A NCM811 positive electrode material precursor and its preparation method and application
By uniformly mixing the spherical precursor particles of large and small particle size in high nickel ternary layered materials, and solubilization method is used to regulate the particle size, the problem of insufficient stacking density of high nickel ternary materials is solved, and the material is improved cyclic stability and rate performance.
Patent Information
- Application Number
- CN202210060895.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-19
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-01-19
AI Technical Summary
The modification of high-nickel ternary layered materials has reached a bottleneck, and the stacking density of monodispersed spherical secondary particles on the positive electrode current collector is limited by the stacking method, making it difficult to further improve storage performance.
By uniformly mixing large-sized spherical precursor particles and small-sized spherical precursor particles, the particle size ratio is 0.16-0.40, the particle size is adjusted by solvothermal method to improve the bulk density and electrochemical properties of the material.
Higher bulk density, cycle stability and rate performance are achieved, which slows down the collapse of the material during the cycle and shortens the distance between charged particles and current collectors.
Smart Images

Figure CN114455646B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery positive electrode material preparation, and specifically relates to an NCM811 positive electrode material precursor and a preparation method and application thereof. Background Art
[0002] The development of new energy vehicles, mobile electronic devices, artificial intelligence and other emerging industries requires the support of lithium-ion batteries. Therefore, people spare no effort to develop new lithium-ion battery materials, among which high-nickel ternary layered materials are currently the most promising lithium-ion battery cathode materials, because they have high energy density (629Wh / kg) and power density, and have excellent rate performance. High-nickel ternary materials have become a popular choice of lithium-ion battery materials in new energy smart cars, helping electric vehicles provide a range of more than 500km.
[0003] At present, the synthesis process of high nickel ternary materials is quite mature, among which LiNi 0.8 Co 0.1 Mn 0.1 O2, referred to as NCM811, is a typical high-nickel ternary material and the main product of major material suppliers. At the same time, researchers in the materials industry have reported their modification methods for NCM811, but many modification schemes have stopped in the laboratory due to their complexity and difficulty in industrialization. In recent years, the modification of high-nickel layered materials has reached a bottleneck, and the improvement of its storage performance will inevitably come at the cost of damaging its structure. The primary particles are agglomerated into spherical polycrystalline NCM811 secondary particles, which can shorten the distance of ion diffusion, thereby accelerating Li + The transmission of spherical particles has an effect on the rate performance of the battery. However, the packing density of monodisperse spherical secondary particles on the positive electrode current collector is limited by the stacking method. As we all know, the packing density of spheres has nothing to do with the particle size, but only with the stacking method. Even the three-dimensional hexagonal stacking and body-centered cubic stacking have a space utilization rate of only 74%. In addition, it is difficult to form the densest stacking during the coating process, and the packing density will further decrease. Therefore, the limitation of the packing density of monodisperse spherical secondary particles on the current collector needs to be improved. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, the present invention provides a NCM811 positive electrode material precursor and a preparation method and application thereof.
[0005] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a NCM811 positive electrode material precursor, the NCM811 positive electrode material precursor comprises large-diameter spherical precursor particles and small-diameter spherical precursor particles, the particle size ratio of the large-diameter spherical precursor particles to the small-diameter spherical precursor particles is 0.16-0.40, and the mass ratio is 0.9-1.1.
[0006] The present invention uniformly mixes two NCM811 spherical precursor particles with different particle sizes, so that the spherical secondary particles with small particle size fill as many gaps between the spherical particles with large particle size as possible, improve the space utilization of the active material on the current collector, and obtain the best packing density. In addition, the particle size ratio of the large-diameter spherical precursor particles and the small-diameter spherical precursor particles of the present invention is within 0.16-0.40, which can effectively improve the packing density of the material, make the secondary particles more compact, and the tightly arranged secondary particles can slow down the collapse of the material during the cycle, and shorten the diffusion distance of the charged particles to the current collector, thereby improving the cycle and rate performance of the NCM811 positive electrode material; the particle size ratio is less than 0.16 or greater than 0.40, which cannot effectively improve the packing density of the material.
[0007] The particle size ratio of the small-diameter spherical precursor particles to the large-diameter spherical precursor particles is 0.16-0.40; the mass ratio of the large-diameter spherical precursor particles to the small-diameter spherical precursor particles is 0.9-1.1.
[0008] The present invention also claims protection for a method for preparing the NCM811 positive electrode material precursor, wherein the preparation method is a solvothermal method; the solvothermal method adjusts the particle size of the NCM811 positive electrode material precursor by controlling the amount of organic solvent added.
[0009] As a preferred embodiment of the present invention, the solvothermal method comprises the following steps:
[0010] (1) preparing a metal salt in a molar ratio of Ni:Co:Mn=8:1:1 to form a solution A, dissolving a precipitant in water to form a solution B, and adding the solution B to the solution A and mixing them uniformly to obtain a solution C;
[0011] (2) Adding solution C into an organic solvent for hydrothermal reaction to obtain a NCM811 positive electrode material precursor; the volume ratio of the organic solvent to water is 0.5 to 5.
[0012] The water is the water in solution C.
[0013] The present invention adopts a solvothermal method to control the ratio of organic solvent to water in the system to regulate the particle size of the precursor, so that the particle size ratio of the large-diameter spherical precursor particles and the small-diameter spherical precursor particles of the present invention is 0.16-0.40, and the precursor particle size obtained by the above method is uniform, which is beneficial to improving the electrochemical performance of the positive electrode material.
[0014] Each particle in the system is a secondary particle composed of several cubic primary particles of equal volume. The smaller the particle, the fewer primary particles; the larger the particle, the more primary particles. In the solvent reaction of the present invention, too large a ratio of organic solvent to water will lead to too many crystal nuclei in the system and too small particle size; on the one hand, small particles are composed of only a few primary particles and are easy to disperse; on the other hand, small particles are easy to agglomerate into a very large mass.
[0015] As a preferred embodiment of the present invention, the organic solvent is polyethylene glycol 200, polyethylene glycol 400 or polyethylene glycol 600.
[0016] As a preferred embodiment of the present invention, in step (1), the metal salt is sulfate, acetate, nitrate or chloride.
[0017] As a preferred embodiment of the present invention, in step (1), the precipitant is urea, and the molar number of urea is 1.2-2 times the molar number of the metal salt.
[0018] The amount of urea used has almost no effect on the particle size of the precursor. Excessive use of urea will lead to excessive ammonia concentration in the solvent thermal reactor, causing the metal salt ions to form complexes, and the solubility product will increase sharply, resulting in some nickel ions being unable to be completely precipitated, thereby destroying the stoichiometric ratio of the NCM811 precursor. In addition, the urea content has a greater impact on the uniformity of the material particle size. The more urea is used, the worse the uniformity of the material particle size.
[0019] As a preferred embodiment of the present invention, in the step (2), the temperature of the hydrothermal reaction is 180 to 220° C., and the time of the hydrothermal reaction is 8 to 12 hours.
[0020] The present invention also claims to protect a NCM811 positive electrode material, which is prepared from the NCM811 positive electrode material precursor and a lithium salt.
[0021] As a preferred embodiment of the present invention, the NCM811 positive electrode material includes large-diameter spherical secondary particles and small-diameter spherical secondary particles, the particle size ratio of the large-diameter spherical secondary particles to the small-diameter spherical secondary particles is 0.16-0.40, and the mass ratio is 0.9-1.1.
[0022] The particle size ratio of the small-diameter spherical secondary particles to the large-diameter spherical secondary particles is 0.16-0.40; the mass ratio of the large-diameter spherical secondary particles to the small-diameter spherical secondary particles is 0.9-1.1.
[0023] The preparation method of the NCM811 positive electrode material comprises the following steps: mixing and grinding the NCM811 positive electrode material precursor and lithium salt, and then calcining for the first time; cooling and grinding, and then calcining for the second time to obtain the NCM811 positive electrode material.
[0024] The purpose of grinding after the first calcination in the present invention is to eliminate further agglomeration of secondary particles during the first calcination. Through the above preparation method, the particle size of the NCM811 positive electrode material precursor can remain unchanged.
[0025] As a preferred embodiment of the present invention, the mass ratio of the NCM811 positive electrode material precursor to the lithium salt is 1:1.05.
[0026] As a preferred embodiment of the present invention, the temperature of the first calcination is 480-500° C. and the time is 4-6 hours.
[0027] As a preferred embodiment of the present invention, the temperature of the second calcination is 750-780°C and the time is 12-18 hours.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The present invention uniformly mixes two NCM811 spherical precursor particles with different particle sizes so that the spherical secondary particles with a small particle size can fill as much of the gaps between the spherical particles with a large particle size as possible, thereby improving the space utilization of the active material on the current collector and obtaining the optimal stacking density. The secondary particles with a high stacking density can slow down the collapse of the material during the cycle and shorten the diffusion distance of the charged particles to the current collector, thereby improving the cycle stability and rate performance of the NCM811 positive electrode material.
[0030] (2) The present invention regulates the particle size of the precursor by controlling the amount of organic solvent added in the solvothermal method, and the obtained NCM811 spherical precursor has a uniform particle size, which is beneficial to improving the electrochemical performance of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A schematic diagram of the bidispersed stacking mode and particle size relationship of the NCM811 positive electrode material of the present invention;
[0032] Figure 2 (a) is a SEM image of the NCM811 cathode material precursor prepared in Example 1; Figure 2 (b) is the SEM image of the NCM811 positive electrode material prepared in Example 1;
[0033] Figure 3 (a) is a SEM image of the NCM811 cathode material precursor prepared in Comparative Example 1; Figure 3 (b) is the SEM image of the NCM811 positive electrode material prepared in Comparative Example 1;
[0034] Figure 4(a) is a SEM image of the NCM811 cathode material precursor prepared in Comparative Example 2; Figure 4 (b) is the SEM image of the NCM811 positive electrode material prepared in Comparative Example 2;
[0035] Figure 5 The normal distribution diagram of the stacking density of the positive electrode material in the positive sheet coated with the NCM811 positive electrode material prepared in Example 1 and Comparative Examples 1-2;
[0036] Figure 6 The figure is a comparison of the rate performance of the positive film coated with NCM811 positive electrode material prepared in Example 1 and Comparative Examples 1-2 at 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, and 10C rates respectively;
[0037] Figure 7 This is the 1C cycle performance diagram of the positive film coated with NCM811 positive electrode material prepared in Example 1 and Comparative Examples 1-2. DETAILED DESCRIPTION
[0038] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0039] Example 1
[0040] The method for preparing the NCM811 positive electrode material precursor in this embodiment comprises the following steps:
[0041] (1) Prepare 30 mL of 1 mol / L solution A with a stoichiometric ratio of Ni:Co:Mn=8:1:1, dissolve 0.036 mol of urea in water to prepare 10 mL of solution B, slowly dropwise add solution B to solution A to obtain solution C, and stir for 10 min;
[0042] (2) 20 mL of polyethylene glycol 200 was measured and added dropwise at a rate of 5 mL / min to the solution C in step (1) at a rotation speed of 500 rpm to obtain a solution D, and the solution D was transferred to a hydrothermal reactor and reacted at 200° C. for 12 h to obtain 6 μm NCM811 spherical precursor particles;
[0043] (3) The metal salt was prepared into 5 mL of 2 mol / L solution A according to the stoichiometric ratio of Ni:Co:Mn=8:1:1, and 0.012 mol of urea was dissolved in water to prepare 5 mL of solution B. Solution B was slowly added dropwise to solution A to obtain solution C, and stirred for 10 min.
[0044] (4) 50 mL of polyethylene glycol 400 was measured and added dropwise at a rate of 5 mL / min to the polyethylene glycol 400 at a speed of 500 rpm to obtain solution D, and solution D was transferred to a hydrothermal reactor and reacted at 200 °C for 12 h to obtain 2 μm NCM811 spherical precursor particles;
[0045] (5) The 6 μm NCM811 spherical precursor particles obtained in step (2) and the 2 μm NCM811 spherical precursor particles obtained in step (4) are mixed in a mass ratio of 1:1 to obtain a NCM811 positive electrode material precursor.
[0046] The method for preparing the NCM811 positive electrode material in this embodiment comprises the following steps:
[0047] The NCM811 cathode material precursor was mixed with lithium carbonate in a mass ratio of 1:1.05 and ground for 30 minutes, then transferred to a muffle furnace for the first calcination at 500°C for 6 hours, and then naturally cooled, ground for 10 minutes and transferred to a muffle furnace for calcination at 750°C for 18 hours in an air atmosphere to finally obtain a double-dispersed spherical NCM811 cathode material.
[0048] from Figure 2 It can be seen that the NCM811 cathode material of the present invention still maintains the spherical morphology and particle size of the precursor, including 6μm NCM811 spherical particles and 2μm NCM811 spherical particles, and the particle size ratio is 0.33.
[0049] Example 2
[0050] The method for preparing the NCM811 positive electrode material precursor in this embodiment comprises the following steps:
[0051] (1) Prepare 30 mL of 1 mol / L solution A with a stoichiometric ratio of Ni:Co:Mn=8:1:1, dissolve 0.036 mol of urea in water to prepare 10 mL of solution B, slowly dropwise add solution B to solution A to obtain solution C, and stir for 10 min;
[0052] (2) 20 mL of polyethylene glycol 200 was measured and added dropwise at a rate of 5 mL / min to the polyethylene glycol 200 at a rotation speed of 500 rpm to obtain solution D, and solution D was transferred to a hydrothermal reactor and reacted at 180° C. for 12 h to obtain 10 μm NCM811 spherical precursor particles;
[0053] (3) The metal salt was prepared into 30 mL of 1 mol / L solution A according to the stoichiometric ratio of Ni:Co:Mn=8:1:1, and 0.036 mol of urea was dissolved in water to prepare 10 mL of solution B. Solution B was slowly added dropwise to solution A to obtain solution C, and stirred for 10 min.
[0054] (4) 20 mL of polyethylene glycol 600 was measured and added dropwise at a rate of 5 mL / min from the solution C in step (3) to the polyethylene glycol 600 at a speed of 500 rpm to obtain a solution D, and the solution D was transferred to a hydrothermal reactor and reacted at 220° C. for 8 h to obtain 4 μm NCM811 spherical precursor particles;
[0055] (5) The 10 μm NCM811 spherical precursor particles obtained in step (2) and the 4 μm NCM811 spherical precursor particles obtained in step (4) are mixed in a mass ratio of 1:1 to obtain an NCM811 positive electrode material precursor.
[0056] The method for preparing the NCM811 positive electrode material in this embodiment comprises the following steps:
[0057] The NCM811 cathode material precursor was mixed with lithium carbonate in a mass ratio of 1:1.05 and ground for 30 minutes, then transferred to a muffle furnace and calcined for the first time at 480°C for 6 hours. After natural cooling, it was ground for 10 minutes and transferred to a muffle furnace and calcined at 780°C for 12 hours in an air atmosphere to finally obtain a double-dispersed spherical NCM811 cathode material.
[0058] The NCM811 cathode material of the present invention still maintains the spherical morphology and particle size of the precursor, including 10 μm NCM811 spherical particles and 4 μm NCM811 spherical particles, with a particle size ratio of 0.4.
[0059] Example 3
[0060] The method for preparing the NCM811 positive electrode material precursor in this embodiment comprises the following steps:
[0061] (1) The metal salt was prepared into 5 mL of 2 mol / L solution A according to the stoichiometric ratio of Ni:Co:Mn=8:1:1, and 0.012 mol of urea was dissolved in water to prepare 5 mL of solution B. Solution B was slowly added dropwise to solution A to obtain solution C, and stirred for 10 min.
[0062] (2) 50 mL of polyethylene glycol 400 was measured and added dropwise at a rate of 5 mL / min to the polyethylene glycol 400 at a speed of 500 rpm to obtain solution D, and solution D was transferred to a hydrothermal reactor and reacted at 220° C. for 8 h to obtain 2 μm NCM811 spherical precursor particles;
[0063] (3) Prepare 30 mL of 1 mol / L solution A with a stoichiometric ratio of Ni:Co:Mn=8:1:1, dissolve 0.02 mol of urea in water to prepare 10 mL of solution B, slowly add solution B dropwise to solution A to obtain solution C, and stir for 10 min;
[0064] (4) 20 mL of polyethylene glycol 600 was measured and added dropwise at a rate of 5 mL / min from the solution C in step (3) to the polyethylene glycol 600 at a speed of 500 rpm to obtain a solution D, and the solution D was transferred to a hydrothermal reactor and reacted at 180° C. for 8 h to obtain 7 μm NCM811 spherical precursor particles;
[0065] (5) The 2 μm NCM811 spherical precursor particles obtained in step (2) and the 7 μm NCM811 spherical precursor particles obtained in step (4) are mixed in a mass ratio of 1:1 to obtain a NCM811 positive electrode material precursor.
[0066] The method for preparing the NCM811 positive electrode material in this embodiment comprises the following steps:
[0067] The NCM811 cathode material precursor was mixed with lithium carbonate in a mass ratio of 1:1.05 and ground for 30 minutes, transferred to a muffle furnace for the first calcination at 520°C for 4 hours, and then naturally cooled, ground for 10 minutes and transferred to a muffle furnace for calcination at 750°C for 18 hours in an air atmosphere to finally obtain a double-dispersed spherical NCM811 cathode material.
[0068] The NCM811 cathode material of the present invention still maintains the spherical morphology and particle size of the precursor, including 2 μm NCM811 spherical particles and 7 μm NCM811 spherical particles, and the particle size ratio is 0.29.
[0069] Example 4
[0070] The only difference between the preparation method of the NCM811 positive electrode material precursor described in this embodiment and that in Example 1 is that in step (5), the 6μm NCM811 spherical precursor particles obtained in step (2) and the 2μm NCM811 spherical precursor particles obtained in step (4) are mixed in a mass ratio of 0.9:1 to obtain the NCM811 positive electrode material precursor.
[0071] The preparation method of the NCM811 positive electrode material described in this embodiment is the same as that in Example 1.
[0072] The NCM811 cathode material described in this embodiment still maintains the spherical morphology and particle size of the precursor, including 6 μm NCM811 spherical particles and 2 μm NCM811 spherical particles, and the particle size ratio is 0.33.
[0073] Example 5
[0074] The only difference between the preparation method of the NCM811 positive electrode material precursor described in this embodiment and that in Example 1 is that in step (5), the 6μm NCM811 spherical precursor particles obtained in step (2) and the 2μm NCM811 spherical precursor particles obtained in step (4) are mixed in a mass ratio of 1.1:1 to obtain the NCM811 positive electrode material precursor.
[0075] The preparation method of the NCM811 positive electrode material described in this embodiment is the same as that in Example 1.
[0076] The NCM811 cathode material described in this embodiment still maintains the spherical morphology and particle size of the precursor, including 6 μm NCM811 spherical particles and 2 μm NCM811 spherical particles, and the particle size ratio is 0.33.
[0077] Example 6
[0078] The only difference between the preparation method of the NCM811 positive electrode material precursor described in this embodiment and that in Example 1 is that in step (2), 40 mL of polyethylene glycol 200 is measured; and in step (4), 30 mL of polyethylene glycol 400 is measured.
[0079] The preparation method of the NCM811 positive electrode material described in this embodiment is the same as that in Example 1.
[0080] The NCM811 cathode material described in this embodiment still maintains the spherical morphology and particle size of the precursor, including 3 μm NCM811 spherical particles and 8 μm NCM811 spherical particles, and the particle size ratio is 0.375.
[0081] Comparative Example 1
[0082] The preparation method of the NCM811 positive electrode material precursor described in this comparison comprises the following steps:
[0083] (1) Prepare 30 mL of 1 mol / L solution A with a stoichiometric ratio of Ni:Co:Mn=8:1:1, dissolve 0.036 mol of urea in water to prepare 10 mL of solution B, slowly dropwise add solution B to solution A to obtain solution C, and stir for 10 min;
[0084] (2) 20 mL of polyethylene glycol 200 was measured and added dropwise at a rate of 5 mL / min to the solution C in step (1) at a rotation speed of 500 rpm to obtain a solution D, and the solution D was transferred to a hydrothermal reactor and reacted at 200° C. for 12 h to obtain 6 μm NCM811 spherical precursor particles;
[0085] The method for preparing the NCM811 positive electrode material in this embodiment comprises the following steps:
[0086] The 6μm NCM811 spherical precursor particles were mixed with lithium carbonate in a mass ratio of 1:1.05 and ground for 30 minutes, transferred to a muffle furnace for the first calcination at 500°C for 6 hours, and then naturally cooled, ground for 10 minutes and transferred to a muffle furnace for calcination at 750°C for 18 hours in an air atmosphere to finally obtain the NCM811 positive electrode material.
[0087] from Figure 3 It can be seen that the NCM811 cathode material described in this comparative example still maintains the spherical morphology and particle size of the precursor, which is 6 μm NCM811 spherical particles.
[0088] Comparative Example 2
[0089] The method for preparing the NCM811 positive electrode material precursor in this embodiment comprises the following steps:
[0090] (1) The metal salt was prepared into 5 mL of 2 mol / L solution A according to the stoichiometric ratio of Ni:Co:Mn=8:1:1, and 0.012 mol of urea was dissolved in water to prepare 5 mL of solution B. Solution B was slowly added dropwise to solution A to obtain solution C, and stirred for 10 min.
[0091] (2) 50 mL of polyethylene glycol 400 was measured and added dropwise at a rate of 5 mL / min to the polyethylene glycol 400 at a speed of 500 rpm to obtain solution D, and solution D was transferred to a hydrothermal reactor and reacted at 200° C. for 12 h to obtain 2 μm NCM811 spherical precursor particles;
[0092] The method for preparing the NCM811 positive electrode material in this embodiment comprises the following steps:
[0093] The 2μm NCM811 spherical precursor particles were mixed with lithium carbonate in a mass ratio of 1:1.05 and ground for 30 minutes, transferred to a muffle furnace for the first calcination at 500°C for 6 hours, and then naturally cooled, ground for 10 minutes and transferred to a muffle furnace for calcination at 750°C for 18 hours in an air atmosphere to finally obtain the NCM811 positive electrode material.
[0094] from Figure 4 It can be seen that the NCM811 cathode material described in this comparative example still maintains the spherical morphology and particle size of the precursor, which is 2 μm NCM811 spherical particles.
[0095] Comparative Example 3
[0096] The preparation method of the NCM811 positive electrode material precursor described in this comparative example comprises the following steps:
[0097] (1) Prepare 30 mL of 1 mol / L solution A with a stoichiometric ratio of Ni:Co:Mn=8:1:1, dissolve 0.072 mol of urea in water to prepare 10 mL of solution B, slowly add solution B dropwise to solution A to obtain solution C, and stir for 10 min;
[0098] (2) 20 mL of polyethylene glycol 200 was measured, and the solution C in step (1) was added dropwise to the polyethylene glycol 200 at a rate of 5 mL / min at a rotation speed of 500 rpm to obtain a solution D, and the solution D was transferred to a hydrothermal reactor and reacted at 200° C. for 12 h to obtain NCM811 spherical precursor particles-1;
[0099] (3) The metal salt was prepared into 5 mL of 2 mol / L solution A according to the stoichiometric ratio of Ni:Co:Mn=8:1:1, and 0.012 mol of urea was dissolved in water to prepare 5 mL of solution B. Solution B was slowly added dropwise to solution A to obtain solution C, and stirred for 10 min.
[0100] (4) 50 mL of polyethylene glycol 400 was measured and added dropwise at a rate of 5 mL / min to the polyethylene glycol 400 at a speed of 500 rpm to obtain solution D, and solution D was transferred to a hydrothermal reactor and reacted at 200 °C for 12 h to obtain 2 μm NCM811 spherical precursor particles;
[0101] (5) The NCM811 spherical precursor particles-1 obtained in step (2) and the 2 μm NCM811 spherical precursor particles obtained in step (4) are mixed in a mass ratio of 1:1 to obtain a NCM811 positive electrode material precursor.
[0102] The preparation method of the NCM811 positive electrode material described in this comparative example comprises the following steps:
[0103] The NCM811 cathode material precursor was mixed with lithium carbonate in a mass ratio of 1:1.05 and ground for 30 minutes, then transferred to a muffle furnace for the first calcination at 500°C for 6 hours, and then naturally cooled, ground for 10 minutes and transferred to a muffle furnace for calcination at 750°C for 18 hours in an air atmosphere to finally obtain a double-dispersed spherical NCM811 cathode material.
[0104] The particle size of the NCM811 spherical precursor particles-1 described in this comparative example is not uniform, and the obtained NCM811 positive electrode material contains spherical particles and non-spherical particles of various particle sizes.
[0105] Comparative Example 4
[0106] The only difference between the preparation method of the NCM811 positive electrode material precursor described in this comparative example and that in Example 1 is that in step (5), the 6μm NCM811 spherical precursor particles obtained in step (2) and the 2μm NCM811 spherical precursor particles obtained in step (4) are mixed in a mass ratio of 0.7:1 to obtain the NCM811 positive electrode material precursor.
[0107] The preparation method of the NCM811 positive electrode material described in this comparative example is the same as that in Example 1.
[0108] The NCM811 cathode material described in this comparative example still maintains the spherical morphology and particle size of the precursor, including 6 μm NCM811 spherical particles and 2 μm NCM811 spherical particles, and the particle size ratio is 0.33.
[0109] Comparative Example 5
[0110] The only difference between the preparation method of the NCM811 positive electrode material precursor described in this comparative example and that in Example 1 is that in step (5), the 6μm NCM811 spherical precursor particles obtained in step (2) and the 2μm NCM811 spherical precursor particles obtained in step (4) are mixed in a mass ratio of 1.3:1 to obtain the NCM811 positive electrode material precursor.
[0111] The preparation method of the NCM811 positive electrode material described in this comparative example is the same as that in Example 1.
[0112] The NCM811 cathode material described in this comparative example still maintains the spherical morphology and particle size of the precursor, including 6 μm NCM811 spherical particles and 2 μm NCM811 spherical particles, and the particle size ratio is 0.33.
[0113] Comparative Example 6
[0114] The only difference between the preparation method of the NCM811 positive electrode material precursor described in this comparison and that in Example 1 is that in step (2), 160 mL of polyethylene glycol 200 is measured; and in step (4), 1 mL of polyethylene glycol 400 is measured.
[0115] The preparation method of the NCM811 positive electrode material described in this comparative example is the same as that in Example 1.
[0116] The NCM811 cathode material described in this comparative example still maintains the spherical morphology and particle size of the precursor, including 0.2 μm NCM811 spherical particles and 6 μm NCM811 spherical particles, and the particle size ratio is 0.033.
[0117] Comparative Example 7
[0118] The only difference between the preparation method of the NCM811 positive electrode material precursor described in this comparison and that in Example 1 is that in step (2), 10 mL of polyethylene glycol 200 is measured; and in step (4), 60 mL of polyethylene glycol 400 is measured.
[0119] The preparation method of the NCM811 positive electrode material described in this comparative example is the same as that in Example 1.
[0120] The NCM811 cathode material described in this comparative example still maintains the spherical morphology and particle size of the precursor, including 7 μm NCM811 spherical particles and 0.8 μm NCM811 spherical particles, and the particle size ratio is 0.114.
[0121] Test example
[0122] The NCM811 positive electrode material prepared in the embodiment and the comparative example was mixed with conductive graphite Super P and polyvinylidene fluoride PVDF in a mass ratio of 8:1:1 and dispersed in nitrogen methyl pyrrolidone, and stirred at a speed of 1000 rpm for 30 minutes to obtain a uniform positive electrode material slurry. The slurry was evenly coated on a 14-micron thick aluminum foil with a 200-micron coater, and then a plurality of 12-mm diameter discs were cut out with a punching machine to obtain a positive electrode sheet.
[0123] In this test example, the stacking density, rate performance and cycle performance of the positive electrode sheets prepared in the examples and comparative examples were tested.
[0124] Table 1: Data on the stacking density of the positive electrode coating of Example 1 and Comparative Examples 1-2
[0125]
[0126]
[0127] According to Table 1 and Figure 5 The data show that the highest packing density of the positive electrode coating prepared by the NCM811 positive electrode material in Example 1 is 0.988 mg / mm 3 , higher than the bulk density of Comparative Example 1-2.
[0128] Table 2: Data on the stacking density of the positive electrode coating prepared in the examples and comparative examples
[0129]
[0130] according to Figure 6 The rate performance comparison diagram shows that the discharge specific capacity of the positive electrode sheet prepared in Example 1 at each discharge rate is better than that of the positive electrode sheet prepared in Comparative Examples 1-2, and the rate performance is good; Figure 7It can be seen from the cycle performance graph that the positive electrode sheet of Example 1 has a greater improvement in long cycle performance compared with Comparative Examples 1-2, indicating that the positive electrode material with a high stacking density is beneficial to improving the electrochemical performance of the battery. According to the results in Table 2, the average stacking density of the coating of the positive electrode sheet prepared in the embodiment of the present invention is large, which is beneficial to improving the electrochemical performance of the battery.
[0131] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A NCM811 positive electrode material, characterized in that: Prepared from NCM811 positive electrode material precursor and lithium salt; the preparation method of the NCM811 positive electrode material comprises the following steps: mixing and grinding the NCM811 positive electrode material precursor and the lithium salt, calcining for the first time, grinding after cooling, and calcining for the second time to obtain the NCM811 positive electrode material; The preparation method of the NCM811 positive electrode material precursor comprises the following steps: (1) preparing a metal salt in a molar ratio of Ni:Co:Mn=8:1:1 to form a solution A, dissolving a precipitant in water to form a solution B, adding the solution B to the solution A and mixing evenly to obtain a solution C, and stirring for 6 hours; (2) adding solution C to an organic solvent for hydrothermal reaction to obtain a NCM811 cathode material precursor; the volume ratio of the organic solvent to water is 0.5-5, the water is the water in solution C, the temperature of the hydrothermal reaction is 180-220° C., and the time of the hydrothermal reaction is 8-12 hours; the NCM811 cathode material precursor is composed of large-diameter spherical precursor particles and small-diameter spherical precursor particles, the particle size ratio of the small-diameter spherical precursor particles to the large-diameter spherical precursor particles is 0.16-0.40, and the mass ratio of the large-diameter spherical precursor particles to the small-diameter spherical precursor particles is 0.9-1.1; Wherein, the organic solvent is polyethylene glycol 200, polyethylene glycol 400 or polyethylene glycol 600; the precipitant is urea, and the molar number of urea is 1.2-2 times the molar number of the metal salt.
2. The NCM811 positive electrode material according to claim 1, characterized in that: The temperature of the first calcination is 480-500° C. and the time is 4-6 hours.
3. The NCM811 positive electrode material according to claim 1, characterized in that: The temperature of the second calcination is 750-780°C and the time is 12-18 hours.
Citation Information
Patent Citations
Method for improving tap density of ternary nickel-cobalt-manganese cathode material for lithium-ion battery
CN105489881A
Ternary anode materials with different particle sizes and preparation method thereof
CN110854385A
Ternary material and preparation method thereof, battery slurry, positive electrode and lithium battery
US20190386293A1