Liquid crystal alignment agent, liquid crystal alignment film, liquid crystal display element, polymer and diamine
By using a polymer with a specific structure as a liquid crystal aligning agent in a liquid crystal display element, the problem of reduced orientation ability of the liquid crystal alignment film under excessive heating is solved, and a high display quality liquid crystal display element is realized.
Patent Information
- Application Number
- CN202080066918.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-15
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-09-15
AI Technical Summary
During the manufacturing process of liquid crystal display elements, the temperature difference caused by the thinning and enlargement of the substrate reduces the orientation ability of the liquid crystal alignment film when overheated, resulting in some display defects.
A polymer with a specific structure is used as a liquid crystal aligning agent, and a composition composed of a polyimide precursor and a polyimide containing specific groups can improve the thermal stability and vertical alignment ability of the liquid crystal alignment film.
Even in the case of excessive heating, it can maintain high liquid crystal orientation ability, avoid display defects, and improve the display quality of liquid crystal display elements.
Smart Images

Figure FDA0004940944260000011 
Figure FDA0004940944260000012 
Figure FDA0004940944260000021
Abstract
Description
Technical Field
[0001] The present invention relates to a liquid crystal alignment agent; a liquid crystal alignment film obtained from the liquid crystal alignment agent; a liquid crystal display element having the liquid crystal alignment film; and novel diamines and polymers suitable for the liquid crystal alignment agent, the liquid crystal alignment film, and the liquid crystal display element. Background Art
[0002] In the past, various driving methods with different electrode structures and physical properties of liquid crystal molecules used have been developed as liquid crystal display elements, such as TN (Twisted Nematic), STN (Super Twisted Nematic), VA (Vertical Alignment), IPS (In-Plane Switching), FFS (fringe field switching) and other display elements. These liquid crystal display elements have a liquid crystal alignment film for orienting liquid crystal molecules. As materials for the liquid crystal alignment film, for example, polyamic acid, polyamic acid ester, polyimide, polyamide and the like are known.
[0003] In a VA-type liquid crystal display element, the manufacturing process includes a step of applying voltage to the liquid crystal molecules while irradiating ultraviolet rays. In such a VA-type liquid crystal display element, the following technology is known: a photopolymerizable compound is added to the liquid crystal composition in advance, and a liquid crystal alignment film such as a polyimide system is used, and a voltage is applied to the liquid crystal box while irradiating ultraviolet rays, thereby accelerating the response speed of the liquid crystal (PSA (Polymer Sustained Alignment: polymer stable orientation) mode element, for example, refer to Patent Document 1 and Non-Patent Document 1). As a liquid crystal alignment agent for the PSA mode element, a liquid crystal alignment agent having a specific ring structure in the side chain is proposed (refer to Patent Document 2). This specific ring structure has a high ability to vertically align the liquid crystal, and the display characteristics of the VA-type liquid crystal display element using this liquid crystal alignment agent are good.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2003-307720
[0007] Patent Document 2: WO2006 / 070819
[0008] Non-patent literature
[0009] Non-patent document 1: K. Hanaoka, SID 04 DIGEST, P. 1200-1202 Summary of the invention
[0010] Problems to be solved by the invention
[0011] However, in recent years, in liquid crystal display elements, due to the influence of thinning and enlargement of the substrates used, a temperature difference is generated between different parts of the same substrate during firing, and the liquid crystal orientation film in the overheated part reduces the ability of the liquid crystal to orient. As a result, the resulting liquid crystal display element has a problem of partial display failure.
[0012] The present invention has been made in view of the above problems, and provides a liquid crystal aligning agent that can obtain a liquid crystal aligning film having a high ability to align liquid crystals even when exposed to excessive heating; and a liquid crystal display element that is less likely to have display failure.
[0013] Solutions for solving problems
[0014] The present inventors have conducted intensive studies to solve the above-mentioned problems, and as a result, have found that the above-mentioned characteristics can be obtained by making a liquid crystal aligning agent contain a polymer having a specific structure, thereby completing the present invention.
[0015] The present invention is based on this finding and has the following contents as its main points.
[0016] A liquid crystal aligning agent comprising at least one polymer (P) selected from the group consisting of a polyimide precursor and a polyimide having a group represented by the following formula (1).
[0017] *- X 1-Q-X2-YR (1)
[0018] (In the formula, X1 represents an alkylene group having 1 to 14 carbon atoms, and one or two non-adjacent methylene groups of the alkylene group are optionally substituted with -O- or -COO-. X2 represents a single bond, -OCO-, -COO-, or CONR 2 -(R 2 represents a hydrogen atom or a methyl group). Q represents a naphthylene group, and Y represents a group containing at least one cyclohexylene group. Any hydrogen atom of the above-mentioned naphthylene group or cyclohexylene group is optionally substituted by at least one selected from the group consisting of an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, a fluorinated alkyl group having 1 to 3 carbon atoms, a fluorinated alkoxy group having 1 to 3 carbon atoms, or a fluorine atom. R represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, a fluorinated alkyl group having 1 to 12 carbon atoms, a fluorinated alkoxy group having 1 to 12 carbon atoms, -CN, -F, -OH, -CO2H, -OCOR 3, or -CO2R 3 , R 3 Indicates a methyl group or an ethyl group. * indicates a bonding bond. )
[0019] Effects of the Invention
[0020] According to the present invention, there are provided a liquid crystal aligning agent capable of obtaining a liquid crystal aligning film having a high ability to align liquid crystals even when exposed to excessive heating, and a liquid crystal display element having a high display quality grade and being less likely to cause display defects.
[0021] The mechanism for obtaining the liquid crystal aligning agent and liquid crystal display element having the above-mentioned excellent characteristics according to the present invention is not necessarily clear, but is roughly estimated as follows.
[0022] As the main factor of the reduction of vertical alignment ability under the condition of being exposed to high temperature, it can be considered that the thermal decomposition of the side chain with vertical alignment ability, the embedding of the film due to the thermal motion of the side chain, etc. On the other hand, in the research of the present inventors, it is known that in the case of a polymer containing a rigid structure, it is helpful to increase the glass transition temperature of the polymer and the improvement of thermal stability. In the polymer with a specific structure of the present invention, there is a rigid structure such as a naphthyl group, and thermal stability is improved, so it is estimated that a liquid crystal alignment film with a high ability to orient the liquid crystal can be obtained. DETAILED DESCRIPTION
[0023] <Polymer (P)>
[0024] The liquid crystal aligning agent of this invention contains at least 1 polymer (P) selected from the group consisting of the polyimide precursor and the polyimide which have a group represented by said formula (1).
[0025] In the above formula (1), X1 preferably represents -O-, -COO-, -(CH2) c -(c is an integer from 1 to 10), -CH2O-, -CO-O-, -(CH2) c -CO-O-(c is an integer from 1 to 10), -(CH2) c -O-CO-(c is an integer from 1 to 10), -CH2O-(CH2) c -(c is an integer from 1 to 10), -CH2O-(CH2) c -(O) d -(c is an integer from 1 to 10, d is an integer from 0 to 1), -CO-O-(CH2) c -(O) d -(c is an integer from 1 to 10, d is an integer from 0 to 1), -O-(CH2) c -(O) d -(c is an integer from 1 to 10, d is an integer from 0 to 1), -CO-O-(CH2)c -O-CO-(c is an integer from 1 to 10), -CO-O-(CH2) c -CO-O-(c is an integer from 1 to 10).
[0026] X2 preferably represents a single bond.
[0027] Y preferably represents a group represented by the following formula (Z).
[0028]
[0029] (where X3 represents a single bond, -(CH2) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -COO-, -OCO- or -((CH2) a1 -A1) m1 -. Wherein, multiple a1s each independently represent an integer of 1 to 15, multiple A1s each independently represent an oxygen atom or -COO-, and m1 represents an integer of 1 to 2. Y1 represents a cyclohexylene group, and any hydrogen atom of the cyclohexylene group is optionally substituted by at least one selected from the group consisting of an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, a fluorinated alkyl group having 1 to 3 carbon atoms, a fluorinated alkoxy group having 1 to 3 carbon atoms, and a fluorine atom. n represents an integer of 1 to 10. )
[0030] In the above formula (Z), X3 preferably represents a single bond, and n represents an integer of 1 to 4, more preferably 2 to 4.
[0031] R preferably represents an alkyl group having 1 to 9 carbon atoms, a fluorinated alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 9 carbon atoms, or a fluorinated alkoxy group having 1 to 10 carbon atoms.
[0032] The group represented by the formula (1) preferably represents a group represented by the following formulae (1-1) to (1-12).
[0033]
[0034] (c is an integer from 1 to 10. d is an integer from 0 to 1. m is an integer from 1 to 2. n is an integer from 1 to 12.)
[0035] <Specific diamine>
[0036] The polymer (P) is, for example, a polymer obtained from a diamine component containing a diamine (hereinafter referred to as “specific diamine”) having a group represented by the above formula (1).
[0037] The specific diamine is preferably at least one diamine selected from the group consisting of diamines represented by the following formulae (2-1) and (2-2).
[0038]
[0039] (Where X 11 , X 21a , X 21b The same meaning as X1 in the above formula (1), Q1, Q 2a , Q 2b The same meaning as Q in the above formula (1), X 12 , X 22a , X 22b The same meaning as X2 in the above formula (1), Y1, Y 2a , Y 2b The same meaning as Y in the above formula (1), R1, R 2a , R 2b The same meaning as R in the above formula (1). L represents a single bond, -O-, -C(CH3)2-, -NR- (R represents a hydrogen atom or a methyl group), -CO-, -NHCO-, -COO-, -(CH2) m -, -SO2-, -O-(CH2) m -O-, -O-C(CH3)2-, -CO-(CH2) m -, -NH-(CH2) m -、-SO2-(CH2) m -、-CONH-(CH2) m -、-CONH-(CH2) m -NHCO-, -COO-(CH2) m -OCO-. m represents an integer from 1 to 8. )
[0040] As specific examples of the specific diamine, at least one diamine selected from the group consisting of the following diamines can be cited: In formula (2-1), the group “—X 11 -Q1-X 12 -Y1-R1" represents a diamine of a group represented by the above formula (1-1) to (1-12); and in formula (2-2), the group "-X 21 -Q 2a -X 22a -Y 2a -R 2a " and group "-X 22 -Q 2b -X 22b -Y 2b -R 2b " respectively independently represent a diamine of a group represented by the above formula (1-1) to (1-12). As a further preferred specific example of the diamine, at least one diamine selected from the following diamines can be listed: In formula (2-1), the group "-X 11-Q1-X 12 -Y1-R1" represents a group represented by the above formula (1-1) to (1-12), and the two amino groups are opposite to the group "-X 11 -Q1-X 12 -Y1-R1" is a diamine bonded at the ortho position and the para position. In particular, at least one diamine selected from the group consisting of diamines represented by the following formulae (d-1) to (d-12) is preferred.
[0041]
[0042]
[0043] (m represents 2. n represents 3, 5 or 7. c represents 1 to 6. d represents 0 or 1.)
[0044] <Other diamines>
[0045] As the diamine component for producing the polymer (P), any other diamine other than the specific diamine may be used. Examples of the other diamine include diamines having a carboxyl group such as p-phenylenediamine, m-phenylenediamine, 4-(2-(methylamino)ethyl)aniline, and 3,5-diaminobenzoic acid, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 1,2-bis(4-aminophenyl)ethane, 1,3-bis(4-aminophenyl)propane, 1,4-bis(4-aminophenyl)butane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,2-bis(4-aminophenoxy)benzene, and 1,2-bis(4-aminophenoxy)benzene. )ethane, 1,2-bis(4-amino-2-methylphenoxy)ethane, 1,3-bis(4-aminophenoxy)propane, 1,4-bis(4-aminophenoxy)butane, 1,5-bis(4-aminophenoxy)pentane, 1,6-bis(4-aminophenoxy)hexane, 4-(2-(4-aminophenoxy)ethoxy)-3-fluoroaniline, bis(2-(4-aminophenoxy)ethyl)ether, 4-amino-4'-(2-(4-aminophenoxy)ethoxy)biphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 1,4-diaminonaphthalene, 1,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2,7-diaminonaphthalene diamines having a urea bond such as aminonaphthalene, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 2,2'-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2'-bis(4-aminophenyl)propane, 1,3-bis(4-aminophenethyl)urea, diamines represented by the following formulas (a-1) to (a-6), preferably diamines having a photopolymerizable group at the end such as 2-(2,4-diaminophenoxy)ethyl methacrylate and 2,4-diamino-N,N-diallylaniline, diamines having a free radical initiating function such as the following formulas (R1) to (R5), 2,6-diaminopyridine, 3,4-diaminopyridine, 2,4-diaminopyrimidine, 3,6-diamino Carbazole, N-methyl-3,6-diaminocarbazole, diamines having a heterocyclic ring such as the following formulas (z-1) to (z-18), diamines having a diphenylamine skeleton such as the following formulas (Dp-1) to (Dp-3), diamines having a group "-N(D)-" (D represents a protective group which is detached by heating and replaced by a hydrogen atom, preferably a tert-butoxycarbonyl group) such as the following formulas (5-1) to (5-11), diamines having an oxazoline structure such as the following formulas (Ox-1) to (Ox-2), diamines having a structure which reflects the vertical alignment property of liquid crystal in the side chain such as the following formulas (V2-1) to (V2-13), diamines containing an organic siloxane such as 1,3-bis(3-aminopropyl)-tetramethyldisiloxane, and the like.
[0046]
[0047]
[0048] (d1 represents an integer from 2 to 10.)
[0049]
[0050] (n represents an integer from 2 to 10.)
[0051]
[0052] (Boc represents tert-butoxycarbonyl.)
[0053]
[0054] (Where, in the formula, X v1 ~X v4 , X p1 ~X p8 Each independently represents -(CH2) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CH2O-, -CH2-OCO-, -COO-, or -OCO-, X v5 represents -O-, -CH2O-, -CH2-OCO-, -COO-, or -OCO-, X V6 ~X V7 , X s1 ~X s4 Each independently represents -O-, -COO- or -OCO-. a ~X f Represents a single bond, -O-, -NH-, -O-(CH2) m -O-, -C(CH3)2-, -CO-, -COO-, -CONH-, -(CH2) m -, -SO2-, -O-C(CH3)2-, -CO-(CH2) m -, -NH-(CH2) m -, -NH-(CH2) m -NH-, -SO2-(CH2) m -、-SO2-(CH2) m -SO2-, -CONH-(CH2) m -、-CONH-(CH2) m -NHCO-, or -COO-(CH2) m -OCO-,R v1 ~R v4, R 1a ~R 1h Represented independently -C n H 2n+1 (n is an integer from 1 to 20), -O-C n H 2n+1 (n is an integer from 2 to 20. m is an integer from 1 to 8.)
[0055] Moreover, as other diamines, aliphatic diamines, such as meta-xylene diamine, alicyclic diamines, such as 4,4-methylenebis(cyclohexylamine), and the diamines described in International Publication No. 2016 / 125870 can also be mentioned.
[0056] From the perspective of improving the response speed of the liquid crystal display element obtained in the process of (1-3B) or (1-3C) described later, the above-mentioned 4,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, a diamine having a photopolymerizable group at the end, a diamine represented by the above-mentioned formula (R1) to (R5), and a diamine represented by the above-mentioned formula (z-1) to (z-18) can also be used in the case of manufacturing the polymer (P). The content of these diamines is preferably 5 to 70 mol% relative to the entire diamine component, and from the perspective of improving the voltage retention of the obtained liquid crystal alignment film, it is more preferably 5 to 60 mol%, and particularly preferably 5 to 50 mol%.
[0057] Other diamines may be used alone or in combination of two or more.
[0058] <Tetracarboxylic acid component>
[0059] The tetracarboxylic acid component refers to a component containing at least one selected from tetracarboxylic acid and a tetracarboxylic acid derivative. Examples of the tetracarboxylic acid derivative include tetracarboxylic acid dihalide, tetracarboxylic dianhydride, tetracarboxylic acid diester dichloride, and tetracarboxylic acid diester.
[0060] The polyimide precursor as the polymer (P) can be obtained by, for example, subjecting a diamine component containing a diamine having a group represented by the above formula (1) to a polymerization reaction with a tetracarboxylic acid component.
[0061] The tetracarboxylic acid components used to manufacture the polymer (P) include: aromatic tetracarboxylic dianhydride, aliphatic tetracarboxylic dianhydride, alicyclic tetracarboxylic dianhydride, or their derivatives. Here, aromatic tetracarboxylic dianhydride is an acid dianhydride obtained by intramolecular dehydration of four carboxyl groups including at least one carboxyl group bonded to an aromatic ring. Aliphatic tetracarboxylic dianhydride is an acid dianhydride obtained by intramolecular dehydration of four carboxyl groups bonded to a chain hydrocarbon structure. However, it is not necessary to consist only of a chain hydrocarbon structure, and a part of it may have an alicyclic structure or an aromatic ring structure. Alicyclic tetracarboxylic dianhydride is an acid dianhydride obtained by intramolecular dehydration of four carboxyl groups including at least one carboxyl group bonded to an alicyclic structure. Among them, none of these four carboxyl groups is bonded to an aromatic ring. In addition, it is not necessary to consist only of an alicyclic structure, and a part of it may have a chain hydrocarbon structure or an aromatic ring structure. The above-mentioned tetracarboxylic acid component preferably includes a tetracarboxylic dianhydride shown in the following formula (3).
[0062]
[0063] (X represents a structure selected from any of the following (x-1) to (x-13).)
[0064]
[0065] (Where R 1 ~R 4 represents a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom or a benzene ring, and may be the same or different. 5 and R 6 represents a hydrogen atom or a methyl group, which may be the same or different. j and k each independently represent 0 or 1, and A1 and A2 each independently represent a single bond, an ether group, a carbonyl group, an ester group, a phenylene group, a sulfonyl group or an amide group. *1 represents a bond to an acid anhydride group on one side, and *2 represents a bond to an acid anhydride group on the other side.)
[0066] Preferred specific examples of (x-12) and (x-13) include the following formulae (x-14) to (x-29): * represents a bonding bond.
[0067]
[0068] Preferred examples of the tetracarboxylic dianhydride or its derivative represented by the above formula (3) include tetracarboxylic dianhydride or its derivative represented by the formula (3) wherein X is the above formula (x-1) to (x-7) and (x-11) to (x-13).
[0069] <Contents of polymer (P), diamine component and tetracarboxylic acid component>
[0070] It is preferable that it is 1-10 mass % with respect to the total mass of a liquid crystal aligning agent, and, as for content of the polymer (P) used for this invention, it is more preferable that it is 2-9 mass %.
[0071] The content of the specific diamine is preferably 10 to 80 mol %, more preferably 20 to 70 mol %, and further preferably 30 to 60 mol % based on the total amount of the diamine components used to produce the polymer (P).
[0072] The diamine component for producing the polymer (P) can be used alone or in combination of two or more depending on the solubility of the polymer in a solvent, the coating property of a liquid crystal aligning agent, the liquid crystal alignment property in the case of a liquid crystal aligning film, the voltage holding ratio, the stored charge and other properties.
[0073] The content of the tetracarboxylic dianhydride represented by formula (3) is preferably 1 mol% or more, more preferably 5 mol% or more, and further preferably 10 mol% or more, based on the total amount of the diamine components used to produce the polymer (P).
[0074] The tetracarboxylic acid component for producing the polymer (P) can be used alone or in combination of two or more thereof depending on the solubility of the polymer in the solvent, the coating property of the liquid crystal aligning agent, the liquid crystal alignment property when formed into a liquid crystal aligning film, the voltage holding ratio, the stored charge and other properties.
[0075] <Polymer>
[0076] The present invention also includes a polymer obtained from a diamine component containing at least one diamine represented by the above formula (2-1) or (2-2). Examples of such a polymer include a polyimide precursor, a polyimide, a polyamide, and a polyurea. The polymer is preferably at least one polymer selected from the group consisting of a polyimide precursor and a polyimide obtained by imidizing the polyimide precursor.
[0077] <Production of polyimide precursor (polyamic acid)>
[0078] As the polyimide precursor used in the present invention, polyamic acid, polyamic acid ester, etc. can be mentioned.
[0079] The polyamic acid as the polyimide precursor used in the present invention can be produced, for example, by the following method: Specifically, it can be synthesized by reacting a diamine component and a tetracarboxylic acid component in the presence of an organic solvent at -20 to 150°C, preferably 0 to 80°C, for 30 minutes to 24 hours, preferably 1 to 12 hours.
[0080] The reaction of the diamine component and the tetracarboxylic acid component is usually carried out in an organic solvent. The organic solvent used at this time is not particularly limited as long as it dissolves the generated polyimide precursor. The following are specific examples of organic solvents used in the reaction, but are not limited to these examples. For example, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone or γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide or 1,3-dimethyl-2-imidazolidinone can be listed.
[0081] When the polyimide precursor has high solubility, methyl ethyl ketone, cyclohexanone, cyclopentanone, 4-hydroxy-4-methyl-2-pentanone, or an organic solvent represented by the following formula [D-1] to [D-3] can be used.
[0082]
[0083] In formula [D-1], D 1 represents an alkyl group having 1 to 3 carbon atoms, wherein D 2 represents an alkyl group having 1 to 3 carbon atoms, wherein D 3 It represents an alkyl group having 1 to 4 carbon atoms.
[0084] These organic solvents may be used alone or in combination. Furthermore, even if the solvent does not dissolve the polyimide precursor, it may be used by mixing with the above-mentioned solvent within a range in which the generated polyimide precursor does not precipitate.
[0085] The concentration of the polyamic acid polymer in the reaction system is preferably 1 to 30% by mass, more preferably 5 to 20% by mass, from the viewpoint of preventing the polymer from precipitating and easily obtaining a high molecular weight product.
[0086] The polyamic acid obtained as described above can be recovered by injecting the reaction solution into a poor solvent while fully stirring the reaction solution. In addition, the polymer is precipitated and recovered. In addition, the precipitation is carried out several times, and after washing with a poor solvent, the powder of the purified polyamic acid can be obtained at room temperature or by heating and drying. The poor solvent is not particularly limited, and examples thereof include water, methanol, ethanol, hexane, butyl cellosolve, acetone, toluene, etc.
[0087] <Production of polyimide precursor (polyamic acid ester)>
[0088] The polyamic acid ester which is a polyimide precursor used in the present invention can be produced by, for example, the production method of (1), (2) or (3) shown below.
[0089] (1) When made from polyamic acid
[0090] Polyamic acid ester can be produced by esterifying the polyamic acid produced as described above. Specifically, it can be produced by reacting polyamic acid and an esterifying agent in the presence of an organic solvent at -20 to 150°C, preferably at 0 to 50°C, for 30 minutes to 24 hours, preferably for 1 to 4 hours.
[0091] As the esterifying agent, an esterifying agent that can be easily removed by purification is preferred, and examples thereof include N,N-dimethylformamide dimethyl acetal, N,N-dimethylformamide diethyl acetal, N,N-dimethylformamide dipropyl acetal, N,N-dimethylformamide dineopentyl butyl acetal, N,N-dimethylformamide di-tert-butyl acetal, 1-methyl-3-p-tolyl triazene, 1-ethyl-3-p-tolyl triazene, 1-propyl-3-p-tolyl triazene, 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride, etc. The amount of the esterifying agent added is preferably 2 to 6 molar equivalents relative to 1 mole of the repeating unit of the polyamic acid.
[0092] Examples of the organic solvent include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and 1,3-dimethyl-2-imidazolidinone. In addition, when the polyimide precursor has high solvent solubility, methyl ethyl ketone, cyclohexanone, cyclopentanone, 4-hydroxy-4-methyl-2-pentanone, or an organic solvent represented by the above formula [D-1] to [D-3] can be used.
[0093] These organic solvents can be used alone or in combination. Moreover, even if it is a solvent that does not dissolve the polyimide precursor, it can be mixed with the above-mentioned solvent in the range that the generated polyimide precursor does not separate out. In addition, the moisture in the organic solvent can hinder the polymerization reaction, and then becomes the reason for hydrolyzing the generated polyimide precursor, so the organic solvent is preferably used after dehydration and drying.
[0094] From the solubility of the polymer, the solvent used in the above reaction is preferably N, N-dimethylformamide, N-methyl-2-pyrrolidone, or γ-butyrolactone, which can be used alone or in combination. From the perspective of not easily causing the precipitation of the polymer and easily obtaining a high molecular weight product, the concentration during production is preferably 1 to 30% by mass, more preferably 5 to 20% by mass.
[0095] (2) When produced by reaction of tetracarboxylic acid diester dichloride and diamine
[0096] Polyamic acid ester can be manufactured from tetracarboxylic acid diester dichloride and diamine. Specifically, it can be manufactured by reacting tetracarboxylic acid diester dichloride and diamine at -20 to 150°C, preferably 0 to 50°C, for 30 minutes to 24 hours, preferably 1 to 4 hours in the presence of a base and an organic solvent.
[0097] As the base, pyridine, triethylamine, 4-dimethylaminopyridine, etc. can be used, but pyridine is preferred to make the reaction proceed mildly. From the perspective of easy removal and easy to obtain a high molecular weight product, the amount of base added is preferably 2 to 4 times the molar amount of the tetracarboxylic acid diester dichloride.
[0098] As the organic solvent, N-methyl-2-pyrrolidone or γ-butyrolactone is preferred from the viewpoint of solubility of the monomer and the polymer, and these may be used alone or in combination of two or more.
[0099] From the viewpoint of not easily causing the precipitation of the polymer and easily obtaining a high molecular weight product, the polymer concentration during production is preferably 1 to 30% by mass, more preferably 5 to 20% by mass. In addition, in order to prevent the hydrolysis of the tetracarboxylic acid diester dichloride, the organic solvent used in the production of the polyamic acid ester is preferably dehydrated as much as possible, preferably in a nitrogen atmosphere, to prevent the mixing of external air.
[0100] (3) When produced from tetracarboxylic acid diester and diamine
[0101] Polyamic acid ester can be produced by polycondensing a tetracarboxylic acid diester and a diamine. Specifically, it can be produced by reacting a tetracarboxylic acid diester and a diamine at 0 to 150°C, preferably 0 to 100°C, for 30 minutes to 24 hours, preferably 3 to 15 hours in the presence of a condensing agent, a base, and an organic solvent.
[0102] As the condensing agent, triphenyl phosphite, dicyclohexylcarbodiimide, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride, N,N'-carbonyldiimidazole, dimethoxy-1,3,5-triazinylmethylmorpholinium, O-(benzotriazol-1-yl)-N,N,N',N'-tetramethyluronium tetrafluoroborate, O-(benzotriazol-1-yl)-N,N,N',N'-tetramethyluronium hexafluorophosphate, (2,3-dihydro-2-thio-3-benzoxazolyl)phosphonic acid diphenyl ester, etc. The amount of the condensing agent added is preferably 2 to 3 times the molar amount of the tetracarboxylic acid diester.
[0103] As the base, a tertiary amine such as pyridine or triethylamine can be used. The amount of the base added is preferably 2 to 4 times the molar amount of the diamine component from the viewpoint of easy removal and easy acquisition of a high molecular weight product.
[0104] In the above reaction, the reaction can be efficiently carried out by adding a Lewis acid as an additive. As the Lewis acid, lithium halides such as lithium chloride and lithium bromide are preferred. The amount of the Lewis acid added is preferably 0 to 1.0 times the mole of the diamine component.
[0105] In order to obtain high molecular weight polyamic acid ester among the three methods for producing polyamic acid ester mentioned above, the production method of (1) or (2) mentioned above is particularly preferred.
[0106] The polymer can be precipitated by injecting the solution of polyamic acid ester obtained as described above into a poor solvent while stirring it thoroughly. The precipitation is performed several times, and after washing with a poor solvent, the purified polyamic acid ester powder can be obtained at room temperature or by heating and drying. The poor solvent is not particularly limited, and examples thereof include water, methanol, ethanol, hexane, butyl cellosolve, acetone, toluene, and the like.
[0107] <Manufacturing of polyimide>
[0108] The polyimide used in the present invention can be produced by imidizing the above-mentioned polyamic acid.
[0109] Imidization can be carried out by stirring the polyamic acid to be imidized in an organic solvent in the presence of a basic catalyst and an acid anhydride. As an organic solvent, the above-mentioned organic solvent used in the polymerization reaction can be used. As a basic catalyst, pyridine, triethylamine, trimethylamine, tributylamine, trioctylamine, etc. can be listed. Among them, pyridine has a moderate alkalinity that allows the reaction to proceed, so it is preferred. In addition, as an acid anhydride, acetic anhydride, trimellitic anhydride, pyromellitic anhydride, etc. can be listed, wherein, if acetic anhydride is used, purification after the reaction is completed becomes easy, so it is preferred.
[0110] It should be noted that the imidization rate in this specification refers to the ratio of the imide group to the total amount of the imide group and the carboxyl group (or its derivative) derived from tetracarboxylic dianhydride or its derivative. In polyimide, the imidization rate does not necessarily need to be 100%, and can be prepared arbitrarily according to the use and purpose. The imidization rate of the polyimide used in the present invention is preferably 20% to 100%, and more preferably 50% to 99%.
[0111] The temperature during the imidization reaction is -20 to 140°C, preferably 0 to 100°C, and the reaction time can be 0.5 to 100 hours, preferably 1 to 80 hours. The amount of the basic catalyst is 0.5 to 30 times by mole of the amic acid, preferably 2 to 20 times by mole, and the amount of the acid anhydride is 1 to 50 times by mole of the amic acid, preferably 3 to 30 times by mole. The imidization rate of the obtained polymer can be controlled by adjusting the amount of catalyst, temperature, and reaction time.
[0112] Since the added catalyst etc. remain in the solution after the imidization reaction of polyamic acid ester or polyamic acid, it is preferable to recover the obtained imidized polymer by the method described below, redissolve it in an organic solvent, and use it as (A) component of the liquid crystal aligning agent of this invention.
[0113] The polymer can be precipitated by injecting the polyimide solution obtained as described above into a poor solvent while stirring it well. The precipitation is performed several times, and after washing with a poor solvent, it is dried at room temperature or by heating to obtain a purified polyimide powder.
[0114] The poor solvent is not particularly limited, and examples thereof include methanol, acetone, hexane, butyl cellulose, heptane, methyl ethyl ketone, methyl isobutyl ketone, ethanol, toluene, and benzene.
[0115] <Other ingredients>
[0116] The liquid crystal aligning agent of the present invention may contain components other than the polymer (P) as required. As components other than the polymer (P), for example, there can be listed: polymers other than the polymer (P), crosslinking compounds, functional silane compounds, surfactants, compounds having photopolymerizable groups, organic solvents, etc.
[0117] Polymers other than the polymer (P) can be used for the purpose of improving the solution properties of the liquid crystal alignment agent, the electrical properties of the liquid crystal alignment film, or imparting photo-alignment properties to the liquid crystal alignment film. Examples of the polymer include polyamic acid, polyimide, polyamic acid ester, polyorganosiloxane, polyester, polyamide, polyurea, cellulose derivatives, polyacetals, polystyrene derivatives, poly(styrene-phenylmaleimide) derivatives, and poly(meth)acrylates.
[0118] When adding a polymer other than the polymer (P) to the liquid crystal aligning agent, the blending ratio is preferably 70 parts by mass or less, more preferably 0.1 to 60 parts by mass, further preferably 0.1 to 40 parts by mass, based on 100 parts by mass of all polymer components in the composition.
[0119] The crosslinking compound can be used for the purpose of improving the strength of the liquid crystal alignment film. Examples of the crosslinking compound include: compounds having an epoxy group, an isocyanate group, an epoxy propylene group, or a cyclocarbonate group as described in paragraphs
[0109] to
[0113] of International Publication WO2016 / 047771; or compounds having at least one group selected from the group consisting of a hydroxyl group, a hydroxyalkyl group, and a lower alkoxyalkyl group, and compounds having a blocked isocyanate group.
[0120] Blocked isocyanate compounds are commercially available, and for example, CORONATE APSTABLE M, CORONATE 2503, 2515, 2507, 2513, 2555, MILLIONATE MS-50 (all manufactured by Nippon Polyurethane Industries, Ltd.), TAKENATE B-830, B-815N, B-820NSU, B-842N, B-846N, B-870N, B-874N, B-882N (all manufactured by Mitsui Chemicals, Inc.) and the like can be preferably used.
[0121] Specific examples of preferred crosslinking compounds include compounds represented by the following formulae (CL-1) to (CL-11).
[0122]
[0123] The above is an example of the crosslinking compound, but the invention is not limited thereto. Moreover, the crosslinking compound used for the liquid crystal aligning agent of the present invention may be one kind or a combination of two or more kinds.
[0124] Content of other crosslinking compounds in the liquid crystal aligning agent of this invention is 0.1-150 mass parts, or 0.1-100 mass parts, or 1-50 mass parts with respect to 100 mass parts of all polymer components.
[0125] Functional silane compounds can be used for the purpose of improving the adhesion between the liquid crystal alignment film and the underlying substrate. As a specific example, the silane compounds described in paragraph
[0019] of International Publication Gazette 2014 / 119682 can be cited. The content of the functional silane compound is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 20 parts by mass relative to 100 parts by mass of the total polymer components.
[0126] Surfactants can be used for the purpose of improving the uniformity of the film thickness and surface smoothness of the liquid crystal alignment film. As surfactants, fluorine-based surfactants, silicone-based surfactants, nonionic surfactants, etc. can be listed. Their specific examples can be listed as the surfactants described in paragraph
[0117] of the International Publication WO2016 / 047771. The amount of the surfactant used is preferably 0.01 to 2 parts by mass, more preferably 0.01 to 1 part by mass, relative to 100 parts by mass of all polymer components contained in the liquid crystal alignment agent.
[0127] Examples of the compound having a photopolymerizable group include compounds having one or more polymerizable unsaturated groups such as an acrylate group or a methacrylate group in the molecule, and examples thereof include compounds represented by the following formulae (M-1) to (M-7).
[0128]
[0129] Moreover, in the liquid crystal aligning agent of the present invention, as a compound that promotes the charge transfer in the liquid crystal aligning film and promotes the charge escape of the element, a nitrogen-containing heterocyclic amine compound represented by formula [M1] to formula [M156] described in paragraphs
[0194] to
[0200] of International Publication WO2011 / 132751 (published on October 27, 2011) can be added, and 3-aminomethylpyridine and 4-aminomethylpyridine are more preferably added. The amine compound can be directly added to the liquid crystal aligning agent, preferably after making a solution with a concentration of 0.1 to 10% by mass, preferably 1 to 7% by mass. The solvent is not particularly limited as long as it dissolves the specific polymer (P).
[0130] When a polyamic acid or a polyamic acid ester is contained in the liquid crystal aligning agent of this invention, you may add an imidization accelerator etc. for the purpose of carrying out imidization efficiently by heating at the time of baking a coating film.
[0131] <Organic solvents>
[0132] The liquid crystal aligning agent of the present invention may be prepared as a liquid composition in which the polymer (P) and other components used as necessary are dispersed or dissolved in an appropriate organic solvent.
[0133] Examples of the organic solvent include lactone solvents such as γ-valerolactone and γ-butyrolactone; γ-butyrolactam, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-(n-propyl)-2-pyrrolidone, N-isopropyl-2-pyrrolidone, N-(n-butyl)-2-pyrrolidone, N-(tert-butyl)-2-pyrrolidone, N-(n-pentyl)-2-pyrrolidone, N-methoxypropyl-2-pyrrolidone, N-ethoxyethyl-2-pyrrolidone, N-methoxybutyl N,N-dimethylformamide, N,N-dimethylacetamide, 3-methoxy-N,N-dimethylpropaneamide, 3-butoxy-N,N-dimethylpropaneamide, N,N-dimethyllactamide and other amide solvents; 4-hydroxy-4-methyl-2-pentanone, methyl lactate, ethyl lactate, n-propyl lactate, n-butyl lactate, isopentyl lactate, n-butyl acetate, propylene glycol monoethyl ether, methyl pyruvate, ethyl pyruvate, methyl methyl Oxypropionate, ethyl ethoxypropionate, ethylene glycol monomethyl ether, ethylene glycol ethyl ether, ethylene glycol n-propyl ether, ethylene glycol isopropyl ether, ethylene glycol n-butyl ether (butyl cellosolve), ethylene glycol monobutyl ether acetate, ethylene glycol dimethyl ether, ethylene glycol ethyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monobutyl ether, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, Dipropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, diisobutyl ketone (2,6-dimethyl-4-heptanone), isoamyl propionate, isoamyl isobutyrate, diisopropyl ether, diisoamyl ether; carbonate solvents such as ethylene carbonate and propylene carbonate, 1-hexanol, cyclohexanol, 1,2-ethylene glycol, diisobutyl carbinol (2,6-dimethyl-4-heptanol), propylene glycol diacetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, propyl 3-methoxypropionate, butyl 3-methoxypropionate, etc. These may be used alone or in combination of two or more.
[0134] Preferred combinations of solvents include: N-methyl-2-pyrrolidone, γ-butyrolactone, and ethylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, and propylene glycol monobutyl ether; N-ethyl-2-pyrrolidone and propylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, 4-hydroxy-4-methyl-2-pentanone, and diethylene glycol diethyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether, and diisopropyl ether. butyl ketone; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and diisopropyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and diisobutyl carbinol; N-methyl-2-pyrrolidone, γ-butyrolactone and dipropylene glycol dimethyl ether; N-ethyl-2-pyrrolidone and 4-hydroxy-4-methyl-2-pentanone; N-ethyl-2-pyrrolidone and propylene glycol diacetate; N-methyl-2-pyrrolidone and 3-ethyl ethyl 2-ethoxypropionate; N-ethyl-2-pyrrolidone and ethyl 3-ethoxypropionate; N-methyl-2-pyrrolidone and ethylene glycol monobutyl ether acetate; N-ethyl-2-pyrrolidone and diethylene glycol diethyl ether; N-methyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone and propylene glycol diacetate; N-ethyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone and propylene glycol diacetate; γ-butyrolactone, 4-hydroxy-4-methyl N-methyl-2-pyrrolidone, propylene glycol monobutyl ether and dipropylene glycol dimethyl ether; N-ethyl-2-pyrrolidone, propylene glycol monobutyl ether and dipropylene glycol monomethyl ether; N-ethyl-2-pyrrolidone, propylene glycol monobutyl ether and propylene glycol diacetate; N-ethyl-2-pyrrolidone, propylene glycol monobutyl ether and diisobutyl ketone; N-ethyl-2-pyrrolidone, N,N-dimethyl lactamide and diisobutyl ketone, etc. The type and content of such solvents are appropriately selected according to the coating device, coating conditions, coating environment, etc. of the liquid crystal alignment agent.
[0135] The solid content concentration in the liquid crystal aligning agent (the ratio of the total mass of the components other than the organic solvent of the liquid crystal aligning agent to the total mass of the liquid crystal aligning agent) is appropriately selected in consideration of viscosity, volatility, etc., and is preferably in the range of 1 to 10 mass %.
[0136] The range of particularly preferred solid content concentration varies depending on the method used when applying the liquid crystal alignment agent on the substrate. For example, in the case of spin coating, the solid content concentration is particularly preferably in the range of 1.5 to 4.5% by mass. In the case of printing, it is particularly preferred to set the solid content concentration in the range of 3 to 9% by mass, thereby setting the solution viscosity in the range of 12 to 50 mPa·s. In the case of inkjet method, it is particularly preferred to set the solid content concentration in the range of 1 to 5% by mass, thereby setting the solution viscosity in the range of 3 to 15 mPa·s.
[0137] <Liquid crystal alignment film and liquid crystal display element>
[0138] The liquid crystal alignment film of the present invention is formed by the liquid crystal alignment agent prepared as described above. In addition, the liquid crystal display element of the present invention has a liquid crystal alignment film formed using the above-mentioned liquid crystal alignment agent. The driving mode of the liquid crystal display element is not particularly limited. From the perspective of obtaining the effect of the present invention, TN type, STN type, VA type (including VA-MVA (Multi-domain Vertical Alignment: multi-domain vertical alignment) type, VA-PVA (Patterned Vertical Alignment: patterned vertical alignment) type, etc.) are preferred.
[0139] The liquid crystal display element can be produced, for example, through a process including the following steps (1-1) to (1-3).
[0140] [Step (1-1): Formation of coating film]
[0141] First, a liquid crystal alignment agent is applied to a substrate, and then the applied surface is heated to form a coating film on the substrate. First, two substrates provided with patterned transparent conductive films are used as a pair, and a liquid crystal alignment agent is applied to each transparent conductive film-forming surface thereof by preferably an offset printing method, a spin coating method, a roll coater method, or an inkjet printing method.
[0142] As the substrate, for example, a transparent substrate made of glass such as float glass and soda glass; or plastics such as polyethylene terephthalate, polybutylene terephthalate, polyethersulfone, polycarbonate, and poly(alicyclic olefin) can be used. As a transparent conductive film provided on one side of the substrate, a NESA film (registered trademark of PPG, USA) made of tin oxide (SnO2), an ITO film made of indium oxide-tin oxide (In2O3-SnO2), etc. can be used.
[0143] After the liquid crystal alignment agent is applied, it is preferred to perform preliminary heating (pre-baking) for the purpose of preventing the liquid of the applied liquid crystal alignment agent from dripping. The pre-baking temperature is preferably 30 to 200°C, more preferably 40 to 150°C, and particularly preferably 40 to 100°C. Then, after the solvent is completely removed, and when the liquid crystal alignment agent contains polyamic acid or polyamic acid ester, a calcination (post-baking) process is performed for the purpose of imidization. The calcination temperature (post-baking temperature) at this time is preferably 80 to 300°C, and more preferably 120 to 250°C. The post-baking time is preferably 5 to 200 minutes, and more preferably 10 to 100 minutes. The thickness of the film formed in this way is preferably 1 to 1000 nm, and more preferably 5 to 500 nm.
[0144] [Step (1-2): Orientation-imparting treatment]
[0145] In the case of manufacturing TN type and STN type liquid crystal display elements, the coating film formed in the above step (1-1) is subjected to a treatment for imparting liquid crystal orientation ability. As an orientation ability imparting treatment, there can be cited: for example, a brushing treatment in which a roll made of a cloth composed of fibers such as nylon, rayon, and cotton is used to rub the coating film in a certain direction. On the other hand, in the case of manufacturing a VA type liquid crystal display element, the coating film formed in the above step (1-1) can be directly used as a liquid crystal orientation film, or the coating film can be subjected to an orientation ability imparting treatment.
[0146] The preferred liquid crystal alignment film in the VA type liquid crystal display element can also be preferably used in the PSA (Polymer sustained alignment) type liquid crystal display element. As a method for manufacturing a liquid crystal display element using the liquid crystal alignment agent of the present invention, for example, the following method can be cited: the liquid crystal alignment agent is applied to a pair of substrates having a conductive film to form a coating film, the coating films are arranged oppositely with a liquid crystal molecule layer interposed therebetween to form a liquid crystal box, and the liquid crystal box is irradiated with light while a voltage is applied between the conductive films of the pair of substrates.
[0147] [Step (1-3): Construction of liquid crystal cell]
[0148] (1-3A) As described above, two substrates with liquid crystal alignment films are prepared, and liquid crystal is arranged between the two opposing substrates, thereby manufacturing a liquid crystal box. In order to manufacture a liquid crystal box, for example, the following two methods can be listed. As for the first method, the two substrates are arranged oppositely with a gap (cell gap) separated by each liquid crystal alignment film, and the peripheral parts of the two substrates are bonded together using a sealant. After the liquid crystal is injected into the cell gap divided by the substrate surface and the sealant, the injection hole is sealed, thereby manufacturing a liquid crystal box. In addition, the second method is a method called ODF (One Drop Fill: liquid crystal dripping) method. A sealant such as a UV-curable sealant is applied to a specified location on one of the two substrates with a liquid crystal alignment film, and after liquid crystal is dripped into several specified locations on the surface of the liquid crystal alignment film, the other substrate is bonded in a manner in which the liquid crystal alignment films are opposite, and the liquid crystal is spread to the entire surface of the substrate, and then the entire surface of the substrate is irradiated with ultraviolet light to cure the sealant, thereby manufacturing a liquid crystal box. In the case of using any method, it is desirable that the liquid crystal used is further heated to a temperature at which it becomes isotropic for each liquid crystal cell manufactured as described above, and then slowly cooled to room temperature to remove the flow alignment during liquid crystal filling.
[0149] As the sealant, for example, an epoxy resin containing a curing agent and alumina balls as spacers can be used. As the liquid crystal, nematic liquid crystal and smectic liquid crystal can be mentioned, and among them, nematic liquid crystal is preferred.
[0150] (1-3B) In the case of manufacturing a PSA type liquid crystal display element, a compound having the above-mentioned photopolymerizable group is injected or dripped together with the liquid crystal, and a liquid crystal box is constructed in the same manner as the above (1-3A). At this time, the content of the compound having a photopolymerizable group is preferably 0.01 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the liquid crystal component. After the liquid crystal box is made, while applying an AC or DC voltage to the liquid crystal box, the polymerizable compound is polymerized by heat and ultraviolet irradiation. In this way, the orientation of the liquid crystal molecules can be controlled. Then, the liquid crystal box is irradiated with light while a voltage is applied between the conductive films of a pair of substrates. Here, the applied voltage can be set to, for example, a DC or AC of 5 to 50V. In addition, as the irradiated light, ultraviolet light containing a wavelength of 300 to 400nm is preferred. As a light source for the irradiated light, for example, a low-pressure mercury lamp, a high-pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, an excimer laser, etc. can be used. The light irradiation dose is preferably 1000 J / m 2 Above and less than 200000J / m 2 , more preferably 1000 to 100000 J / m 2 .
[0151] (1-3C) When a coating film is formed on a substrate using a liquid crystal alignment agent containing a compound having a photopolymerizable group, the following method can also be used: a liquid crystal box is constructed in the same manner as in the above (1-3A), and then a liquid crystal display element is manufactured by irradiating the liquid crystal box with light while a voltage is applied between the conductive films of a pair of substrates. At this time, the content of the compound having a photopolymerizable group is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, relative to 100 parts by mass of all polymer components. According to this method, the advantages of the PSA mode can be achieved with a small amount of light irradiation. The conditions of the applied voltage and the irradiated light can be applied to the description of the above (1-3B).
[0152] Furthermore, a liquid crystal display element can be obtained by attaching a polarizing plate to the outer surface of the liquid crystal cell. Examples of the polarizing plate attached to the outer surface of the liquid crystal cell include a polarizing plate formed by sandwiching a polarizing film called "H film" that stretches and orients polyvinyl alcohol and absorbs iodine with a cellulose acetate protective film, or a polarizing plate composed of the H film itself.
[0153] Example
[0154] The present invention will be described in further detail below with reference to Examples, but the present invention is not limited thereto. The meanings of the abbreviations of the compounds used in the Examples are shown below.
[0155] (Tetracarboxylic dianhydride)
[0156] BODA: bicyclo[3,3,0]octane-2,4,6,8-tetracarboxylic dianhydride.
[0157] CBDA: 1,2,3,4-cyclobutanetetracarboxylic dianhydride.
[0158] (Diamine)
[0159] m-PDA: 1,3-phenylenediamine.
[0160]
[0161] (Solvent)
[0162] NMP: N-methyl-2-pyrrolidone.
[0163] BCS: Butyl Cellosolve.
[0164] THF: tetrahydrofuran.
[0165] <Determination of Molecular Weight of Polyimide>
[0166] Measuring apparatus: Normal temperature gel permeation chromatography (GPC) (SSC-7200) manufactured by SENSHU Scientific Co., Ltd.
[0167] Chromatographic column: chromatographic column manufactured by Shodex (KD-803, KD-805), chromatographic column temperature: 50°C.
[0168] Eluent: N,N'-dimethylformamide (as additives, lithium bromide monohydrate (LiBr·H2O) is 30 mmol / L, phosphoric acid / anhydrous crystals (o-phosphoric acid) is 30 mmol / L, and tetrahydrofuran (THF) is 10 ml / L).
[0169] Flow rate: 1.0 ml / min.
[0170] Standard samples for preparing the calibration curve: TSK standard polyethylene oxide manufactured by Tosoh Corporation (molecular weight of about 9,000,000, 150,000, 100,000, and 30,000); and polyethylene glycol manufactured by Polymer Laboratory (molecular weight of about 12,000, 4,000, and 1,000).
[0171] <Determination of chemical imidization rate>
[0172] 20 mg of polyimide powder was added to an NMR sample tube (NMR standard sampling tube φ5 manufactured by Kusano Scientific Co., Ltd.), 1.0 ml of deuterated dimethyl sulfoxide (DMSO-d6, 0.05% TMS mixed product) was added, and ultrasonic waves were applied to completely dissolve it. The solution was measured for 500 MHz proton NMR using an NMR measuring instrument (JNW-ECA500) manufactured by DATUM, Japan Electronics Co., Ltd. The imidization rate was calculated as follows: the proton derived from the structure that did not change before and after imidization was determined as the reference proton, and the peak integral value of the proton derived from the NH group of the amic acid appearing around 9.5 to 10.0 ppm was used to calculate it using the following formula. It should be noted that in the formula, x is the peak integral value of the proton derived from the NH group of the amic acid, y is the peak integral value of the reference proton, and α is the ratio of the number of reference protons to the protons of one NH group of the amic acid in the case of polyamic acid (imidization rate 0%).
[0173] Chemical imidization rate (%) = (1-α·x / y) × 100
[0174] DA-S1 is a novel compound, and its synthesis method is described in detail below.
[0175] The product described in the following Monomer Synthesis Example 1 was identified by 1H-NMR analysis. The analysis conditions were as follows.
[0176] Apparatus: Varian NMR System 400NB (400 MHz).
[0177] Determination solvent: CDCl3.
[0178] Reference substance: tetramethylsilane (TMS) (δ0.0 ppm for 1H).
[0179] <Synthesis of Monomer Synthesis Example DA-S1>
[0180]
[0181] Synthesis of compound 3 (mixture of 3a and 3b)
[0182] Magnesium (15.39 g, 63.3 mmol, 1.5 eq.) was added to a four-necked flask, and after vacuum drying for 1 hour in a vacuum pump, THF (100 g) was added using a syringe and stirred at room temperature. Then, a solution of compound 1 (100 g, 42.2 mmol) in THF (300 g) was slowly added dropwise at a rate of about stable reflux. Then, the reaction solution was cooled to 0°C, and a solution of compound 2 (105.60 g, 42.2 mmol, 1.0 eq.) in THF (200 g) was added dropwise. After the addition was completed, the temperature of the reaction solution was returned to room temperature, and stirred at room temperature for 3 hours. Then, toluene (1 L) was added to dilute the reaction solution, and the reaction solution was cooled to 0°C again, and a 10% acetic acid solution (500 g) was slowly added dropwise.
[0183] Then, the water layer was removed by liquid separation, and the organic layer was washed with saturated saline (1 L), saturated sodium bicarbonate solution (1 L), and saturated saline (1 L), and the organic layer was dried with anhydrous magnesium sulfate. Then, the mixture was filtered and distilled off using an evaporator to obtain 172 g of crude crystals of compound 3. The obtained crude crystals were directly used for the following reaction.
[0184] Synthesis of compound 4
[0185] A mixture of compound 3 (172 g, 422 mmol) as crude crystals and p-toluenesulfonic acid monohydrate (4.82 g, 25.3 mmol, 0.06 eq.) in dehydrated toluene (MS4A dehydrated product, 2 L) was reacted for 2 hours under reflux while removing water. After the reaction was completed, about half of the toluene used was distilled off in an evaporator, and the solution was stirred at room temperature to precipitate solids. The obtained solids were filtered to obtain crystals of compound 4 (yield 150 g, yield 91%).
[0186] Synthesis of compound 5 (mixture of 5a and 5b)
[0187] A mixture of compound 4 (108 g, 276 mmol), 5% palladium carbon powder (containing water, 11 g, 10 wt%), ethyl acetate (1 L), and ethanol (1 L) was stirred at room temperature in the presence of hydrogen. After the reaction was completed, toluene (2 L) was added to dissolve the crystals, and the reaction mixture was filtered using celite, and the celite was washed with 1 L of toluene. The filtrate was concentrated under reduced pressure, and as a result, the target compound 5 (yield 103.3 g, yield 95%) was obtained.
[0188] Synthesis of compound 6
[0189] To a solution of compound 5 (95.4 g, 243 mmol) in dichloromethane (800 mL) at 0°C under nitrogen substitution, add BBr3 (1.0 M-CH2Cl2, 243 mL, 1.01 mol). After the addition, stir at 0°C for 2 hours. After the reaction is completed, add the reaction solution to distilled water in small amounts each time. Extract with ethyl acetate (1 L), and wash the extract twice with 500 mL of distilled water. After drying the organic layer with magnesium sulfate, distill off the solvent under reduced pressure. The resulting crude product is recrystallized in ethanol, filtered, and washed with ethanol. As a result, the target compound 6 (yield 18.6 g, yield 21%) is obtained.
[0190] Synthesis of compound 8
[0191] To a mixture of compound 6 (10.0 g, 26.4 mmol), potassium carbonate (11.0 g, 79.2 mmol, 3 eq.), and toluene (50 g), a toluene (20 g) solution of compound 7 (5.35 g, 26.4 mmol) was added dropwise under reflux. After the addition, the mixture was stirred overnight under reflux. After the reaction was completed, the reaction solution was cooled to about 60°C, ethyl acetate (500 g) was added, and the mixture was washed three times with distilled water. After the organic layer was dried with anhydrous magnesium sulfate, the solvent was distilled off under reduced pressure. The obtained crude product was recrystallized in an acetonitrile / ethanol (2:1) solution, filtered, and the filtered crystals were washed with ethanol to obtain crude crystals of compound 8. The crude crystals were purified by column chromatography (SiO2, CHCl3) to obtain crystals of compound 8 (yield 7.1 g, yield 49%).
[0192] Synthesis of DA-S1
[0193] A mixture of compound 8 (12.2 g, 22.4 mmol), 5% palladium carbon powder (water-containing product 1.22 g, 10 wt%), and dioxane (120 g) was stirred at 60°C for 4 hours in the presence of hydrogen. After the reaction was completed, nitrogen substitution was performed and the mixture was filtered using diatomaceous earth while maintaining the temperature at 60°C. The filtrate was distilled under reduced pressure to remove the solvent, and as a result, a crude product was obtained. The crude product was recrystallized from 2-propanol / ethyl acetate (2:1) to obtain the target product DA-S1 (yield 8.0 g, yield 74%).
[0194] 1H NMR (CDCl3, δppm): 7.725 (1H, d), 7.577 (2H, m), 7.272 (2H, m), 7.102 (1H, s), 6.791 (1H, d ), 6.207 (1H, d), 6.117 (1H, dd), 3.621 (4H, broad), 2.553 (1H, m), 2.067-0.863 (31H, m).
[0195] <Synthesis example 1>
[0196] BODA (1.50 g, 6.00 mmol), m-PDA (0.78 g, 7.20 mmol) and DA-S1 (2.33 g, 4.80 mmol) were dissolved in NMP (18.4 g), and reacted at 60 ° C for 3 hours. Then, CBDA (1.15 g, 5.88 mmol) and NMP (4.60 g) were added, and the reaction was carried out at 40 ° C for 6 hours to obtain a polyamic acid solution. After adding NMP to the polyamic acid solution (23.0 g) to dilute it to 6.5% by mass, acetic anhydride (4.87 g) and pyridine (1.51 g) as imidization catalysts were added, and the reaction was carried out at 80 ° C for 2.5 hours. The reaction solution was put into methanol (270 g) and the obtained precipitate was filtered out. The precipitate was washed with methanol and dried under reduced pressure at 60 ° C to obtain a polyimide powder. The chemical imidization rate of the polyimide was 82%, Mn was 14,100, and Mw was 51,800.
[0197] NMP (24.3 g) was added to the obtained polyimide powder (2.7 g), and it stirred at 70 degreeC for 12 hours and dissolved. BCS (18.0g) was added to this solution, and it stirred at room temperature for 2 hours, and obtained the liquid crystal aligning agent SPI-1.
[0198] <Synthesis example 2>
[0199] BODA (2.75 g, 11.0 mmol), m-PDA (1.43 g, 13.2 mmol) and DA-S2 (3.83 g, 8.80 mmol) were dissolved in NMP (32.0 g), and reacted at 60 ° C for 3 hours. Then, CBDA (2.11 g, 10.8 mmol) and NMP (8.50 g) were added, and the reaction was carried out at 40 ° C for 6 hours to obtain a polyamic acid solution. After adding NMP to the polyamic acid solution (44.6 g) to dilute it to 6.5% by mass, acetic anhydride (9.86 g) and pyridine (3.06 g) as imidization catalysts were added, and the reaction was carried out at 80 ° C for 2.5 hours. The reaction solution was put into methanol (526 g) and the obtained precipitate was filtered out. The precipitate was washed with methanol and dried under reduced pressure at 60 ° C to obtain a polyimide powder. The chemical imidization rate of the polyimide was 78%, Mn was 13,700, and Mw was 47,400.
[0200] NMP (24.3 g) was added to the obtained polyimide powder (2.7 g), and it stirred at 70 degreeC for 12 hours and dissolved. BCS (18.0 g) was added to this solution, and it stirred at room temperature for 2 hours, and obtained the liquid crystal aligning agent SPI-2.
[0201] <Synthesis example 3>
[0202] BODA (2.75 g, 11.0 mmol), m-PDA (1.43 g, 13.2 mmol) and DA-S3 (3.35 g, 8.80 mmol) were dissolved in NMP (30.1 g), and reacted at 60 ° C for 3 hours. Then, CBDA (2.11 g, 10.8 mmol) and NMP (8.50 g) were added, and the reaction was carried out at 40 ° C for 6 hours to obtain a polyamic acid solution. After adding NMP to the polyamic acid solution (42 g) to dilute it to 6.5% by mass, acetic anhydride (9.74 g) and pyridine (3.02 g) as imidization catalysts were added, and the reaction was carried out at 80 ° C for 2.5 hours. The reaction solution was put into methanol (497 g) and the obtained precipitate was filtered out. The precipitate was washed with methanol and dried under reduced pressure at 60 ° C to obtain a polyimide powder. The chemical imidization rate of the polyimide was 70%, Mn was 15,400, and Mw was 51,200.
[0203] NMP (24.3 g) was added to the obtained polyimide powder (2.7 g), and it stirred at 70 degreeC for 12 hours and dissolved. BCS (18.0 g) was added to this solution, and it stirred at room temperature for 2 hours, and obtained the liquid crystal aligning agent SPI-3.
[0204] [Table 1]
[0205]
[0206] <Example 1>
[0207] Using the liquid crystal aligning agent SPI-1 obtained in Synthesis Example 1, a liquid crystal cell was prepared in the following procedure.
[0208] The liquid crystal alignment agent SPI-1 obtained in Synthesis Example 1 was spin-coated on a glass substrate with an ITO electrode and a substrate with an ITO electrode pattern with a line width / line spacing of 500 μm, and dried on a hot plate at 80°C for 90 seconds, and then fired in a hot air circulation oven at 230°C for 30 minutes, or set to severe conditions for 90 minutes to form a liquid crystal alignment film with a film thickness of 100 nm. 4 μm bead spacers were spread on the liquid crystal alignment film on one side, and a thermosetting sealant (XN-1500T manufactured by Kyoritsu Chemical Co., Ltd.) was further printed. Next, the surface of the other substrate on which the liquid crystal alignment film was formed was used as the inner side, and after being bonded to the previous substrate, the sealant was cured to produce an empty box. Liquid crystal MLC-3023 (trade name manufactured by MERCK Co., Ltd.) containing a polymerizable compound for PSA was injected into the empty box by a reduced pressure injection method to produce a liquid crystal box. Then, the obtained liquid crystal box was subjected to PSA treatment and the pretilt angle was measured.
[0209] [PSA treatment]
[0210] With a DC voltage of 15 V applied, 10 J / cm 2 UV that passed through the cutoff filter below 325nm. It should be noted that, in terms of UV illumination, a UV-35 light receiver was connected to UV-MO3A manufactured by ORC. Then, in order to deactivate the unreacted polymerizable compound remaining in the liquid crystal box, UV was irradiated for 30 minutes using a UV-FL irradiation device manufactured by Toshiba Lighting & Technology without applying voltage (UV lamp: FLR40SUV32 / A-1).
[0211] [Pretilt angle measurement]
[0212] The pretilt angle of the cell produced above was measured using an LCD analyzer (LCA-LUV42A manufactured by Meiling Technica Corporation).
[0213] <Comparative Examples 1 and 2>
[0214] Each liquid crystal cell was produced in the same manner as in Example 1 except that SPI-2 and SPI-3 were used instead of the liquid crystal aligning agent SPI-1, and the pretilt angle was measured after the PSA treatment.
[0215] [Table 2]
[0216]
[0217] As shown in Table 2, it was confirmed that: for Comparative Examples 1 and 2 using liquid crystal alignment agents SPI-2 and SPI-3 containing diamines having a vertical alignment side chain without a naphthylene group, the difference between the pretilt angle under the severe condition and the standard condition was large, while on the other hand, for Example 1 using liquid crystal alignment agent SPI-1 containing diamines having a vertical alignment side chain DA-S1 having a naphthylene group, the difference between the pretilt angles under the severe condition and the standard condition was extremely small. It can be seen that the liquid crystal alignment agent containing diamines having a vertical alignment side chain having a naphthylene group can obtain a liquid crystal alignment film having a high ability to align the liquid crystal even when exposed to excessive heating.
[0218] It should be noted that all the contents of the specification, claims, and abstract of Japanese Patent Application No. 2019-173214 filed on September 24, 2019 are cited herein and introduced as a disclosure of the specification of the present invention.
Claims
1. A liquid crystal aligning agent comprising at least one polymer (P) selected from the group consisting of a polyimide precursor obtained from a diamine component containing a diamine represented by the following formula (2-1) and a polyimide, In formula (2-1), X 11 represents an alkylene group having 1 carbon atom, which may be substituted by -O- or -COO-; X 12 represents a single bond; Q1 represents a naphthylene group, Y1 represents two cyclohexylene groups; R1 represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms.
2. The liquid crystal alignment agent according to claim 1, wherein The diamine represented by the formula (2-1) is at least one diamine selected from the group consisting of diamines represented by the following formulae (d-1) to (d-2) and (d-4) to (d-5), Here, m represents 2; n represents 3, 5 or 7; and c represents 1.
3. The liquid crystal aligning agent according to claim 1 or 2, wherein: The polymer (P) is at least one polymer selected from the group consisting of a polyimide precursor obtained by polymerization reaction of a diamine component including a diamine represented by the formula (2-1) and a tetracarboxylic acid component, and a polyimide obtained by imidating the polyimide precursor.
4. The liquid crystal alignment agent according to claim 3, wherein: The tetracarboxylic acid component includes tetracarboxylic dianhydride represented by the following formula (3): X represents a structure selected from any of the following (x-1) to (x-13), In formulas (x-1) to (x-13), R 1 ~R 4 Each independently represents a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom or a benzene ring; R 5 and R 6 Each independently represents a hydrogen atom or a methyl group; j and k each independently represent 0 or 1; A1 and A2 each independently represent a single bond, an ether group, a carbonyl group, an ester group, a phenylene group, a sulfonyl group or an amide group; *1 represents a bond to the acid anhydride group of one side, and *2 represents a bond to the acid anhydride group of the other side.
5. The liquid crystal aligning agent according to claim 1 or 2, wherein The diamine represented by the above formula (2-1) accounts for 10 to 80 mol% in 100 mol% of all diamine components.
6. The liquid crystal aligning agent according to claim 1 or 2, wherein: Content of the said polymer (P) is 1-10 mass % with respect to the total mass of a liquid crystal aligning agent.
7. A liquid crystal alignment film, characterized in that: The liquid crystal aligning agent according to any one of claims 1 to 6 is used.
8. A liquid crystal display element, characterized in that: A liquid crystal alignment film according to claim 7 is provided.
9. A method for manufacturing a liquid crystal display element, which is the following method: The liquid crystal alignment agent described in any one of claims 1 to 6 is applied onto a pair of substrates having a conductive film to form a coating film, the coating films are arranged opposite to each other with a liquid crystal molecule layer interposed therebetween to form a liquid crystal box, and the liquid crystal box is irradiated with light while a voltage is applied between the conductive films of the pair of substrates.
10. A diamine represented by the following formula (2-1): The definitions of the symbols are the same as those in claim 1.
11. A polymer obtained from a diamine component comprising at least one diamine as defined in claim 10.
12. The polymer according to claim 11, wherein The polymer is at least one polymer selected from the group consisting of a polyimide precursor and a polyimide obtained by imidating the polyimide precursor.
Citation Information
Patent Citations
Liquid crystal display device
JP2003307720A
Beating apparatus for loom, and motor control method in beating apparatus for loom
JP2019173214A
Liquid-crystal alignment material for vertical alignment, liquid-crystal alignment film, and liquid-crystal display element employing the same
WO2006070819A1
Liquid-crystal alignment agent, liquid-crystal alignment film, and liquid-crystal display element
WO2011132751A1
Liquid crystal aligning agent, liquid crystal alignment film, and liquid crystal display element
WO2014119682A1