Negative electrode slurry, negative electrode and rechargeable battery
By using acrylic-acrylonitrile copolymer and particle dispersion in the negative electrode slurry, the problems of cracks and expansion during the coating and drying process of the negative electrode slurry are solved, and the stability and cycle characteristics of the negative electrode are improved.
Patent Information
- Application Number
- CN202111192235.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-05-20
- Filing Date
- 2021-10-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-10-13
AI Technical Summary
Existing anode slurries are prone to cracks during the coating and drying processes, leading to expansion of the anode and deterioration of cycle characteristics, and it is difficult to suppress the expansion of silicon-containing active materials.
A water-soluble polymer containing acrylic acid-acrylonitrile copolymer is used as a binder, combined with the particle dispersion, to adjust the viscosity and flexibility of the negative electrode slurry, ensuring that no cracks occur during the coating and drying process, and inhibiting the expansion of the negative electrode .
It effectively suppresses the expansion of the negative electrode, prevents the occurrence of cracks, improves the cycle characteristics and capacity retention rate, and enhances the stability of the negative electrode and the cycle life of the battery.
Smart Images

Figure GDA0003479804820000131 
Figure GDA0003479804820000221 
Figure GDA0003479804820000231
Abstract
Description
Technical Field
[0001] Disclosed are a negative electrode slurry, a negative electrode formed using the negative electrode slurry, and a rechargeable battery including the negative electrode. Background Art
[0002] One method for ensuring high capacity of non-aqueous electrolyte rechargeable batteries including rechargeable lithium ion batteries is to apply a silicon-containing active material that includes an amount of intercalated lithium that is larger than the amount of conventional graphite-based active materials. However, since the silicon-containing active material exhibits a large volume change due to the insertion / deintercalation of lithium, the negative electrode mixture layer expands and contracts violently during charging and discharging. As a result, there are problems such as reducing the electronic conductivity between the negative electrode active material and the negative electrode active material, isolating the silicon-containing active material in the mixture layer, blocking the conductive path between the negative electrode active material and the current collector, etc., thereby deteriorating the cycle characteristics of the rechargeable battery.
[0003] Therefore, in order to suppress the expansion of the negative electrode, as shown in Patent Documents 1 to 3, the negative electrode may be manufactured using a negative electrode slurry including an acrylic polymer having relatively high hardness as a binder.
[0004] [Existing Technology]
[0005] [Patent Document 1] Japanese Patent Publication No. 2019-160690
[0006] [Patent Document 2] Japanese Patent No. 6412689
[0007] [Patent Document 3] Japanese Patent No. 5279047 Summary of the invention
[0008] When a negative electrode is manufactured using the negative electrode slurry described in Patent Documents 1 to 3, for example, when a negative electrode having a capacity of about 3.5 mAh / cm 2 When the negative electrode has an area capacity of 2.5×10-1.5A, cracks may appear in the negative electrode during the coating and drying process of the negative electrode slurry.
[0009] The embodiments have been made in view of the above problems, and provide a negative electrode slurry for forming a negative electrode which suppresses expansion of a negative electrode containing silicon atoms and capacity degradation due to repetition of charge / discharge cycles and is difficult to generate cracks during coating and drying processes.
[0010] The negative electrode slurry according to the embodiment includes: a negative electrode active material, including a first active material containing silicon atoms in an amount greater than or equal to about 5wt% and less than or equal to about 100wt%; a binder for binding the negative electrode active material; and a solvent for the negative electrode slurry to disperse the negative electrode active material and the binder, wherein the first active material contains silicon atoms in an amount greater than or equal to about 20wt% and less than or equal to about 100wt%, the binder includes a particle dispersion and a water-soluble polymer, the water-soluble polymer includes a copolymer containing an acrylic monomer and an acrylonitrile monomer (hereinafter, also referred to as an acrylic acid-acrylonitrile copolymer), and when the total of the negative electrode active material and the binder is 100wt%, the content of the water-soluble polymer is greater than or equal to about 0.5wt% and less than or equal to about 2wt%.
[0011] According to the negative electrode slurry configured in this manner, since the binder includes the water-soluble polymer including the acrylic acid-acrylonitrile-based copolymer, expansion of the negative electrode including the silicon-containing active material can be effectively suppressed.
[0012] In addition, since the binder contains not only a water-soluble polymer but also a particle dispersion and the content of the water-soluble polymer in the binder is greater than or equal to about 0.5 wt % and less than or equal to about 2 wt %, the flexibility of the negative electrode mixture layer formed by coating and drying the negative electrode slurry can be adjusted to an appropriate range.
[0013] As a result, the occurrence of cracks in the negative electrode at the time of coating and drying can be suppressed.
[0014] In order to suppress expansion of the negative electrode, the acrylic acid-acrylonitrile copolymer may include a (meth)acrylic acid monomer-derived unit in an amount greater than or equal to about 40 wt % and less than or equal to about 70 wt % and a (meth)acrylonitrile monomer-derived unit in an amount greater than or equal to about 30 wt % and less than or equal to about 60 wt %.
[0015] By applying the copolymer having such a configuration, it is possible to suppress the negative electrode mixture layer formed by coating and drying the negative electrode slurry including the copolymer on the negative electrode collector from being peeled off from the negative electrode collector, and improve the cycle maintenance ratio.
[0016] The acrylic acid-acrylonitrile-based copolymer may further include a unit derived from other monomers copolymerizable with the (meth)acrylic acid-based monomer and / or the (meth)acrylonitrile-based monomer.
[0017] From the viewpoint of reducing expansion of the negative electrode during charge and peeling of the negative electrode mixture layer from the negative electrode collector, it is desirable that the water-soluble polymer includes the acrylic acid-acrylonitrile-based copolymer in an amount of greater than or equal to about 50 wt %.
[0018] As a specific example, for example, the (meth)acrylic monomer may be at least one type selected from (meth)acrylic acid, a metal salt of (meth)acrylic acid, an ammonium salt of (meth)acrylic acid, and an amine salt of (meth)acrylic acid.
[0019] From the viewpoint of suppressing expansion of the negative electrode during charge and peeling of the negative electrode mixture layer from the negative electrode collector, the 8 wt % aqueous solution of the acrylic acid-acrylonitrile-based copolymer may have a viscosity of greater than or equal to about 500 mPas at 25° C.
[0020] In addition, if the viscosity of the aqueous solution of 8 wt % acrylic acid-acrylonitrile copolymer is less than or equal to about 10,000 mPas at 25° C., the viscosity of the negative electrode slurry will not become too large, and there is no need to reduce the solid content concentration of the negative electrode slurry to adjust the viscosity, and the drying time can be reduced to improve productivity.
[0021] From the viewpoint of improving the stability of the negative electrode slurry, the particle dispersion may include a polymer having a glass transition temperature of greater than or equal to about -30°C and less than or equal to about 20°C.
[0022] Specific examples of the particle dispersion may include a copolymer including a styrene monomer-derived unit and a butadiene monomer-derived unit.
[0023] From the viewpoint of adjusting the negative electrode slurry to a viscosity suitable for coating, the water-soluble polymer may further include a cellulose ether containing a carboxymethyl group or a salt of a cellulose ether containing a carboxymethyl group.
[0024] From the viewpoint of ease of coating, the negative electrode slurry may have a viscosity of greater than or equal to about 1000 mPa·s and less than or equal to about 5000 mPa·s at a solid content concentration of greater than or equal to about 45 wt % and less than or equal to about 60 wt % at 25° C.
[0025] On the other hand, the solid content concentration of the negative electrode slurry can be obtained from the ratio of the total mass of each component except the solvent for the negative electrode slurry added when preparing the negative electrode slurry (for the components added as powder, the mass as the powder, or for the components added as an aqueous solution, the mass as the solid component calculated from the concentration in the aqueous solution) to the total mass of the negative electrode slurry.
[0026] In a specific embodiment, the negative electrode active material may further include a graphite-based active material as a second active material.
[0027] In addition, the negative electrode slurry may further include a conductive agent.
[0028] The negative electrode slurry may suppress expansion of an electrode caused by a silicon-containing active material and capacity degradation of a rechargeable battery due to repeated charge and discharge cycles, and may form a negative electrode that is less susceptible to cracking during coating and drying processes. DETAILED DESCRIPTION
[0029] Hereinafter, specific embodiments will be described in detail so that those skilled in the art can easily implement them. However, the present disclosure may be embodied in many different forms and is not to be construed as limited to the example embodiments set forth herein.
[0030] The terms used herein are for describing the embodiments only and are not intended to limit the present invention. Unless the context clearly dictates otherwise, a singular expression includes a plural expression.
[0031] As used herein, "combinations thereof" refers to mixtures, laminates, composites, copolymers, alloys, blends, reaction products, and the like of the components.
[0032] Here, it should be understood that terms such as "comprising", "including" or "having" are intended to indicate the presence of the embodied features, quantities, steps, elements or combinations thereof, but do not exclude the possibility of the presence or addition of one or more other features, quantities, steps, elements or combinations thereof.
[0033] It will be understood that when an element such as a layer, film, region, or substrate is referred to as being "on" another element, the element can be directly on the other element or intervening elements may also be present. In contrast, when an element is referred to as being "directly on" another element, there are no intervening elements.
[0034] In addition, the "layer" here includes not only a shape formed on the entire surface when viewed from a plan view but also a shape formed on a part of the surface.
[0035] Hereinafter, a detailed configuration of a rechargeable battery according to an embodiment will be described.
[0036] <1. Non-aqueous electrolyte rechargeable battery>
[0037] The rechargeable lithium ion battery according to the embodiment includes a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte. The charging voltage (redox potential) of the rechargeable lithium ion battery can be greater than or equal to about 4.0V (relative to Li / Li+) and less than or equal to about 5.0V, or greater than or equal to about 4.2V and less than or equal to about 5.0V. The shape of the rechargeable lithium ion battery is not particularly limited, but it can be, for example, cylindrical, prismatic, laminated or button-shaped.
[0038] (1-1, positive electrode)
[0039] The positive electrode includes a positive electrode current collector and a positive electrode mixture layer formed on the positive electrode current collector. The positive electrode current collector may be any conductor as long as it is a conductor, and the positive electrode current collector may be, for example, plate-shaped or thin-shaped, and is desirably made of aluminum, stainless steel, nickel-plated steel, etc. The positive electrode mixture layer includes a positive electrode active material, and may also include a conductive agent and a positive electrode binder.
[0040] The positive electrode active material may be, for example, a transition metal oxide or a solid solution oxide containing lithium, and is not particularly limited as long as it is a material capable of electrochemically intercalating and deintercalating lithium ions.
[0041] Examples of transition metal oxides containing lithium may include Li 1.0 Ni 0.88 Co 0.1 Al 0.01 Mg 0.01 O2, etc. In addition, it may include Li-Co based composite oxides such as LiCoO2, such as LiNi x Co y Mn z O2 or the like, a Li-Ni-Co-Mn based composite oxide such as LiNiO2 or the like, a Li-Ni based composite oxide such as LiMn2O4 or the like.
[0042] Examples of solid solution oxides may include Li a Mn x Co y Ni z O2 (1.150≤a≤1.430, 0.45≤x≤0.6, 0.10≤y≤0.15 and 0.20≤z≤0.28), LiMn 1.5 Ni 0.5 O4, etc.
[0043] On the other hand, the content (content ratio) of the positive electrode active material is not particularly limited, and any content suitable for the positive electrode mixture layer of the nonaqueous electrolyte rechargeable battery may be sufficient. In addition, these compounds may be used independently, or a plurality of types of compounds may be mixed and used.
[0044] The conductive agent is not particularly limited as long as it is used to increase the conductivity of the positive electrode. Specific examples of the conductive agent include conductive agents containing at least one selected from carbon black, natural graphite, artificial graphite and fibrous carbon. Examples of carbon black include furnace black, channel black, thermal cracking black, Ketjen black and acetylene black. Examples of fibrous carbon include carbon nanotubes, graphene and carbon nanofibers.
[0045] The content of the conductive agent is not particularly limited, and any content suitable for the positive electrode mixture layer of the nonaqueous electrolyte rechargeable battery may suffice.
[0046] Examples of binders for the positive electrode may include fluorine-containing resins (such as polyvinylidene fluoride), ethylene-containing resins (such as styrene-butadiene rubber and ethylene-propylene-diene terpolymers), acrylonitrile-butadiene rubber, fluororubber, polyvinyl acetate, polymethyl methacrylate, polyethylene, polyvinyl alcohol, carboxymethyl cellulose or carboxymethyl cellulose derivatives (such as salts of carboxymethyl cellulose), or nitrocellulose.
[0047] The binder used for the positive electrode may be any binder capable of binding the positive electrode active material and the conductive agent to the positive electrode collector, and is not particularly limited.
[0048] (1-2, negative electrode)
[0049] The negative electrode includes a negative electrode current collector and a negative electrode mixture layer formed on the negative electrode current collector. The negative electrode current collector can be any conductor as long as it is a conductor (e.g., a plate-shaped or thin-shaped conductor), and the negative electrode current collector can be desirably composed of copper, stainless steel, nickel-plated steel, etc. The negative electrode mixture layer may include, for example, a negative electrode active material and a negative electrode binder. The configuration of the negative electrode mixture layer is a characteristic part of the present invention and will be described in detail later.
[0050] (1-3, diaphragm)
[0051] The separator is not particularly limited, and any separator can be used as long as it is used as a separator for a rechargeable lithium ion battery. The separator may be a porous film or nonwoven fabric having excellent high-rate discharge performance that can be used alone or together with other materials.
[0052] Examples of resins that constitute the diaphragm may include polyolefin resins (such as polyethylene and polypropylene), polyester resins (such as polyethylene terephthalate and polybutylene terephthalate), polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-perfluorovinyl ether copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-vinyl fluoride copolymer, vinylidene fluoride-hexafluoroacetone copolymer, vinylidene fluoride-ethylene copolymer, vinylidene fluoride-propylene copolymer, vinylidene fluoride-trifluoropropylene copolymer, vinylidene fluoride-tetrafluoroethylene copolymer or vinylidene fluoride-ethylene-tetrafluoroethylene copolymer.
[0053] On the other hand, the porosity of the separator is not particularly limited and may be any porosity that a separator of a conventional rechargeable lithium ion battery has. On the surface of the separator, a heat-resistant layer including inorganic particles for improving heat resistance or a layer including an adhesive for adhering to an electrode to fix the battery element may be provided.
[0054] The inorganic particles may include Al2O3, AlOOH, Mg(OH)2, SiO2, etc. Examples of the binder may include vinylidene fluoride - hexafluoropropylene copolymer, acid - modified products of vinylidene fluoride polymers, and styrene - (meth)acrylate copolymers.
[0055] (1 - 4, Non - aqueous electrolyte)
[0056] For the non - aqueous electrolyte, a commonly used non - aqueous electrolyte for rechargeable lithium - ion batteries can be used without particular limitation. The non - aqueous electrolyte has a composition in which an electrolyte salt is contained in a non - aqueous solvent (which is a solvent for the electrolyte).
[0057] The non - aqueous solvent may include, for example, cyclic carbonates (such as propylene carbonate, ethylene carbonate, butylene carbonate, chloroethylene carbonate, fluoroethylene carbonate, or vinylene carbonate) that can be used alone or as a mixture of two or more, cyclic esters (such as γ - butyrolactone or γ - valerolactone), linear carbonates (such as dimethyl carbonate, diethyl carbonate, or ethyl methyl carbonate), linear esters (such as methyl formate, methyl acetate, methyl butyrate, ethyl propionate, or propyl propionate), ethers (such as tetrahydrofuran or its derivatives, 1,3 - dioxane, 1,4 - dioxane, 1,2 - dimethane, 1,2 - dimethoxyethane, 1,4 - dibutoxyethane, methyl diglycol dimethyl ether, ethylene glycol monopropyl ether, or propylene glycol monopropyl ether), nitriles (such as acetonitrile and benzonitrile), dioxolane or its derivatives, ethyl thioether, sulfolane, sultone or its derivatives. On the other hand, when two or more of the non - aqueous solvents are mixed and used, the mixing ratio of each non - aqueous solvent can be a mixing ratio applicable to conventional rechargeable lithium - ion batteries.
[0058] Examples of the electrolyte salt may include inorganic ionic salts containing lithium (Li), sodium (Na), or potassium (K) (such as LiClO4, LiBF4, LiAsF6, LiPF6, LiPF 6-x (C n F 2n+1 ) x [provided that 1 < x < 6, n = 1 or 2], LiSCN, LiBr, LiI, Li2SO4, Li2B 10 Cl 10, NaClO4, NaI, NaSCN, NaBr, KClO4, KSCN), organic ion salts (such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(CF3SO2)(C4F9SO2), LiC(CF3SO2)3, LiC(C2F5SO2)3, (CH3)4NBF4, (CH3)4NBr, (C2H5 )4NClO4, (C2H5)4NI, (C3H7)4NBr, (n-C4H9)4NClO4, (n-C4H9)4NI, (C2H5)4N-maleate, (C2H5)4N-benzoate, (C2H5)4N-phthalate, lithium stearyl sulfonate, lithium octyl sulfonate or lithium dodecylbenzene sulfonate), and these ionic compounds can be used alone or in mixture of two or more.
[0059] On the other hand, the concentration of the electrolyte salt is the same as that of the electrolyte salt in the non-aqueous electrolyte for conventional rechargeable lithium ion batteries without particular limitation. In an embodiment, the non-aqueous electrolyte may include the aforementioned lithium compound (electrolyte salt) at a concentration greater than or equal to about 0.8 mol / L and less than or equal to about 1.5 mol / L.
[0060] On the other hand, various additives can be added to the non-aqueous electrolyte. Examples of such additives can include additives for the negative electrode, additives for the positive electrode, ester additives, carbonate additives, sulfate additives, phosphate additives, borate additives, anhydride additives, and electrolyte additives. One of these additives can be added to the non-aqueous electrolyte, or multiple types of additives can be added to the non-aqueous electrolyte.
[0061] <2. Method for manufacturing a non-aqueous electrolyte rechargeable battery>
[0062] A method for manufacturing a rechargeable lithium-ion battery is described.
[0063] The positive electrode can be manufactured as follows. First, a mixture of a desired ratio of a positive electrode active material, a conductive agent, and a binder for a positive electrode is dispersed in a solvent for a positive electrode slurry (e.g., N-methyl-2-pyrrolidone) to form a positive electrode slurry. Subsequently, the positive electrode slurry is coated on a positive electrode current collector and dried to form a positive electrode mixture layer.
[0064] In addition, the coating method is not particularly limited. The coating method can be, for example, a blade coater method, a gravure coater method, a reverse roll coater method, or a slot die coater method. Each coating method can also be performed by the same method. Next, the positive electrode material mixture layer can be pressed to a desired density by a press. Thus, a positive electrode is manufactured.
[0065] The negative electrode can also be manufactured in the same manner as the positive electrode. First, a negative electrode slurry is prepared by dispersing a mixture of materials constituting the negative electrode mixture layer in a solvent for the negative electrode slurry (taking an aqueous solvent such as water as an example). Then, the negative electrode slurry is applied to the negative electrode current collector and dried to form the negative electrode mixture layer. Subsequently, the negative electrode mixture layer is pressed to a desired density using a press. Thus, the negative electrode is manufactured.
[0066] Subsequently, an electrode structure is prepared by sandwiching a separator between the positive electrode and the negative electrode. Then, the electrode structure is processed into a desired shape (e.g., cylindrical, prismatic, laminated, button, etc.) and inserted into a container of the above shape. Then, by injecting a non-aqueous electrolyte into the container, the electrolyte is impregnated into the pores in the separator and the voids in the positive electrode and the negative electrode. Thus, a rechargeable lithium-ion battery is manufactured.
[0067] <3. Characteristics of the Adhesive Composition>
[0068] Hereinafter, the negative electrode mixture layer according to the embodiment and the negative electrode slurry for forming the negative electrode mixture layer will be described in detail.
[0069] (3-1. Negative Electrode Slurry)
[0070] As described above, the negative electrode slurry includes a negative electrode active material and a negative electrode binder. The negative electrode slurry also includes a solvent for the negative electrode slurry in which the negative electrode active material and the negative electrode binder are dispersed.
[0071] The negative electrode active material includes, for example, an Si-based active material (also referred to as the first active material) as a silicon-containing active material containing silicon atoms, and optionally includes a graphite-based active material containing graphite (also referred to as the second active material).
[0072] Specific examples of the Si-based active material may include, for example, at least one active material selected from a mixture (silicon-carbon composite active material) of particles of silicon (Si) or silicon oxide (SiO x (0 < x ≤ 2)) combined with graphite carbon or amorphous carbon, silicon particles, silicon-based alloys, etc.
[0073] Specific examples of the graphite-based active material may include, for example, at least one active material selected from the following: coke (such as coal-based, petroleum-based pure coke, calcined coke, and needle coke), artificial graphite obtained by graphitizing a graphite precursor (such as mesophase carbon (such as mesophase spheres or massive mesophase)) at about 1500 °C or higher (e.g., about 2800 °C to about 3200 °C), natural graphite (natural graphite in the form of flakes, lumps, or granular spheres), a mixture of artificial graphite and natural graphite, natural graphite coated with artificial graphite, etc.
[0074] These graphite-based active materials may be subjected to chemical or physical treatment, and the treatment methods may include pulverization, classification, granulation, lamination, compression, compounding, mixing, coating, oxidation, vapor deposition, mechanochemical treatment, angle removal, spheroidization, bending, heat treatment, and the like.
[0075] In the case of artificial graphite, these treatments may be combined before or after the graphitization treatment. Specific examples of artificial graphite may include, but are not limited to, MCMB, MCF, and MAG.
[0076] From the perspective of sufficiently increasing the charge / discharge capacity of the negative electrode mixture layer, the content ratio of the graphite-based active material to the Si-based active material can be adjusted, for example, so that the specific capacity (unit: mAh / g) of the Si-based active material can be 3.5 times or more relative to the specific capacity (unit: mAh / g) of the graphite-based active material.
[0077] To achieve such a capacity ratio, the Si-based active material contains silicon atoms in an amount greater than or equal to about 20 wt % and less than or equal to about 100 wt %, and the content of the Si-based active material in the negative active material may be greater than or equal to about 5 wt % and less than or equal to about 100 wt %.
[0078] In addition to the above, the negative electrode active material may also include, for example, a mixture of Sn-based active materials (e.g., tin (Sn) or tin oxide particles and graphite-based active materials, tin particles, tin-based alloys), metallic lithium, and titanium oxide compounds (such as Li4Ti5O 12 ), at least one negative electrode active material selected from lithium nitride, etc.
[0079] The negative electrode binder may be a binder for binding the negative electrode active material and the negative electrode mixture layer to the negative electrode collector, and includes a particle dispersion and a water-soluble polymer.
[0080] The particle dispersion may be particles that may be uniformly dispersed in an aqueous solvent such as water that may be a solvent for the negative electrode slurry, and may be particles of a hydrophobic polymer having a glass transition temperature greater than or equal to about -50° C. or more desirably greater than or equal to about -30° C. The hydrophobic polymer may include, for example, styrene monomer-derived units and butadiene monomer-derived units.
[0081] Specific examples of the hydrophobic polymer may include, for example, styrene-butadiene copolymers, modified styrene-butadiene copolymers obtained by vulcanizing styrene-butadiene copolymers, styrene-acrylate copolymers, polyolefin-based polymers, and polyvinylidene fluoride-based polymers.
[0082] The hydrophobic polymer may be a synthetic rubber having a glass transition temperature less than or equal to room temperature (e.g., less than or equal to about 20° C.). The glass transition temperature may be measured by increasing the temperature from -40° C. to 200° C. at a rate of 10° C. / min using a thermomechanical analyzer (manufactured by TA).
[0083] Meanwhile, in addition to the above-mentioned water, the aqueous solvent may be, for example, a mixture of water and a water-miscible organic solvent, and the water content may be greater than or equal to about 50 wt %. Examples of the water-miscible organic solvent include water-soluble alcohols.
[0084] The average particle size of the particle dispersion may be greater than or equal to about 10 nm and less than or equal to 500 nm, greater than or equal to about 30 nm and less than or equal to 400 nm, or greater than or equal to about 50 nm and less than or equal to 300 nm. The average particle size may be measured by a laser diffraction method using a commercially available laser diffraction particle size measurement device (e.g., MT 3000 from Microtrac).
[0085] The water-soluble polymer may include an acrylic acid-acrylonitrile copolymer. The acrylic acid-acrylonitrile copolymer may include a (meth) acrylic acid monomer-derived unit and a (meth) acrylonitrile monomer-derived unit. In the acrylic acid-acrylonitrile copolymer, the content of the (meth) acrylic acid monomer-derived unit may be greater than or equal to about 40wt% and less than or equal to about 70wt%, and the content of the (meth) acrylonitrile monomer-derived unit may be greater than or equal to about 30wt% and less than or equal to about 60wt%.
[0086] In addition, the acrylic acid-acrylonitrile copolymer may further include units derived from other monomers copolymerizable with the (meth)acrylic acid monomer and / or the (meth)acrylonitrile monomer, and the content of the units derived from other monomers may be in the range of greater than about 0 wt % and less than or equal to about 20 wt %.
[0087] In the acrylic acid-acrylonitrile copolymer, if the content of the (meth)acrylic acid monomer-derived unit is greater than or equal to about 40 wt %, the acrylic acid-acrylonitrile copolymer can be easily dissolved in water and the dispersibility of the negative active material and the storage stability of the negative electrode slurry can be further improved.
[0088] In addition, if the content of the structural unit derived from the (meth)acrylic acid-based monomer in the acrylic acid-acrylonitrile-based copolymer is less than or equal to about 70 wt %, the occurrence of cracks in the coating and drying processes of the negative electrode slurry may be further suppressed.
[0089] If the content of the structural unit derived from the (meth)acrylonitrile-based monomer in the acrylic acid-acrylonitrile-based copolymer is greater than or equal to about 30 wt %, the close contact property of the negative electrode mixture layer with the negative electrode collector may be further improved.
[0090] In addition, when the content of the structural unit derived from the (meth)acrylonitrile monomer in the acrylic acid-acrylonitrile copolymer is less than or equal to about 60 wt %, the acrylic acid-acrylonitrile copolymer can be easily dissolved in water and the dispersibility of the negative active material and the storage stability of the negative electrode slurry can be further improved.
[0091] In the acrylic acid-acrylonitrile copolymer, if the content of the structural unit derived from other monomers copolymerizable with the (meth)acrylic acid monomer and / or the (meth)acrylonitrile monomer is less than or equal to about 20 wt %, cracks may be suppressed from occurring during the coating and drying processes of the negative electrode slurry or the negative electrode mixture layer may be peeled off from the negative electrode current collector during charging.
[0092] The (meth)acrylic acid-based monomer may include at least one selected from the group consisting of (meth)acrylic acid, a metal salt of (meth)acrylic acid, an ammonium salt of (meth)acrylic acid, and an amine salt of (meth)acrylic acid.
[0093] The metal salt of (meth)acrylic acid may be, for example, an alkali metal salt of acrylic acid. Examples of the metal salt of acrylic acid may include sodium acrylate, lithium acrylate, potassium acrylate, calcium acrylate, magnesium acrylate, sodium methacrylate, lithium methacrylate, potassium methacrylate, and calcium methacrylate. Among these, sodium acrylate may be desirable.
[0094] Examples of the ammonium salt of (meth)acrylic acid may include a product of neutralization of (meth)acrylic acid with ammonia, a product of neutralization with monoethanolamine, a product of neutralization with diethanolamine, and a product of neutralization with hydroxylamine. Among these, a product of neutralization of acrylic acid with ammonia may be desirable.
[0095] Other monomers copolymerizable with (meth) acrylic acid monomer and / or (meth) acrylonitrile monomer in acrylic acid-acrylonitrile copolymer can be, for example, water-soluble monomers. Specific examples of water-soluble monomers can include (meth) acrylamide, N-(2-hydroxyethyl) acrylamide, N-(2-hydroxyethyl) methacrylamide, 2-hydroxyethyl (meth) acrylate, vinyl pyrrolidone, vinyl acetamide, vinyl formamide, vinyl alcohol, etc.
[0096] The viscosity of an aqueous solution of 8 wt % of the acrylic acid-acrylonitrile copolymer at 25° C. may be greater than or equal to about 500 mPas and less than or equal to about 10000 mPas.
[0097] When the viscosity of the aqueous solution of the acrylic acid-acrylonitrile-based copolymer is greater than or equal to about 500 mPa·s, close contact properties of the negative electrode mixture layer and the negative electrode collector may be improved.
[0098] In addition, when the viscosity of the aqueous solution of the acrylic acid-acrylonitrile copolymer is less than or equal to about 10000 mPa·s, the negative electrode slurry for forming the negative electrode mixture layer is not given too high a viscosity, so that the slurry can be coated in a high solid content state, and the negative electrode slurry can be effectively dried to obtain the negative electrode.
[0099] The preparation method for making the viscosity of the aqueous solution of the acrylic acid-acrylonitrile copolymer fall within the above range is not particularly limited, but, for example, when synthesizing the acrylic acid-acrylonitrile copolymer, a divinyl monomer as another monomer other than the above may be copolymerized to increase the viscosity.
[0100] Examples of the divinyl-based monomer may include N,N′-methylenebisacrylamide, ethylene glycol dimethacrylate, N,N′-ethylenebis[2-(vinylsulfonyl)acetamide], N,N′-trimethylenebis[2-(vinylsulfonyl)acetamide], and the like.
[0101] The water-soluble polymer may also include water-soluble polymer compounds other than acrylic acid-acrylonitrile copolymers. The water-soluble polymer compound may include, for example, a cellulose ether containing a carboxymethyl group or a salt of a cellulose ether containing a carboxymethyl group. A specific example of such a water-soluble polymer compound may include an alkali metal salt of carboxymethyl cellulose.
[0102] From the viewpoint of reducing expansion of the negative electrode caused by the Si-based active material and peeling of the negative electrode mixture layer from the negative electrode collector, the content of the acrylic acid-acrylonitrile copolymer in the water-soluble polymer may be greater than or equal to about 50 wt %, or greater than or equal to about 70 wt %.
[0103] When the total mass of the negative electrode active material and the negative electrode binder is 100 wt %, the content of the negative electrode binder may be about 2.5 wt % to about 4.5 wt %.
[0104] If the content of the negative electrode binder is greater than or equal to about 2.5wt%, the negative electrode mixture layer can be suppressed from cracking or peeling when the negative electrode mixture layer is coated, dried and rolled (pressed). In addition, if the content of the negative electrode binder is less than or equal to about 4.5wt%, excessive electrode resistance can be suppressed, and a negative electrode with good cycle performance can be obtained.
[0105] When the total mass of the negative electrode active material and the negative electrode binder is 100wt%, the content of the water-soluble polymer may be in a range of greater than or equal to about 0.5wt% and less than or equal to about 2wt%. When the content of the water-soluble polymer is greater than or equal to about 0.5wt%, the expansion of the negative electrode caused by the Si-based active material may be sufficiently suppressed. In addition, when the content of the water-soluble polymer is less than or equal to about 2wt%, cracks are unlikely to occur in the negative electrode mixture layer when coating, drying, and rolling the negative electrode slurry.
[0106] The viscosity of the negative electrode slurry at a solid content concentration of greater than or equal to about 45 wt % and less than or equal to about 60 wt % at 25° C. may be greater than or equal to about 1000 mPa·s and less than or equal to about 5000 mPa·s, or, for example, greater than or equal to about 1500 mPa·s and less than or equal to about 4500 mPa·s. The viscosity of the negative electrode slurry can be adjusted by, for example, the amount of water-soluble polymer compound added.
[0107] (3-2. Negative Electrode Mixture Layer)
[0108] As described above, the negative electrode mixture layer is formed by applying the negative electrode slurry to one or both surfaces on the negative electrode collector and then drying and pressing the negative electrode slurry.
[0109] In the drying process, the solvent for the negative electrode slurry is volatilized, and the solid components (such as the negative electrode active material and the negative electrode binder) dispersed in the negative electrode slurry remain on the negative electrode current collector to form a negative electrode mixture layer. The content ratio of each component in the negative electrode mixture layer actually reflects the content ratio of the solid components in the negative electrode slurry.
[0110] The negative electrode mixture layer may have a value greater than or equal to about 3.5 mAh / cm after pressing. 2 and less than or equal to about 10 mAh / cm 2 area capacity.
[0111] When such a negative electrode mixture layer is formed, for example, the amount of the negative electrode mixture may be about 5 mg / cm or more. 2 and less than or equal to about 25 mg / cm 2 or, for example, greater than or equal to about 10 mg / cm 2 and less than or equal to about 20 mg / cm 2 The negative electrode slurry mentioned above is coated as the surface density of a single surface. In addition, the thickness of the negative electrode mixture layer after drying and pressing can be the thickness of one surface, for example, greater than or equal to about 50 μm and less than or equal to about 150 μm. The charge / discharge capacity of the rechargeable lithium ion battery can be increased by making the coating amount and thickness of the negative electrode mixture layer within these ranges.
[0112] On the other hand, the negative electrode mixture layer may further include a conductive agent. As the conductive agent, for example, the conductive agent exemplified as used for the positive electrode can be used.
[0113] <4. Effects of the Embodiment>
[0114] According to the negative electrode slurry, the negative electrode mixture layer, and the negative electrode formed of the negative electrode slurry configured as described above, the following effects can be obtained.
[0115] Since the binder includes a particle dispersion and a water-soluble polymer including an acrylic acid-acrylonitrile copolymer, and the content of the water-soluble polymer is greater than or equal to about 0.5 wt % and less than or equal to about 2 wt % based on 100 wt % of the total mass of the negative electrode active material and the binder, even if the negative electrode active material contains silicon atoms, expansion of the negative electrode can be sufficiently suppressed, and at the same time, cracks can be suppressed during coating and drying of the negative electrode slurry.
[0116] As described in the Examples, when a 3.5 mAh / cm 2 When the negative electrode mixture layer has an area capacity of 1000 μm or when a cylindrical battery is formed, the aforementioned effect is particularly significantly exhibited.
[0117] Hereinafter, the present invention will be described in detail using specific examples. However, the following examples are merely examples of the present invention, and the present invention is not limited to the following examples.
[0118] In this embodiment, acrylic acid-acrylonitrile copolymers A to E were first synthesized. Subsequently, these acrylic acid-acrylonitrile copolymers A to E were used to prepare negative electrode slurries, and the negative electrode slurries were used to manufacture rechargeable battery cells according to Examples 1 to 14 and Comparative Examples 1 to 8, and the rechargeable battery cells were evaluated. Hereinafter, each example and comparative example are shown.
[0119] <Synthesis of acrylic acid-acrylonitrile copolymer>
[0120] First, acrylic acid-acrylonitrile copolymers AE having respective compositions shown in Table 1 were synthesized.
[0121] (Table 1)
[0122]
[0123] In Table 1, AA represents acrylic acid, and AN represents acrylonitrile. In addition, the monomer implantation ratio shown in Table 1 is directly reflected in the content ratio of each monomer-derived unit in each acrylic acid-acrylonitrile-based copolymer after synthesis.
[0124] The specific synthesis sequence of acrylic acid-acrylonitrile copolymers A to E is as follows.
[0125] (Synthesis of acrylic acid-acrylonitrile copolymer A)
[0126] In a 2000mL detachable flask equipped with a mechanical stirrer, a stirring rod and a thermometer, 114.0g of acrylic acid, 76.0g of acrylonitrile, 158.2mL of 4mol / L sodium hydroxide aqueous solution, 107.77g of 10wt% ammonia water and 705.5g of ion exchange water were added, and then stirred at 400rpm, and after the system was internally replaced with nitrogen and the jacket temperature was set to 85°C, its temperature was raised. When the system temperature reached 60°C, an initiator aqueous solution prepared by dissolving 2608mg of 2,2'-azobis(2-methyl-N-2-hydroxyethylpropionamide) in 26.0g of ion exchange water was added thereto. At a jacket temperature of 85°C, the above-mentioned initiator was added thereto, and then stirred continuously for 12 hours to obtain a light yellow polymer aqueous solution. After the reaction, when the non-volatile components of the aqueous solution were measured, the result was 16.0wt%.
[0127] Subsequently, the reaction solution was concentrated by heating and distillation under reduced pressure to remove unreacted monomers, to which ammonia water and ion exchange water were added to adjust the concentration and pH of the polymer aqueous solution to obtain an acrylic acid-acrylonitrile copolymer A aqueous solution including 8 wt % of the polymer and having a pH of 7.5 (viscosity of 8 wt % polymer aqueous solution = 2160 mPa·s when measured by a B-type viscometer at 25° C. and 30 rpm). On the other hand, the concentration of the polymer aqueous solution was calculated by the mass of the non-volatile component in a state where the unreacted monomers were removed.
[0128] (Synthesis of acrylic acid-acrylonitrile copolymer B)
[0129] In a 2000 mL detachable flask equipped with a mechanical stirrer, a stirring rod and a thermometer, 80.0 g of acrylic acid, 80.0 g of acrylonitrile, 222.0 mL of a 4 mol / L sodium hydroxide aqueous solution and 592.0 g of ion exchange water were added, followed by stirring at 400 rpm, and after internally replacing the system with nitrogen and setting the jacket temperature to 85°C, the temperature was increased.
[0130] When the system temperature reached 60°C, an initiator aqueous solution prepared by dissolving 2642 mg of 2,2'-azobis(2-methyl-N-2-hydroxyethylpropionamide) in 26.0 g of ion exchange water was added thereto. At a jacket temperature of 85°C, after adding the above initiator, the obtained mixture was continuously stirred for 12 hours to obtain a light yellow polymer aqueous solution. After the reaction, when the non-volatile component of the aqueous solution was measured, the result was 16.1 wt%.
[0131] Subsequently, the reaction solution was concentrated by heating and distillation under reduced pressure to remove unreacted monomers, and aqueous ammonia and ion-exchanged water were added thereto to adjust the concentration and pH of the polymer aqueous solution to obtain an acrylic acid-acrylonitrile copolymer B aqueous solution including 8 wt % of the polymer and having a pH of 7.5 (when measured by a B-type viscometer at 25° C. and 30 rpm, the viscosity of the 8 wt % polymer aqueous solution = 2020 mPa·s).
[0132] (Synthesis of acrylic acid-acrylonitrile copolymer C)
[0133] In a 2000mL detachable flask equipped with a mechanical stirrer, a stirring rod and a thermometer, 128.0g of acrylic acid, 32.0g of acrylonitrile, 177.6mL of 4mol / L sodium hydroxide aqueous solution, 121.0g of 10wt% ammonia water and 541.4g of ion exchange water were added, and then stirred at 400rpm, and after the system was internally replaced with nitrogen and the jacket temperature was set to 85°C, its temperature was raised. When the system temperature reached 60°C, an initiator aqueous solution prepared by dissolving 2744mg of 2,2'-azobis(2-methyl-N-2-hydroxyethylpropionamide) in 26.0g of ion exchange water was added thereto. At a jacket temperature of 85°C, after adding the above-mentioned initiator, the obtained mixture was continuously stirred for 12 hours to obtain a yellow polymer aqueous solution. After the reaction, when the non-volatile components of the aqueous solution were measured, the result was 16.5wt%.
[0134] Subsequently, the reaction solution was concentrated by heating and distillation under reduced pressure to remove unreacted monomers, and aqueous ammonia and ion-exchanged water were added thereto to adjust the concentration and pH of the polymer aqueous solution to obtain an acrylic acid-acrylonitrile copolymer C aqueous solution including 8 wt % of the polymer and having a pH of 7.5 (when measured by a B-type viscometer at 25° C. and 30 rpm, the viscosity of the 8 wt % polymer aqueous solution = 1840 mPa·s).
[0135] (Synthesis of acrylic acid-acrylonitrile copolymer D)
[0136] In a 2000mL detachable flask equipped with a mechanical stirrer, a stirring rod and a thermometer, 48.0g of acrylic acid, 112.0g of acrylonitrile, 133.2mL of a 4mol / L sodium hydroxide aqueous solution and 670.8g of ion exchange water were added, and then stirred at 400rpm, and after the system was internally replaced with nitrogen and the jacket temperature was set to 85°C, its temperature was raised. When the system temperature reached 60°C, an initiator aqueous solution prepared by dissolving 3600mg of 2,2'-azobis(2-methyl-N-2-hydroxyethylpropionamide) in 36.0g of ion exchange water was added thereto. At a jacket temperature of 85°C, after adding the above-mentioned initiator, the obtained mixture was continuously stirred for 12 hours to obtain a yellow polymer suspension. After the reaction, when the non-volatile components of the suspension were measured, the result was 15.5wt%.
[0137] Subsequently, the reaction solution was concentrated by heating and distillation under reduced pressure to remove unreacted monomers, and aqueous ammonia and ion-exchanged water were added thereto to adjust the concentration and pH of the polymer suspension to obtain an acrylic acid-acrylonitrile copolymer D aqueous suspension including 8 wt % of the polymer and having a pH of 7.5 (when measured by a B-type viscometer at 25° C. and 30 rpm, the viscosity of the 8 wt % polymer aqueous suspension = 1520 mPa·s).
[0138] (Synthesis of acrylic acid-acrylonitrile copolymer E)
[0139] In a 2000mL detachable flask equipped with a mechanical stirrer, a stirring rod and a thermometer, 30.0g of acrylic acid, 20.0g of acrylonitrile, 27.75mL of 4mol / L sodium hydroxide aqueous solution, 28.36g of 10wt% ammonia water and 883.9g of ion exchange water were added, and then stirred at 400rpm, and after the system was internally replaced with nitrogen and the jacket temperature was set to 85°C, its temperature was raised. When the system temperature reached 60°C, an initiator aqueous solution prepared by dissolving 944mg of 2,2'-azobis(2-methyl-N-2-hydroxyethylpropionamide) in 10.0g of ion exchange water was added thereto. At a jacket temperature of 85°C, after adding the above initiator, the obtained mixture was continuously stirred for 12 hours to obtain a yellow polymer aqueous solution. After the reaction, when the non-volatile components of the aqueous solution were measured, the result was 4.9wt%.
[0140] Subsequently, the reaction solution was concentrated by heating and distillation under reduced pressure to remove unreacted monomers, and aqueous ammonia and ion-exchanged water were added thereto to adjust the concentration and pH of the polymer aqueous solution to obtain an aqueous solution of acrylic acid-acrylonitrile copolymer E including 8 wt % of the polymer and having a pH of 7.5 (when measured by a B-type viscometer at 25° C. and 30 rpm, the viscosity of the 8 wt % polymer aqueous solution = 250 mPa·s).
[0141] <Example 1>
[0142] A rechargeable lithium-ion battery cell was manufactured as follows.
[0143] (Manufacturing of negative electrode)
[0144] 15.0 g of a silicon-carbon composite active material as a Si-based active material, 85.0 g of an artificial graphite active material as a graphite-based active material, 1.042 g of acetylene black, 14.32 g of an 8.0 wt % aqueous solution of an acrylic acid-acrylonitrile copolymer A, 41.67 g of an aqueous solution including 1.0 wt % of a sodium salt of carboxymethyl cellulose (CMC) and 35.60 g of ion exchange water were mixed, and then 3.91 g of a 40 wt % aqueous dispersion of a particle dispersion a (average particle size of 170 nm) from a modified styrene butadiene copolymer having a glass transition temperature of -15°C was added thereto to prepare a negative electrode slurry.
[0145] Subsequently, the negative electrode slurry was coated on both surfaces of a copper foil as a negative electrode collector by using a reverse roll coater and dried so that the negative electrode mixture layer could have a surface area of 10.3 mg / cm 2 Then, the negative electrode mixture layer was pressed using a roll press to have a density of 1.65 g / cc, and a negative electrode having a density of 4.9 mAh / cm 2 The area capacity of the negative electrode.
[0146] (Manufacturing of positive electrode)
[0147] Li 1.0 Ni 0.88 Co 0.1 Al 0.01 Mg 0.01 O2, acetylene black and polyvinylidene fluoride were dispersed in N-methyl-2-pyrrolidone, a solvent for positive electrode slurry, at a mass powder ratio of 97.7:1.0:1.3 to prepare a positive electrode slurry.
[0148] Subsequently, the slurry was coated and dried on one surface of an aluminum foil as a current collector using a reverse roll coater so that the positive electrode mixture layer could have a carbon content of 24.0 mg / cm 2 (area density), and then pressed using a roll press to have a mixture layer density of 3.65 g / cc, thereby manufacturing a positive electrode.
[0149] (Manufacturing of rechargeable battery cells)
[0150] After welding each nickel and aluminum lead to the aforementioned negative electrode and positive electrode, a polyethylene porous separator is provided to produce an electrode laminate formed by inserting one negative electrode between two positive electrodes. Subsequently, the electrode laminate is stored in an aluminum laminate film with the lead pulled out, and after injecting an electrolyte solution therein, the aluminum laminate film is sealed under reduced pressure, manufacturing a rechargeable battery cell before initial charging.
[0151] The electrolyte was prepared by dissolving 1.3 M LiPF6 and 1 wt% vinylene carbonate in a mixed solvent of ethylene carbonate / dimethyl carbonate / fluoroethylene carbonate in a volume ratio of 15 / 80 / 5.
[0152] (Manufacturing of Metal Lithium Counter Electrode Unit)
[0153] A metal lithium counter electrode unit before initial charge was manufactured according to the same procedure as above except that the cross-sectional positive electrode was changed to a metal lithium bonded copper foil.
[0154] <Example 2>
[0155] A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as that of Example 1, except that the acrylic acid-acrylonitrile based copolymer B was used instead of the acrylic acid-acrylonitrile based copolymer A in the process of manufacturing a negative electrode of Example 1.
[0156] <Example 3>
[0157] A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as that of Example 1, except that particle dispersion b (average particle size of 180 nm) obtained from a modified styrene butadiene copolymer having a glass transition temperature of 9°C was used instead of particle dispersion a in the process of manufacturing the negative electrode of Example 1.
[0158] <Example 4>
[0159] A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as that of Example 1, except that acrylic acid-acrylonitrile copolymer B was used instead of acrylic acid-acrylonitrile copolymer A and particle dispersion b was used instead of particle dispersion a in the process of manufacturing the negative electrode of Example 1.
[0160] <Example 5>
[0161] In the method of manufacturing the negative electrode of Example 4, 15.0 g of a silicon-carbon composite active material, 85.0 g of an artificial graphite active material, 1.042 g of acetylene black, 26.04 g of an aqueous solution including 8.0 wt% of an acrylic acid-acrylonitrile copolymer A, and 49.92 g of ion exchange water were mixed, and 2.60 g of a 40 wt% aqueous dispersion of a particle dispersion a was added thereto to prepare a negative electrode slurry. A rechargeable battery cell and a metal lithium counter electrode cell were manufactured using the negative electrode slurry according to the same procedure as that of Example 1.
[0162] <Example 6>
[0163] A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as that of Example 5, except that the acrylic acid-acrylonitrile based copolymer B was used instead of the acrylic acid-acrylonitrile based copolymer A in the process of manufacturing the negative electrode of Example 5.
[0164] <Example 7>
[0165] A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as that of Example 5, except that the particle dispersion b was used instead of the particle dispersion a in the process of manufacturing the negative electrode of Example 5.
[0166] <Example 8>
[0167] A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as that of Example 5, except that acrylic acid-acrylonitrile copolymer B was used instead of acrylic acid-acrylonitrile copolymer A and particle dispersion b was used instead of particle dispersion a in the process of manufacturing the negative electrode of Example 5.
[0168] <Comparative Example 1>
[0169] In the process of manufacturing the negative electrode of Example 1, 15.0 g of a silicon-carbon composite active material, 85.0 g of an artificial graphite active material, 1.042 g of acetylene black, 62.5 g of an aqueous solution including 5 wt % of polyacrylic acid sodium salt, and 40.71 g of ion exchange water were mixed to prepare a negative electrode slurry. The negative electrode slurry was coated and dried on a copper foil in the same process as that of Example 1, but the negative electrode mixture layer formed therefrom was cracked during coating and drying, and a rechargeable battery cell and a metal lithium counter electrode cell could not be manufactured.
[0170] <Comparative Example 2>
[0171] In the process of manufacturing the negative electrode of Example 1, 15.0 g of a silicon-carbon composite active material, 85.0 g of an artificial graphite active material, 1.042 g of acetylene black (, 39.06 g of an 8.0 wt % aqueous solution of acrylic acid-acrylonitrile copolymer A, and 52.80 g of ion exchange water were mixed to prepare a negative electrode slurry. The negative electrode slurry was coated on a copper foil and dried in the same procedure as in Example 1, but the negative electrode mixture layer formed therefrom was cracked during coating and drying, and a rechargeable battery cell and a metal lithium counter electrode cell could not be manufactured.
[0172] <Comparative Example 3>
[0173] In the process of manufacturing the negative electrode of Example 1, 15.0 g of a silicon-carbon composite active material, 85.0 g of an artificial graphite active material, 1.042 g of acetylene black, 39.06 g of an aqueous solution including 8.0 wt % of an acrylic acid-acrylonitrile copolymer B, and 52.80 g of ion exchange water were mixed to prepare a negative electrode slurry. The negative electrode slurry was coated and dried on a copper foil in the same procedure as that of Example 1, but the negative electrode mixture layer formed therefrom was cracked during coating and drying, and a rechargeable battery cell and a metal lithium counter electrode cell could not be manufactured.
[0174] <Comparative Example 4>
[0175] In the process of manufacturing the negative electrode of Example 1, 15.0 g of a silicon-carbon composite active material, 85.0 g of an artificial graphite active material, 1.042 g of acetylene black, 19.53 g of an aqueous solution including 8.0 wt % of an acrylic acid-acrylonitrile copolymer A, 104.17 g of an aqueous solution including 1.5 wt % of carboxymethyl cellulose (CMC), and 6.74 g of ion exchange water were mixed to prepare a negative electrode slurry. The negative electrode slurry was coated and dried on a copper foil in the same process as that of Example 1, but the negative electrode mixture layer formed thereof was broken during coating and drying, and a rechargeable battery cell and a metal lithium counter electrode cell could not be manufactured.
[0176] <Comparative Example 5>
[0177] In the method for manufacturing a negative electrode of Example 1, 15.0 g of a silicon-carbon composite active material, 85.0 g of an artificial graphite active material, 1.042 g of acetylene black, 19.53 g of an aqueous solution including 8.0 wt % of an acrylic acid-acrylonitrile copolymer B, 104.17 g of an aqueous solution including 1.5 wt % of carboxymethyl cellulose (CMC), and 6.74 g of ion exchange water were mixed to prepare a negative electrode slurry. The negative electrode slurry was coated and dried on a copper foil in the same process as that of Example 1, but the negative electrode mixture layer formed thereof was broken during coating and drying, and a rechargeable battery cell and a metal lithium counter electrode cell could not be manufactured.
[0178] <Comparative Example 6>
[0179] In the method for manufacturing the negative electrode of Example 1, 15.0 g of a silicon-carbon composite active material, 85.0 g of an artificial graphite active material, 1.042 g of acetylene black, 104.16 g of an aqueous solution including 1.5 wt % of carboxymethyl cellulose (CMC), and 49.92 g of ion exchange water were mixed, and 3.91 g of a 40 wt % aqueous dispersion of particle dispersion a was added thereto to prepare a negative electrode slurry. A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as that of Example 1 except that the composition of the negative electrode slurry was changed.
[0180] <Comparative Example 7>
[0181] In the process of manufacturing the negative electrode of Example 1, 15.0 g of a silicon-carbon composite active material, 85.0 g of an artificial graphite active material, 1.042 g of acetylene black, 104.16 g of an aqueous solution including 1.5 wt % of carboxymethyl cellulose (CMC), and 49.92 g of ion exchange water were mixed, and 3.91 g of a 40 wt % aqueous dispersion of particle dispersion b was added thereto to prepare a negative electrode slurry. A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as that of Example 1 except that the composition of the negative electrode slurry was changed.
[0182] <Comparative Example 8>
[0183] In the method for manufacturing the negative electrode of Example 1, 15.0 g of a silicon-carbon composite active material, 85.0 g of an artificial graphite active material, 1.042 g of acetylene black, 22.92 g of an aqueous solution including 5 wt % of polyacrylic acid sodium salt, 41.67 g of an aqueous solution including 1.0 wt % of carboxymethyl cellulose (CMC), and 52.09 g of ion exchange water were mixed, and 3.91 g of a 40 wt % aqueous dispersion of particle dispersion a was added thereto to prepare a negative electrode slurry. A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as that of Example 1 except that the composition of the negative electrode slurry was changed.
[0184] <Example 9>
[0185] A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as that of Example 1, except that the acrylic acid-acrylonitrile based copolymer C was used instead of the acrylic acid-acrylonitrile based copolymer A in the process of manufacturing the negative electrode of Example 1.
[0186] <Example 10>
[0187] A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as that of Example 1, except that the acrylic acid-acrylonitrile based copolymer D was used instead of the acrylic acid-acrylonitrile based copolymer A in the process of manufacturing a negative electrode of Example 1.
[0188] <Example 11>
[0189] In the process of manufacturing the negative electrode of Example 1, 15.0 g of silicon-carbon composite active material, 85.0 g of artificial graphite active material, 1.042 g of acetylene black, 14.32 g of an aqueous solution including 8.0 wt% of acrylic acid-acrylonitrile copolymer E, 41.67 g of an aqueous solution including 5 wt% of polyacrylic acid sodium salt, 41.67 g of an aqueous solution including 1.0 wt% of carboxymethyl cellulose (CMC) and 18.66 g of ion exchange water were mixed, and 3.91 g of 40 wt% of an aqueous dispersion of particle dispersion a was added thereto to prepare a negative electrode slurry. A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as that of Example 1 except that the composition of the negative electrode slurry was changed.
[0190] <Example 12>
[0191] A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as in Example 1, except that a particle dispersion c (average particle size of 180 nm) made of a modified styrene butadiene copolymer having a glass transition temperature of -35°C was used instead of a particle dispersion a in the process of manufacturing the negative electrode in Example 1.
[0192] <Example 13>
[0193] A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as in Example 1, except that a particle dispersion d (average particle size of 180 nm) made of a modified styrene butadiene copolymer having a glass transition temperature of -50°C was used instead of a particle dispersion a in the process of manufacturing the negative electrode in Example 1.
[0194] <Example 14>
[0195] A rechargeable battery cell and a metal lithium counter electrode cell were manufactured according to the same procedure as in Example 1, except that in the process of manufacturing the negative electrode in Example 1, the amount of the aqueous solution including 8.0 wt % of acrylic acid-acrylonitrile copolymer A was changed to 6.48 g, the amount of the aqueous solution including 1.0 wt % of sodium salt of carboxymethyl cellulose (CMC) was changed to 51.87 g, and the amount of the aqueous dispersion of 40 wt % of particle dispersion a was changed to 4.15 g.
[0196] <Evaluation of Negative Electrode Slurry, Negative Electrode, and Rechargeable Battery Cell>
[0197] (Coating suitability)
[0198] The coating suitability of Examples 1 to 14 and Comparative Examples 1 to 8 was evaluated by checking whether cracks occurred in the negative electrode mixture layer in the process of coating and drying the negative electrode slurry on the copper foil. The evaluation criteria are as follows.
[0199] ○: No cracks
[0200] ×: Cracks appear
[0201] (Viscosity change)
[0202] The viscosity stability of Examples 1 to 14 and Comparative Examples 1 to 8 was evaluated by comparing the viscosity of the negative electrode slurry just after preparation with the viscosity of the negative electrode slurry after stirring at 40 rpm at room temperature while storing for 24 hours. On the other hand, the slurry viscosity (unit: mPa·s) was measured by using a B-type viscometer while stirring at 25° C. and 30 rpm. The evaluation criteria are as follows.
[0203] ○: The viscosity of the slurry changes within the range of 50% to 150% immediately after preparation and after 24 hours of storage
[0204] △: The change in slurry viscosity immediately after preparation and after 24 hours of storage is 150% or more
[0205] (Close contact properties)
[0206] The negative electrodes according to Examples 1 to 14 and Comparative Examples 1 to 8 were cut into rectangles with a width of 25 mm and a length of 100 mm. Subsequently, the active material side of each cut negative electrode was attached to a stainless steel plate using a double-sided tape to prepare a sample for evaluating the close contact property. The sample was mounted on a peel tester (EZ-S, SHIMAZU Corp.) and the 180° peel strength was measured.
[0207] (Expansion rate of negative electrode after first charge)
[0208] The metal lithium counter electrode units according to Examples 1 to 14 and Comparative Examples 6 to 8 were charged to 0.005V at a constant current of 0.1CA (1CA = 1 hour discharge rate) at a designed capacity in a 25°C thermostat, and were continuously charged to 0.01CA at 0.005V. Subsequently, the battery was disassembled to remove the negative electrode, and the thickness of each negative electrode was measured with a micrometer, and then compared with the thickness of the negative electrode before the first charge (before the electrolyte was injected) to evaluate the expansion rate of the negative electrode. Here, the expansion rate is calculated by ((negative electrode thickness after charging)-(negative electrode thickness before charging) / (negative electrode thickness before charging)×100%.
[0209] (Peeling off of negative electrode mixture layer after first charge)
[0210] In the aforementioned evaluation of the expansion rate of the negative electrode after the first charge, the negative electrode taken out after the first charge was visually inspected and evaluated according to the following criteria.
[0211] ○: The negative electrode mixture layer was not peeled off from the copper foil substrate
[0212] △: A portion of the negative electrode mixture layer peels off from the bottom of the copper foil substrate
[0213] ×: The entire negative electrode mixture layer is peeled off from the copper foil substrate
[0214] (Cycle Characteristics)
[0215] The rechargeable battery cells according to Examples 1 to 4 and Comparative Examples 3 to 5 were charged to 4.3V at a constant current of 0.1CA in a 25°C thermostat, and continuously charged to 0.05CA at a constant voltage of 4.3V. Subsequently, the cells were discharged to 2.5V at a constant current of 0.1CA. In addition, in a 25°C thermostat, the first cycle was performed by performing a constant current charge of 0.2CA, a constant voltage charge of 0.05CA, and a constant current discharge of 0.2CA at a discharge cutoff voltage of 2.5V and a charge cutoff voltage of 4.3V to measure the initial discharge capacity.
[0216] The cycle life of these rechargeable battery cells was tested by performing 100 cycles of 0.5CA constant current charge, 0.05CA constant voltage charge, and 0.5CA constant current discharge at 25° C. at a charge cutoff voltage of 4.3 V and a discharge cutoff voltage of 2.5 V. After 100 cycles of 0.2CA constant current charge, 0.05CA constant voltage charge, and 0.2CA constant current discharge, the discharge capacity was measured and then divided by the initial discharge capacity to obtain the capacity retention rate after 100 cycles.
[0217] (Evaluation results)
[0218] The evaluation results of Examples 1 to 14 and Comparative Examples 1 to 8 are shown in Tables 2 and 3.
[0219] (Table 2)
[0220]
[0221]
[0222] (Table 3)
[0223]
[0224] (Consideration on Results of Examples and Comparative Examples)
[0225] First, as shown in Table 2 and Table 3, in Comparative Example 1 using the negative electrode binder made of a polyacrylic acid homopolymer, the negative electrode mixture layer was broken in the coating / drying process of the negative electrode slurry, and a practically applicable negative electrode could not be obtained.
[0226] Since polyacrylic acid is known to have a high elastic modulus but insufficient flexibility, sufficient flexibility required for the negative electrode mixture layer was not obtained. This is also inferred from the fact that the close contact property after pressing was greatly deteriorated in Table 3.
[0227] In Comparative Examples 2 to 3 using acrylic acid-acrylonitrile copolymer alone as the negative electrode binder, as in Comparative Example 1, the negative electrode mixture layer was broken during the coating / drying process of the negative electrode slurry, and a practically applicable negative electrode could not be obtained.
[0228] Also, in Comparative Examples 4 and 5 using the water-soluble polymer including the acrylic acid-acrylonitrile-based copolymer and CMC, the problem of cracks generated during the coating / drying process of the negative electrode slurry was not improved.
[0229] Referring to Table 3, Comparative Examples 2 to 5 also showed that the close contact property after pressing was greatly deteriorated, and thus, as in Comparative Example 1, as a result, sufficient flexibility required as a negative electrode mixture layer could not be ensured.
[0230] In addition, as shown in Table 3, Comparative Examples 6 to 8 not using the acrylic acid-acrylonitrile copolymer showed that the negative electrode expansion ratio increased to more than 43% after the first charge, and the capacity retention ratio was less than 76% after 100 cycles.
[0231] Referring to these results, the negative electrode slurries according to Comparative Examples 6 to 8 do not include acrylic acid-acrylonitrile copolymers, and thus cannot sufficiently suppress expansion of the negative electrode, resulting in deterioration of cycle life. In addition, in the comparative examples, the negative electrode mixture layer is easily peeled off after the first charge.
[0232] On the other hand, in Examples 1 to 14 of the specific examples of the present invention, as shown in Table 3, the aforementioned problem of crack generation is solved by using a water-soluble polymer including an acrylic acid-acrylonitrile copolymer and a particle dispersion, and also limiting the content of the water-soluble polymer to a predetermined range.
[0233] The reason is that the flexibility of the negative electrode mixture layer is improved to a practically applicable level by limiting the content of the water-soluble polymer including the acrylic acid-acrylonitrile copolymer within a predetermined range to prepare the negative electrode binder.
[0234] On the other hand, in Examples 1 to 14, the content of the water-soluble polymer is in the range of 1.0 wt % to 2.0 wt % based on 100 wt % of the total mass of the negative electrode active material and the binder, but the present invention is not limited thereto, and it is demonstrated that even if the content of the water-soluble polymer is 0.5 wt %, the negative electrode expansion is sufficiently suppressed.
[0235] In addition, comparing Examples 1 to 14 with Comparative Examples 6 to 8, the negative electrode was sufficiently suppressed from swelling accompanying charging while exhibiting excellent cycle characteristics, thereby suppressing capacity degradation of the battery according to repeated charge and discharge cycles. In addition, the peeling of the negative electrode mixture layer after the first charge in Examples 1 to 14 was suppressed.
[0236] Although Examples 9 to 14 fully exhibited the effects of the present invention, as shown in Table 3, Examples 1 to 8 exhibited excellent performance in all items as rechargeable batteries.
[0237] Referring to these results, the copolymerization ratios of acrylic acid and acrylonitrile in the acrylic acid-acrylonitrile copolymer, the viscosity of the aqueous solution including each acrylic acid-acrylonitrile copolymer, the viscosity of the negative electrode slurry, etc. are designed within appropriate ranges, thereby enhancing the effects of suppressing the expansion of the negative electrode, improving the cycle life, and suppressing the peeling of the negative electrode mixture layer.
[0238] Additionally, when the glass transition temperature of the particle dispersion is greater than or equal to about -30°C and less than or equal to about 20°C, the stability of the slurry over time is improved.
[0239] In Examples 1 to 14, even though the coating area capacity is 4.9 mAh / cm 2 , crack generation was also sufficiently suppressed, but it was proved that when the negative electrode slurries of Examples 1 to 14 were used, at 10 mAh / cm 2 There are almost no cracks within the area capacity range.
[0240] While the present invention has been described in conjunction with what are presently considered to be practical example embodiments, it is to be understood that the invention is not limited to the disclosed embodiments, but is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.
Claims
1. A negative electrode slurry, comprising: a negative electrode active material including a first active material containing silicon atoms in an amount greater than or equal to 5 wt % and less than or equal to 100 wt %; A binder, used to bind the negative electrode active material; as well as Solvent used in negative electrode slurry to disperse negative electrode active material and binder. wherein the first active material contains silicon atoms in an amount greater than or equal to 20 wt % and less than or equal to 100 wt %, The binder comprises a particle dispersion and a water-soluble polymer, the water-soluble polymer comprises a copolymer comprising a (meth)acrylic acid monomer and a (meth)acrylonitrile monomer, When the total amount of the negative electrode active material and the binder is 100 wt %, the content of the water-soluble polymer is greater than or equal to 0.5 wt % and less than or equal to 2 wt %, and The particle dispersion includes a copolymer comprising units derived from styrene monomers and units derived from butadiene monomers.
2. The negative electrode slurry according to claim 1, wherein The solvent used for the negative electrode slurry is an aqueous solvent.
3. The negative electrode slurry according to claim 1, wherein The first active material includes at least one active material selected from a mixture of silicon or silicon oxide particles combined with graphite carbon or amorphous carbon, silicon particles, and a silicon-based alloy.
4. The negative electrode slurry according to claim 1, wherein The copolymer includes (meth)acrylic acid-based monomer-derived units in an amount of greater than or equal to 40 wt % and less than or equal to 70 wt % and (meth)acrylonitrile-based monomer-derived units in an amount of greater than or equal to 30 wt % and less than or equal to 60 wt %.
5. The negative electrode slurry according to claim 1, wherein The copolymer further includes units derived from other monomers copolymerizable with the (meth)acrylic acid-based monomer-derived units and / or the (meth)acrylonitrile-based monomer-derived units.
6. The negative electrode slurry according to claim 1, wherein: The water-soluble polymer includes the copolymer in an amount greater than or equal to 50 wt %.
7. The negative electrode slurry according to claim 1, wherein: The (meth)acrylic acid-based monomer includes at least one selected from (meth)acrylic acid, a metal salt of (meth)acrylic acid, an ammonium salt of (meth)acrylic acid, and an amine salt of (meth)acrylic acid.
8. The negative electrode slurry according to claim 1, wherein An 8 wt % aqueous solution of the acrylic acid-acrylonitrile copolymer has a viscosity at 25° C. of 500 mPa·s or more and 10000 mPa·s or less.
9. The negative electrode slurry according to claim 1, wherein: The particle dispersion includes a polymer having a glass transition temperature greater than or equal to -30°C and less than or equal to 20°C.
10. The negative electrode slurry according to claim 1, wherein: The water-soluble polymers also include cellulose ethers containing carboxymethyl groups or salts of cellulose ethers containing carboxymethyl groups.
11. The negative electrode slurry according to claim 1, wherein: The negative electrode slurry has a viscosity of greater than or equal to 1000 mPa·s and less than or equal to 5000 mPa·s at a solid content concentration of greater than or equal to 45 wt % and less than or equal to 60 wt % at 25° C.
12. The negative electrode slurry according to claim 1, wherein: The negative electrode active material further includes a graphite-based active material as a second active material. 13 . The negative electrode slurry according to claim 1 , further comprising a conductive agent. 14 . A negative electrode comprising the solid component of the negative electrode slurry according to claim 1 .
15. The negative electrode according to claim 14, wherein The area capacity of the negative electrode is greater than or equal to 3.5 mAh / cm 2 And less than or equal to 10mAh / cm 2 . 16 . A rechargeable battery comprising the negative electrode according to claim 14 .