011079435.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-10
Publication Date
2024-11-26
Estimated Expiration
2040-10-10

AI Technical Summary

Technical Problem

In the prior art, the back film that improves the back efficiency of P-type double-sided PERC solar cells has a complex structure, and the preparation process is difficult to simplify, which affects production efficiency and battery performance.

Method used

Alumina film is used as the basis, and silicon nitride film and silicon nitride film are deposited thereon respectively to ensure that the refractive index of the silicon nitride film and the refractive index product of the silicon nitride film is equal to the refractive index of silicon, and the optical path is equal. To minimize the reflection of sunlight on the back and improve the efficiency of the battery back.

Benefits of technology

By optimizing the back film structure and coating process, the back conversion efficiency of P-type double-sided PERC batteries is improved, the double-sided rate is increased by 2-3%, and the front conversion efficiency is improved, enhancing the competitiveness of the enterprise.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114420766B_ABST
    Figure CN114420766B_ABST
Patent Text Reader

Abstract

The present invention provides a back film structure for improving the efficiency of the back side of a bifacial PERC cell, and a preparation method and application thereof, wherein the back film structure comprises an aluminum oxide film located on the back side of a cell, a silicon nitride film is arranged on the aluminum oxide film, and a silicon oxynitride film is arranged on the silicon nitride film; wherein the product of the refractive index of the silicon nitride film and the refractive index of the silicon oxynitride film is equal to the refractive index of silicon, and the optical path of the silicon nitride film is equal to the optical path of the silicon oxynitride film. The back film structure of the present invention can improve the back side efficiency of a bifacial cell, improve the opening voltage and FF of the cell, improve the front conversion efficiency, and improve the benefits and competitiveness of the enterprise.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solar cells and relates to a back film structure for improving the back efficiency of a double-sided PERC and a preparation method and application thereof. Background Art

[0002] In recent years, with the continuous advancement of solar cell production technology, the main research hotspots are HIT cells, WMT cells, N-type bifacial cells, P-type PERC cells, etc. Among them, P-type PERC cells have become the mainstream battery technology in the market due to their relatively mature technology and low difficulty in mass production. At present, the bifacial rate of bifacial modules prepared by bifacial PERC solar cells is 65-75%, and there is a lot of room for improving the back efficiency. Therefore, improving the back film structure and optimizing the coating process, reducing the reflectivity of the back of the cell, increasing the absorption of light, improving the back conversion efficiency of P-type bifacial PERC cells, and improving the bifacial rate of P-type bifacial PERC cells are the current focus of the industry.

[0003] CN110957378A discloses a back film structure for improving the bifaciality of a P-type bifacial cell, including a cell, an aluminum oxide film, a silicon nitride film, a silicon oxynitride film, and a silicon oxide film are sequentially deposited on the back of the cell, and the silicon nitride film includes an upper silicon nitride film, a middle silicon nitride film, and a lower silicon nitride film. The thickness of the upper, middle, and lower three silicon nitride films gradually increases, and the refractive index gradually decreases. The total film thickness of the silicon nitride film is 35 to 55 nanometers, and the total refractive index of the silicon nitride film is 2.12 to 2.20. By improving the back film structure and optimizing the coating process, the reflectivity of the back of the cell is effectively reduced, the absorption of light is increased, and the back conversion efficiency of the P-type bifacial SE PERC cell is improved. The bifaciality of the P-type bifacial SE PERC cell is increased from 72.9% to 74.14%. However, the invention needs to include three layers of silicon nitride films that meet the specific conditions as described above, which increases the complexity of the preparation process.

[0004] Therefore, in the art, it is expected to develop a simpler and more efficient back film structure that can improve the bifaciality of bifacial PERC. Summary of the invention

[0005] In view of the deficiencies of the prior art, an object of the present invention is to provide a back film structure for improving the back efficiency of a bifacial PERC cell, and a preparation method and application thereof.

[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0007] On the one hand, the present invention provides a back film structure for improving the back efficiency of a double-sided PERC, the back film structure comprising an aluminum oxide film located on the back of a cell, a silicon nitride film disposed on the aluminum oxide film, and a silicon oxynitride film disposed on the silicon nitride film; wherein the product of the refractive index of the silicon nitride film and the refractive index of the silicon oxynitride film is equal to the refractive index of silicon, and the optical path of the silicon nitride film is equal to the optical path of the silicon oxynitride film.

[0008] In the back film structure of the present invention, the product of the refractive index of the silicon nitride film and the refractive index of the silicon oxynitride film is equal to the refractive index of silicon, and the optical path of the silicon nitride film is equal to the optical path of the silicon oxynitride film, which can minimize the reflection of sunlight on the back side, thereby greatly improving the back side efficiency of the bifacial cell; at the same time, the unique back side film layer structure has a better hydrogen passivation effect, and can also improve the opening voltage and FF of the cell, thereby achieving an improvement in the front side conversion efficiency.

[0009] In the present invention, if the product of the refractive index of the silicon nitride film and the refractive index of the silicon oxynitride film is not equal to the refractive index of silicon, the anti-reflection effect is poor; if the optical path of the silicon nitride film and the optical path of the silicon oxynitride film are not equal, the anti-reflection effect is poor.

[0010] In the present invention, the refractive index of silicon is 3.9.

[0011] Preferably, the optical path length of the silicon nitride film and the silicon oxynitride film is 60 to 180 nm, for example, 60 nm, 80 nm, 100 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 175 nm, 180 nm, etc.

[0012] Preferably, the thickness of the aluminum oxide film is 5 to 15 nm (e.g., 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm or 15 nm), and the refractive index is 1.5 to 1.7 (e.g., 1.55, 1.60, 1.63, 1.68). In the present invention, if the thickness of the aluminum oxide film is less than 5 nm, the silicon surface recombination rate will increase, affecting its passivation effect; if the thickness of the aluminum oxide film is greater than 15 nm, the process time will be long, affecting the production capacity.

[0013] Preferably, the aluminum oxide film has a thickness of 8 to 10 nm and a refractive index of 1.5.

[0014] Preferably, the thickness of the silicon nitride film is 20 to 90 nm (e.g., 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 70 nm, 80 nm or 90 nm), and the refractive index is 2.0 to 2.6 (e.g., 2.0, 2.1, 2.2, 2.3, 2.4, 2.6). In the present invention, if the thickness of the silicon nitride film is less than 20 nm, the absorption of medium and long wave light is less, and the reflectivity will increase; if the thickness of the silicon nitride film is greater than 90 nm, the absorption of short wave light is less, and the reflectivity will also increase; if the refractive index of the silicon nitride film is less than 2.0, the passivation effect will deteriorate and the battery efficiency will decrease; if the refractive index of the silicon nitride film is greater than 2.6, the extinction coefficient will be very large, which will reduce the effective absorption of light by silicon, reduce the back current, and ultimately reduce the back efficiency.

[0015] Preferably, the silicon nitride film has a thickness of 40 to 70 nm and a refractive index of 2.25 to 2.5.

[0016] Preferably, the thickness of the silicon oxynitride film is 30 to 120 nm (e.g., 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 120 nm), and the refractive index is 1.5 to 1.95 (e.g., 1.5, 1.55, 1.6, 1.7, 1.8, 1.9, 1.95). In the present invention, if the thickness of the silicon oxynitride film is less than 30 nm, the absorption of medium and long wave light is less, and the reflectivity will increase; if the thickness of the silicon oxynitride film is greater than 120 nm, the absorption of short wave light is less, and the reflectivity will also increase; if the refractive index of the silicon oxynitride film is less than 1.5, the effective H content will be low, affecting the passivation effect and reducing the efficiency of the front and back cells; if the refractive index of the silicon oxynitride film is greater than 1.95, it is difficult to complete the existing preparation process.

[0017] Preferably, the silicon oxynitride film has a thickness of 68 to 80 nm and a refractive index of 1.56 to 1.73.

[0018] Preferably, the reflectivity curve of the back film structure has two troughs in the wavelength range of 300nm to 1200nm, one of which is between short waves 330 and 500nm, and the other is between medium and long waves 650 and 1000nm.

[0019] Preferably, in the reflectivity curve of the back film structure in the wavelength range of 300nm to 1200nm, the wavelength corresponding to the trough of short wave is 360 to 440nm, and the wavelength corresponding to the trough of medium and long wave is 850 to 950nm.

[0020] On the other hand, the present invention provides a method for preparing a back film structure for improving the back efficiency of a bifacial PERC as described above, the preparation method comprising the following steps:

[0021] A. Place the cell with the back side facing upward into the graphite plate, then place the graphite plate into the ALD plate chamber, and coat the back side of the cell to obtain an aluminum oxide film;

[0022] B. Place the battery cell obtained in step A with the back side facing upward into a graphite boat, then place the graphite boat into a tubular PECVD, introduce a certain proportion of ammonia and silane gas, set the coating time and other coating conditions, and coat the aluminum oxide film to prepare a silicon nitride film;

[0023] C. introducing laughing gas, ammonia and silane gas to coat the silicon nitride film to prepare a silicon oxynitride film, and making the product of the refractive index of the silicon nitride film and the refractive index of the silicon oxynitride film equal to the refractive index of silicon, and the optical path of the silicon nitride film equal to the optical path of the silicon oxynitride film, thereby obtaining the back film structure.

[0024] In step B, the flow ratio of the silane and ammonia introduced is certain, so the refractive index of the plated silicon nitride is known (the inventors have found, based on the accumulated experience of making single-layer films, that under a certain coating process, such as power, pressure, duty cycle, etc., different flow ratios of silane and ammonia correspond to different refractive indices, and the refractive index is obtained by ellipsometer testing); the coating time is certain, and under a certain coating process (such as power, pressure, duty cycle, flow ratio, etc.), the film thickness of the plated silicon nitride can be calculated, that is, the film thickness is equal to the coating rate multiplied by the coating time.

[0025] In step C, according to the silicon nitride coating conditions of step B, the refractive index and corresponding film thickness of silicon nitride are known, and the coated silicon oxynitride film must meet two conditions: one is that the product of the refractive index of the silicon nitride film and the refractive index of the silicon oxynitride film is equal to the refractive index of silicon 3.9, and the other is that the optical path of the silicon nitride film is equal to the optical path of the silicon oxynitride film; through these two conditions, the refractive index and film thickness of the silicon oxynitride film coated in this step are determined. Under a certain coating process (such as power, pressure, duty cycle, etc.), different refractive indices can be obtained by regulating the flow ratio of different laughing gas, silane and ammonia, and different film thicknesses can be obtained by regulating different coating times (refractive index and film thickness can be obtained by ellipsometer testing).

[0026] Preferably, the coating is performed 6-15 times in step A, for example, 6 times, 8 times, 10 times, 12 times, 14 times or 15 times.

[0027] Preferably, the silane in step B is SiH4.

[0028] Preferably, the flow ratio of ammonia and silane introduced in step B is 17:1 to 2:1, for example, 17:1, 12:1, 10:1, 9:1, 8:1, 7:1, 7.5:1, 6:1, 6.5:1, 5:1, 4:1, 3:1 or 2:1.

[0029] Preferably, the coating power in step B is 8 kilowatts and the duty cycle is 1:15.

[0030] Preferably, the coating time in step B is 200-600 s, for example, 200 s, 300 s, 350 s, 380 s, 400 s, 450 s, 500 s, 550 s or 600 s.

[0031] Preferably, the coating temperature in step B is 450-500°C, such as 450°C, 470°C, 490°C or 500°C.

[0032] Preferably, the flow ratio of laughing gas, ammonia and silane introduced in step C is 14:2:1 to 5:0.5:1, for example, 14:2:1, 14:1.8:1, 14:1.2:1, 14:1:1, 14:0.8:1, 12:0.8:1, 13:0.5:1, 8:0.8:1, 7:1.5:1, 6:0.5:1, 5:2:1, 5:1:1, 5:0.5:1, etc.

[0033] Preferably, the coating power in step C is 7 kilowatts and the duty cycle is 1:20.

[0034] Preferably, the coating time in step C is 300-800 s, for example, 300 s, 350 s, 400 s, 500 s, 650 s or 800 s.

[0035] Preferably, the coating temperature in step C is 450-500°C, such as 450°C, 470°C, 490°C or 500°C.

[0036] In the present invention, after growing a layer of AlO film by ALD, silane, ammonia and nitrous oxide are introduced into a tubular PECVD furnace tube in steps and batches, and a certain proportion is controlled, the coating time, coating power and duty cycle are adjusted to form a film layer structure with different refractive index and film thickness. The obtained back film structure not only has the effect of improving the back short-circuit current and the back efficiency, but also has the effect of improving the front opening voltage and FF and the front efficiency.

[0037] The present invention improves the back conversion efficiency of the P-type bifacial PERC battery by improving the back film structure and optimizing the coating process. The bifacial rate of the P-type bifacial PERC battery is increased by 2-3%, and the efficiency of the front side of the battery is increased by about 0.1%, thereby improving the efficiency and competitiveness of the enterprise, and is very worthy of industrial application.

[0038] In another aspect, the present invention provides a bifacial PERC cell, wherein the bifacial PERC cell comprises the back film structure for improving the back efficiency of the bifacial PERC cell as described above.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] In the back film structure of the present invention, the product of the refractive index of the silicon nitride film and the refractive index of the silicon oxynitride film is equal to the refractive index of silicon, and the optical path of the silicon nitride film is equal to the optical path of the silicon oxynitride film, which can minimize the reflection of the back sunlight, thereby greatly improving the back efficiency of the bifacial cell; at the same time, the unique back film layer structure has a better hydrogen passivation effect, and can also improve the opening voltage and FF of the cell, thereby achieving an improvement in the front conversion efficiency. The bifaciality of the P-type bifacial PERC cell is increased by 2-3%, and the efficiency of the front of the cell is increased by about 0.1%, which improves the benefits and competitiveness of the enterprise and is very worthy of industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 Schematic diagram of the back film structure of the present invention, wherein the Si layer represents a P-type solar silicon wafer, 1 is an aluminum oxide (AlO) film, 2 is a silicon nitride (SiN) film, and 3 is a silicon oxynitride (SiON) film.

[0042] Figure 2 3 and 4 are reflectivity curves of the back film structures of Example 1 and Comparative Example 1 in the wavelength range of 300nm to 1200nm.

[0043] Figure 3 Schematic diagram of the structure of the back film structure of comparative example 2, wherein the Si layer represents a P-type solar silicon wafer, 1 is an aluminum oxide (AlO) film, 2 is a silicon nitride (SiN) film, 3 is a silicon oxynitride (SiON) film, and 4 is a silicon oxide (SiO) film. DETAILED DESCRIPTION

[0044] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0045] Example 1

[0046] In this embodiment, a back film structure is provided, such as Figure 1 As shown, the back film structure includes an aluminum oxide (AlO) film located on the back of the cell, a silicon nitride (SiN) film is disposed on the aluminum oxide film, and a silicon oxynitride (SiON) film is disposed on the silicon nitride film.

[0047] The preparation method comprises the following steps:

[0048] A. Place the cell 1 with the back side facing upwards into the graphite plate, then place the graphite plate into the ALD plate chamber, and plate a layer of AlO film 1 on the back side of the cell 1 for 10 times. The thickness of the AlO film 1 is 8-10 nm, and the refractive index is 1.56.

[0049] B. Place the battery cell with the back side facing up into a graphite boat, then place the graphite boat into a tubular PECVD, introduce ammonia and silane at a flow ratio of 5:1, and prepare SiN film 2 on AlO film 1. In this step, 6500sccm of ammonia and 1300sccm of silane are introduced, the coating time is 358s, the temperature is 450-500℃, the coating power is 8 kW, the duty cycle is 1:15, the thickness of SiN film 2 is 49-51nm, the refractive index is 2.25, and the optical path of silicon nitride film is 112nm.

[0050] C. Nitrous oxide, ammonia and silane were introduced at a flow ratio of 6:1.5:1 to prepare a SiON film 3 on a SiN film 2. 4800 sccm of nitric oxide, 1200 sccm of ammonia and 800 sccm of silane were introduced. The coating time was 430 s, the temperature was 450-500° C., the coating power was 7 kW, the duty cycle was 1:20, the thickness of the SiON film 3 was 64-66 nm, the refractive index was 1.73, and the optical path of the silicon oxynitride film was 112 nm.

[0051] The back film structure of this embodiment has an average reflectivity of 9.4%. In its back reflectivity curve, the wavelength of the short-wave trough is 400nm, and the wavelength of the medium- and long-wave trough is 890nm.

[0052] Example 2

[0053] In this embodiment, a back film structure is provided, which includes an aluminum oxide (AlO) film located on the back of the cell, a silicon nitride (SiN) film is provided on the aluminum oxide film, and a silicon oxynitride (SiON) film is provided on the silicon nitride film.

[0054] The preparation method comprises the following steps:

[0055] A. Place the cell 1 with the back side facing upwards into the graphite plate, then place the graphite plate into the ALD plate chamber, and plate a layer of AlO film 1 on the back side of the cell for 13 times. The thickness of the AlO film 1 is 10-12 nm, and the refractive index is 1.60.

[0056] B. Place the battery cell with the back side facing up into a graphite boat, then place the graphite boat into a tubular PECVD, introduce ammonia and silane at a flow ratio of 5:1, and prepare SiN film 2 on AlO film 1. In this step, 6500sccm of ammonia and 1300sccm of silane are introduced, the coating time is 500s, the temperature is 450-500℃, the coating power is 8 kW, the duty cycle is 1:15, the thickness of SiN film 2 is 68-72nm, the refractive index is 2.25, and the optical path of silicon nitride film is 158nm.

[0057] C. Nitrous oxide, ammonia and silane were introduced at a flow ratio of 6:1.5:1 to prepare a SiON film 3 on a SiN film 2. 4800 sccm of nitric oxide, 1200 sccm of ammonia and 800 sccm of silane were introduced. The coating time was 650 s, the temperature was 450-500° C., the coating power was 7 kW, the duty cycle was 1:20, the thickness of the SiON film 3 was 89-93 nm, the refractive index was 1.73, and the optical path of the silicon oxynitride film was 158 nm.

[0058] The back film structure of this embodiment has an average reflectivity of 9.5%. In its back reflectivity curve, the wavelength of the short-wave trough is 450nm, and the wavelength of the medium- and long-wave trough is 940nm.

[0059] Example 3

[0060] In this embodiment, a back film structure is provided, which includes an aluminum oxide (AlO) film located on the back of the cell, a silicon nitride (SiN) film is provided on the aluminum oxide film, and a silicon oxynitride (SiON) film is provided on the silicon nitride film.

[0061] The preparation method comprises the following steps:

[0062] A. Place the battery cell 1 with the back side facing upward into the graphite plate, then place the graphite plate into the ALD plate-type chamber, and coat a layer of AlO film 1 on the back side of the battery for 10 times. The thickness of the AlO film 1 is 8 to 10 nm, and the refractive index is 1.56;

[0063] B. Place the battery cell with the back side facing up into a graphite boat, then place the graphite boat into a tubular PECVD, introduce ammonia and silane at a flow ratio of 2:1, and prepare SiN film 2 on AlO film 1. In this step, 5000sccm of ammonia and 2500sccm of silane are introduced, the coating time is 180s, the temperature is 450-500℃, the coating power is 8 kW, the duty cycle is 1:15, the thickness of SiN film 2 is 22-24nm, the refractive index is 2.6, and the optical path of silicon nitride film is 60nm.

[0064] C. Nitrous oxide, ammonia and silane are introduced at a flow ratio of 14:0.5:1 to prepare a SiON film 3 on a SiN film 2. 7000 sccm of nitric oxide, 250 sccm of ammonia and 500 sccm of silane are introduced. The coating time is 300 s, the temperature is 450-500° C., the coating power is 7 kW, the duty cycle is 1:20, the thickness of the SiON film 3 is 39-41 nm, the refractive index is 1.5, and the optical path of the silicon oxynitride film is 60 nm.

[0065] The back film structure of this embodiment has an average reflectivity of 10.2%. In its back reflectivity curve, the wavelength of the short-wave trough is 330 nm, and the wavelength of the medium- and long-wave trough is 650 nm.

[0066] Example 4

[0067] In this embodiment, a back film structure is provided, which includes an aluminum oxide (AlO) film located on the back of the cell, a silicon nitride (SiN) film is provided on the aluminum oxide film, and a silicon oxynitride (SiON) film is provided on the silicon nitride film.

[0068] The preparation method comprises the following steps:

[0069] A. Place the battery cell 1 with the back side facing upward into the graphite plate, then place the graphite plate into the ALD plate-type chamber, and coat a layer of AlO film 1 on the back side of the battery for 10 times. The thickness of the AlO film 1 is 8 to 10 nm, and the refractive index is 1.56;

[0070] B. Place the battery cell with the back side facing up into a graphite boat, then place the graphite boat into a tubular PECVD, introduce ammonia and silane at a flow ratio of 17:1, and prepare SiN film 2 on AlO film 1. In this step, 8500sccm of ammonia and 500sccm of silane are introduced, the coating time is 600s, the temperature is 450-500℃, the coating power is 8 kW, the duty cycle is 1:15, the thickness of SiN film 2 is 88-92nm, the refractive index is 2.0, and the optical path of silicon nitride film is 180nm.

[0071] C. Nitrous oxide, ammonia and silane were introduced at a flow ratio of 6:0.5:1 to prepare a SiON film 3 on a SiN film 2. 6000 sccm of nitric oxide, 500 sccm of ammonia and 1000 sccm of silane were introduced. The coating time was 500 s, the temperature was 450-500° C., the coating power was 7 kW, the duty cycle was 1:20, the thickness of the SiON film 3 was 91-93 nm, the refractive index was 1.95, and the optical path of the silicon oxynitride film was 180 nm.

[0072] The back film structure of this embodiment has an average reflectivity of 10.1%. In its back reflectivity curve, the wavelength of the short-wave trough is 490nm, and the wavelength of the medium- and long-wave trough is 970nm.

[0073] Example 5

[0074] In this embodiment, a back film structure is provided, which includes an aluminum oxide (AlO) film located on the back of the cell, a silicon nitride (SiN) film is provided on the aluminum oxide film, and a silicon oxynitride (SiON) film is provided on the silicon nitride film.

[0075] The preparation method comprises the following steps:

[0076] A. Place the battery cell 1 with the back side facing upward into the graphite plate, then place the graphite plate into the ALD plate-type chamber, and coat a layer of AlO film 1 on the back side of the battery for 10 times. The thickness of the AlO film 1 is 8 to 10 nm, and the refractive index is 1.56;

[0077] B. Place the battery cell with the back side facing up into a graphite boat, then place the graphite boat into a tubular PECVD, introduce ammonia and silane at a flow ratio of 4.2:1, and prepare SiN film 2 on AlO film 1. In this step, introduce 6300sccm of ammonia and 1500sccm of silane, the coating time is 400s, the temperature is 450-500℃, the coating power is 8 kW, the duty cycle is 1:15, the thickness of SiN film 2 is 55-57nm, the refractive index is 2.35, and the optical path of silicon nitride film is 132nm.

[0078] C. Nitrous oxide, ammonia and silane were introduced at a flow ratio of 5:2:1 to prepare a SiON film 3 on the SiN film 2. 4000 sccm of nitric oxide, 1600 sccm of ammonia and 800 sccm of silane were introduced. The coating time was 608 s, the temperature was 450-500° C., the coating power was 7 kW, the duty cycle was 1:20, the thickness of the SiON film 3 was 77-81 nm, the refractive index was 1.66, and the optical path of the silicon oxynitride film was 132 nm.

[0079] The back film structure of this embodiment has an average reflectivity of 9.5%. In its back reflectivity curve, the wavelength of the short-wave trough is 430nm, and the wavelength of the medium- and long-wave trough is 920nm.

[0080] Comparative Example 1

[0081] In this comparative example, a back film structure is provided, which includes an aluminum oxide (AlO) film located on the back side of a cell, and a silicon nitride (SiN) film is disposed on the aluminum oxide film.

[0082] A. Place the cell with the back side facing upward on the graphite plate, then place the graphite plate in the ALD plate chamber, and coat a layer of AlO film 1 on the back side of the cell for 10 times. The thickness of the AlO film 1 is 8-10 nm, and the refractive index is 1.56.

[0083] B. Place the battery cell with the back side facing up into a graphite boat, then place the graphite boat into a tubular PECVD, introduce ammonia and silane at a flow ratio of 6:1, and prepare SiN film 2 on AlO film 1. 6000sccm of ammonia and 1000sccm of silane are introduced. The coating time is 700s, the temperature is 450-500℃, the coating power is 8 kW, the duty cycle is 1:15, the thickness of SiN film 1 is 84-88nm, and the refractive index is 2.2.

[0084] The average reflectance of this comparative example is 13.1%.

[0085] Comparative Example 2

[0086] This comparative example provides a back film structure such as Figure 3 As shown, the back film structure includes an aluminum oxide (AlO) film located on the back of the battery cell, a silicon nitride (SiN) film is provided on the aluminum oxide film, a silicon oxynitride (SiON) film is provided on the silicon nitride film, and a silicon oxide (SiO) film is provided on the silicon oxynitride (SiON) film.

[0087] The preparation method comprises the following steps:

[0088] A. Place the battery cell with the back side facing upwards into the graphite plate, then place the graphite plate into the ALD plate chamber, and coat a layer of AlO film 1 on the back side of the battery for 10 times. The thickness of the AlO film 1 is 8-10 nm, and the refractive index is 1.56.

[0089] B. Place the battery cell obtained in step A with the back side facing up into a graphite boat, then place the graphite boat into a tubular PECVD, introduce ammonia and silane at a flow ratio of 6:1, and prepare SiN film 2 on AlO film 1. In this step, 6000 sccm of ammonia and 1000 sccm of silane are introduced, the coating time is 500 s, the temperature is 450°C, the coating power is 8 kW, the duty cycle is 1:15, the thickness of SiN film 2 is 60-65 nm, and the refractive index is 2.2.

[0090] C. Nitrous oxide, ammonia and silane were introduced at a flow ratio of 5:2:1 to prepare a SiON film 3 on the SiN film 2. 4000 sccm of nitrous oxide, 1600 sccm of ammonia and 800 sccm of silane were introduced. The coating time was 400 s, the temperature was 450° C., the coating power was 7 kW, the duty cycle was 1:20, the thickness of the SiON film 3 was 52-56 nm, and the refractive index was 1.8.

[0091] D. Laughing gas and silane were introduced at a flow ratio of 14:1 to prepare a SiO film 4 on the SiON film 3. 8400 sccm of laughing gas and 600 sccm of silane were introduced. The coating time was 100 s, the temperature was 450° C., the coating power was 6 kW, the duty cycle was 1:25, the thickness of the SiO film 4 was 15-16 nm, and the refractive index was 1.5.

[0092] Comparative Example 3

[0093] In this embodiment, a back film structure is provided, which includes an aluminum oxide (AlO) film located on the back of the cell, a silicon nitride (SiN) film is provided on the aluminum oxide film, and a silicon oxynitride (SiON) film is provided on the silicon nitride film.

[0094] The preparation method comprises the following steps:

[0095] A. Place the battery cell 1 with the back side facing upward into the graphite plate, then place the graphite plate into the ALD plate-type chamber, and coat a layer of AlO film 1 on the back side of the battery for 10 times. The thickness of the AlO film 1 is 8 to 10 nm, and the refractive index is 1.56;

[0096] B. Place the battery cell with the back side facing up into a graphite boat, then place the graphite boat into a tubular PECVD, introduce ammonia and silane at a flow ratio of 5:1, and prepare SiN film 2 on AlO film 1. In this step, 6500sccm of ammonia and 1300sccm of silane are introduced, the coating time is 530s, the temperature is 450-500℃, the coating power is 8 kW, the duty cycle is 1:15, the thickness of SiN film 2 is 78-82nm, the refractive index is 2.25, and the optical path of silicon nitride film is 180nm.

[0097] C. Nitrous oxide, ammonia and silane were introduced at a flow ratio of 6:0.5:1 to prepare a SiON film 3 on a SiN film 2. 6000 sccm of nitric oxide, 500 sccm of ammonia and 1000 sccm of silane were introduced. The coating time was 500 s, the temperature was 450-500° C., the coating power was 7 kW, the duty cycle was 1:20, the thickness of the SiON film 3 was 91-93 nm, the refractive index was 1.95, and the optical path of the silicon oxynitride film was 180 nm.

[0098] Comparative Example 4

[0099] In this embodiment, a back film structure is provided, which includes an aluminum oxide (AlO) film located on the back of the cell, a silicon nitride (SiN) film is provided on the aluminum oxide film, and a silicon oxynitride (SiON) film is provided on the silicon nitride film.

[0100] The preparation method comprises the following steps:

[0101] A. Place the battery cell 1 with the back side facing upward into the graphite plate, then place the graphite plate into the ALD plate-type chamber, and coat a layer of AlO film 1 on the back side of the battery for 10 times. The thickness of the AlO film 1 is 8 to 10 nm, and the refractive index is 1.56;

[0102] B. Place the battery cell with the back side facing up into a graphite boat, then place the graphite boat into a tubular PECVD, introduce ammonia and silane at a flow ratio of 17:1, and prepare SiN film 2 on AlO film 1. In this step, 8500sccm of ammonia and 500sccm of silane are introduced, the coating time is 600s, the temperature is 450-500℃, the coating power is 8 kW, the duty cycle is 1:15, the thickness of SiN film 2 is 88-92nm, the refractive index is 2.0, and the optical path of silicon nitride film is 180nm.

[0103] C. Nitrous oxide, ammonia and silane were introduced at a flow ratio of 5:2:1 to prepare a SiON film 3 on the SiN film 2. 4000 sccm of nitric oxide, 1600 sccm of ammonia and 800 sccm of silane were introduced. The coating time was 667 s, the temperature was 450-500° C., the coating power was 7 kW, the duty cycle was 1:20, the thickness of the SiON film 3 was 98-102 nm, the refractive index was 1.8, and the optical path of the silicon oxynitride film was 180 nm.

[0104] Comparative Example 5

[0105] In this embodiment, a back film structure is provided, which includes an aluminum oxide (AlO) film located on the back of the cell, a silicon nitride (SiN) film is provided on the aluminum oxide film, and a silicon oxynitride (SiON) film is provided on the silicon nitride film.

[0106] The preparation method comprises the following steps:

[0107] A. Place the battery cell 1 with the back side facing upward into the graphite plate, then place the graphite plate into the ALD plate-type chamber, and coat a layer of AlO film 1 on the back side of the battery for 10 times. The thickness of the AlO film 1 is 8 to 10 nm, and the refractive index is 1.56;

[0108] B. Place the battery cell with the back side facing up into a graphite boat, then place the graphite boat into a tubular PECVD, introduce ammonia and silane at a flow ratio of 17:1, and prepare SiN film 2 on AlO film 1. In this step, 8500sccm of ammonia and 500sccm of silane are introduced, the coating time is 600s, the temperature is 450-500℃, the coating power is 8 kW, the duty cycle is 1:15, the thickness of SiN film 2 is 88-92nm, the refractive index is 2.0, and the optical path of silicon nitride film is 182nm.

[0109] C. Nitrous oxide, ammonia and silane were introduced at a flow ratio of 6:0.5:1 to prepare a SiON film 3 on a SiN film 2. 6000 sccm of nitric oxide, 500 sccm of ammonia and 1000 sccm of silane were introduced. The coating time was 467 s, the temperature was 450-500° C., the coating power was 7 kW, the duty cycle was 1:20, the thickness of the SiON film 3 was 69-71 nm, the refractive index was 1.95, and the optical path of the silicon oxynitride film was 137 nm.

[0110] Comparative Example 6

[0111] The difference between this comparative example and Example 1 is that the coating parameters in step A are adjusted, that is, the coating is performed 4 times so that the thickness of the aluminum oxide film is 3 nm and the refractive index is 1.5.

[0112] Comparative Example 7

[0113] The difference between this comparative example and Example 1 is that by adjusting the coating parameters in step A, that is, coating 22 times, the thickness of the aluminum oxide film is 22 nm and the refractive index is 1.8.

[0114] Comparative Example 8

[0115] The difference between this comparative example and Example 1 is that the thickness of the silicon nitride film is 15 nm and the refractive index is 2.0. In step B, the battery cell is placed in a graphite boat with the back side facing upward, and then the graphite boat is placed in a tubular PECVD, and ammonia and silane are introduced at a flow ratio of 17:1 to prepare a SiN film 2 on the AlO film 1. In this step, 8500 sccm of ammonia and 500 sccm of silane are introduced, the coating time is 110 s, the temperature is 450-500°C, and the thickness of the SiN film 2 is 15 nm and the refractive index is 2.0.

[0116] Comparative Example 9

[0117] The difference between this comparative example and Example 1 is that the thickness of the silicon nitride film is 100 nm and the refractive index is 2.65. In step B, the battery cell is placed in a graphite boat with the back side facing upward, and then the graphite boat is placed in a tubular PECVD, and ammonia and silane are introduced at a flow ratio of 1.5:1 to prepare a SiN film 2 on the AlO film 1. In this step, 4500 sccm of ammonia and 3000 sccm of silane are introduced, the coating time is 660 s, the temperature is 450-500°C, and the thickness of the SiN film 2 is 98-102 nm and the refractive index is 2.65.

[0118] Comparative Example 10

[0119] The difference between this comparative example and Example 1 is that the thickness of the silicon oxynitride film is 17nm and the refractive index is 1.5. In step C, laughing gas, ammonia and silane are introduced at a flow ratio of 14:0.5:1 to prepare a SiON film 3 on a SiN film 2, 7000sccm of laughing gas, 250sccm of ammonia, 500sccm of silane are introduced, the coating time is 130s, the temperature is 450-500°C, the thickness of the SiON film 3 is 16-18nm, and the refractive index is 1.5.

[0120] Comparative Example 11

[0121] The difference between this comparative example and Example 1 is that the thickness of the silicon oxynitride film is 130nm and the refractive index is 2.2. In step C, laughing gas, ammonia and silane are introduced at a flow ratio of 1:4:1.5 to prepare a SiON film 3 on a SiN film 2, 800sccm of laughing gas, 3200sccm of ammonia, 1200sccm of silane are introduced, the coating time is 870s, the temperature is 450-500°C, and the thickness of the SiON film 3 is 128-132nm and the refractive index is 2.2.

[0122] like Figure 2 The reflectivity curves of the back film structures of Example 1 and Comparative Example 1 in the wavelength range of 300nm to 1200nm are given. From the test results of the figure, it is found that the back film structure has an average reflectivity of 9.4%, and the wavelength of the short-wave trough in its back reflectivity curve is 400nm, and the wavelength of the medium- and long-wave trough is 890nm. The average reflectivity of Comparative Example 1 is 13.1%, and the wavelength corresponding to the lowest reflectivity in its curve is 780nm.

[0123] The batteries prepared by the preparation methods of Examples 1 to 5 and Comparative Examples 1 to 11 were subjected to IV tests on the front and back batteries to characterize the electrical properties of the back and front batteries. The electrical properties data of the back batteries are shown in Table 1 below:

[0124] Table 1 Back electrical properties

[0125]

[0126]

[0127] The front electrical performance data is shown in Table 2 below:

[0128] Table 2 Front electrical properties

[0129] name Open circuit voltage Voc(V) Short circuit current Isc(A) Filling factor FF(%) Conversion efficiency EFF (%) Comparative Example 1 0.6652 10.187 78.17 21.56 Comparative Example 2 0.6658 10.186 78.26 21.60 Comparative Example 3 0.6662 10.187 78.38 21.65 Comparative Example 4 0.6657 10.183 78.31 21.61 Comparative Example 5 0.6657 10.182 78.31 21.61 Comparative Example 6 0.6641 10.170 78.21 21.50 Comparative Example 7 0.6660 10.187 78.40 21.65 Comparative Example 8 0.6651 10.187 78.14 21.55 Comparative Example 9 0.6664 10.184 78.33 21.64 Comparative Example 10 0.6658 10.186 78.20 21.59 Comparative Example 11 0.6660 10.187 78.29 21.62 Example 1 0.6662 10.190 78.43 21.67 Example 2 0.6661 10.188 78.42 21.66 Example 3 0.6664 10.187 78.43 21.67 Example 4 0.6660 10.187 78.40 21.65 Example 5 0.6662 10.186 78.43 21.67

[0130] As can be seen from Table 1, the Isc of Example 1 is significantly improved compared with that of Comparative Example 1, with a gain of about 188 mA, mainly because the reflectivity of the film made by the film structure and the coating method in Example 1 is about 3.49% lower than that of the comparative example, so the Isc gain is more obvious. The Isc in Examples 2 to 5 is improved compared with the Isc in Comparative Examples 2 to 5 and Comparative Examples 8 to 11, because the film structure of silicon oxynitride and silicon nitride in the examples satisfies two conditions at the same time: the product of their refractive index is equal to the refractive index of silicon 3.9 and their optical path is equal, which is beneficial to reduce the reflectivity of the back side; while in Comparative Examples 3 to 5 and Comparative Examples 8 to 11, only one of the conditions is met or none of them are met, which is not conducive to the anti-reflection effect.

[0131] As shown in Table 2, the opening voltage of Example 1 is increased by 1.0mV and the FF is increased by 0.26% compared with that of Comparative Example 1. The unique back film structure and back reflectivity curve are beneficial to the overall passivation of the battery, so the opening voltage and FF gain are more obvious. The opening voltage of Comparative Example 6 is 2.1mV lower than that of Example 1, the short-circuit current is 20mA lower, and the FF is 0.22% lower. This is because the thickness of aluminum oxide in the comparative example is only 3nm, and the overall passivation effect of the battery is poor, so its opening voltage, short-circuit current and FF are low. The efficiency difference of Comparative Example 7 is not much, but the thickness of aluminum oxide is 22nm, which will reduce the production capacity of the equipment.

[0132] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the back film structure for improving the efficiency of the back side of bifacial PERC and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A back film structure for improving the back efficiency of a bifacial PERC, characterized in that: The back film structure includes an aluminum oxide film located on the back of the cell, a silicon nitride film is provided on the aluminum oxide film, and a silicon oxynitride film is provided on the silicon nitride film; wherein the product of the refractive index of the silicon nitride film and the refractive index of the silicon oxynitride film is equal to the refractive index of silicon, and the optical path of the silicon nitride film is equal to the optical path of the silicon oxynitride film; The silicon nitride film has a thickness of 20 to 90 nm and a refractive index of 2.0 to 2.

6.

2. The back film structure for improving the back efficiency of bifacial PERC according to claim 1, characterized in that: The refractive index of silicon is 3.

9.

3. The back film structure for improving the back efficiency of bifacial PERC according to claim 1, characterized in that: The optical path length of the silicon nitride film and the silicon oxynitride film is 60nm to 180nm.

4. The back film structure for improving the back efficiency of bifacial PERC according to claim 1, characterized in that: The aluminum oxide film has a thickness of 5 to 15 nm and a refractive index of 1.5 to 1.

7.

5. The back film structure for improving the back efficiency of bifacial PERC according to claim 4, characterized in that: The aluminum oxide film has a thickness of 8-10 nm and a refractive index of 1.

5.

6. The back film structure for improving the back efficiency of bifacial PERC according to claim 1, characterized in that: The silicon nitride film has a thickness of 40 to 70 nm and a refractive index of 2.25 to 2.

5.

7. The back film structure for improving the back efficiency of bifacial PERC according to claim 1, characterized in that: The silicon oxynitride film has a thickness of 30 to 120 nm and a refractive index of 1.5 to 1.

95.

8. The back film structure for improving the back efficiency of bifacial PERC according to claim 7, characterized in that: The silicon oxynitride film has a thickness of 68 to 80 nm and a refractive index of 1.56 to 1.

73.

9. The back film structure for improving the back efficiency of bifacial PERC according to claim 1, characterized in that: The reflectivity curve of the back film structure has two troughs in the wavelength range of 300nm to 1200nm, one of which is between short waves of 330 and 500nm, and the other is between medium and long waves of 650 and 1000nm.

10. The back film structure for improving the back efficiency of bifacial PERC according to claim 9, characterized in that: In the reflectivity curve of the back film structure within the wavelength range of 300nm to 1200nm, the wavelength corresponding to the trough of short wave is 360 to 440nm, and the wavelength corresponding to the trough of medium and long wave is 850 to 950nm.

11. The method for preparing a back film structure for improving the back efficiency of a bifacial PERC according to any one of claims 1 to 10, characterized in that: The preparation method comprises the following steps: A. Place the cell with the back side facing upward into the graphite plate, then place the graphite plate into the ALD plate chamber, and coat the back side of the cell to obtain an aluminum oxide film; B. Place the battery cell obtained in step A with the back side facing upward into a graphite boat, then place the graphite boat into a tubular PECVD, introduce ammonia and silane gases, and coat the aluminum oxide film to prepare a silicon nitride film; C. introducing laughing gas, ammonia and silane gas to coat the silicon nitride film to prepare a silicon oxynitride film, and making the product of the refractive index of the silicon nitride film and the refractive index of the silicon oxynitride film equal to the refractive index of silicon, and the optical path of the silicon nitride film equal to the optical path of the silicon oxynitride film, thereby obtaining the back film structure.

12. The preparation method according to claim 11, characterized in that: The number of times of coating in step A is 6-15 times.

13. The preparation method according to claim 11, characterized in that: The silane in step B is SiH4.

14. The preparation method according to claim 11, characterized in that: The flow ratio of ammonia and silane introduced in step B is 17:1 to 2:

1.

15. The preparation method according to claim 11, characterized in that: The coating power in step B is 8 kilowatts and the duty cycle is 1:

15.

16. The preparation method according to claim 11, characterized in that: The coating time in step B is 160-600s.

17. The preparation method according to claim 11, characterized in that: The coating temperature in step B is 450-500°C.

18. The preparation method according to claim 11, characterized in that: The flow ratio of the laughing gas, ammonia and silane introduced in step C is 14:2:1 to 5:0.5:

1.

19. The preparation method according to claim 11, characterized in that: The coating power in step C is 7 kilowatts and the duty cycle is 1:

20.

20. The preparation method according to claim 11, characterized in that: The coating time in step C is 300-800s.

21. The preparation method according to claim 11, characterized in that: The coating temperature in step C is 450-500°C.

22. A bifacial PERC cell, characterized in that: The bifacial PERC cell comprises a back film structure for improving the back efficiency of the bifacial PERC cell as described in any one of claims 1 to 10.