A device and process for fully automatic electric pulse combined segment welding of different metal pipes

Through fully automatic electrical pulse combined segmented welding device, combined with Tig, Mag, and Mig welding technologies, high-energy electrical pulses and PC control systems, the problems of welding speed instability and roughening of weld structure in different metal welding are solved, and the problem of welding speed instability and weld structure is achieved. Efficient and rapid welding process reduces costs and improves welding quality and efficiency.

CN114473151BActive Publication Date: 2024-12-06CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210036105.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-12
Publication Date
2024-12-06
Estimated Expiration
2042-01-12

AI Technical Summary

Technical Problem

The existing different metal welding process has the phenomenon of undercutting and overfiring caused by instability in welding speed, and the weld structure tends to be roughened, segregated and cracked. The heat treatment after welding takes a long time and is costly, making it difficult to meet the needs of efficient and rapid welding of materials. .

Method used

Adopt fully automatic electrical pulse combined segment welding device, combined with Tig, Mag, and Mig welding technologies, use high-energy electrical pulses to improve welding structure, and realize intelligent and automated welding process management through PC control system, including eddy current heating, electrical pulse processing and Quenching system, optimize welding parameters to improve welding efficiency and quality.

Benefits of technology

It effectively solves the problems of welding speed instability and weld structure, reduces welding costs, improves welding efficiency and the mechanical properties of the finished products, reduces welding thermal stress, and significantly improves the microstructure morphology and mechanical properties of the weld.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114473151B_ABST
    Figure CN114473151B_ABST
Patent Text Reader

Abstract

The invention discloses a device and a process for fully automatic electric pulse combined segmented welding of different metal pipes. The device comprises a heating system and a welding system. The electric pulse system comprises an eddy current coil for pre-treating eddy current heating of a workpiece to be welded. The welding system comprises a Tig welding gun, a Mag welding gun, a Mig welding gun, and a bearing rotating device, wherein the Tig welding gun, the Mag welding gun, and the Mig welding gun are installed on the bearing rotating device, and the bearing rotating device is used to automatically rotate and select the welding gun to weld the workpiece to be welded. The electric pulse system comprises a high-frequency pulse power supply and a graphite brush rod, and the graphite brush rod is used to connect the high-frequency pulse power supply to provide electric pulse current to the welded piece. The device of the invention can be used in the welding process between the same or different metals such as steel, cast iron and non-ferrous metals to prevent grain coarsening and segregation, improve the mechanical properties of the welding structure, and is simple to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding and forming of metal pipes, and in particular to a device and a process for fully automatic electric pulse combined segmented welding of butt joints of different metal pipes. Background Art

[0002] With the development, mining, machinery, metallurgy and other industries have put forward higher and higher requirements on the performance and mechanical properties of materials. As mining, machinery, metallurgy and other industries, they have certain requirements on the hardness, strength and plasticity of materials. However, there is an exclusive relationship between the strength, hardness and plasticity of materials. Improving the strength and hardness of materials cannot meet the toughness of materials, and vice versa, the strength and hardness of materials cannot be guaranteed. In order to ensure the service life of equipment, welding of dissimilar metals is usually adopted, that is, welding materials with higher strength and hardness with materials with higher plasticity and toughness.

[0003] Although the mechanical properties of a single material have been greatly developed under the efforts of scientific researchers, the research progress on welding of different materials is relatively slow, and more research is done on the influence of post-weld heat treatment process on the structure and performance of welding materials. This is because the thermal effect of the welding structure during the welding process causes a large amount of thermal stress in the welding area, and the grains of the welding structure are relatively coarse. Although the structure is regulated by a certain post-weld heat treatment, this process not only requires a lot of insulation time, resulting in a significant increase in cost and reduced efficiency, but also still has a network structure and segregation, which makes the plastic toughness of the material increase slightly.

[0004] At present, the main welding method for dissimilar steels is Mag welding. After the pipe to be welded is heated to a certain temperature by a flame spray gun, the Mag welding gun is used for base filling, and air cooling is performed after the filling is completed; the subsequent heat treatment process, such as annealing, tempering, normalizing and other processes are used for organizational regulation by a heat treatment furnace. This process has certain shortcomings, such as: a. A large amount of manpower is required to operate each process, which reduces the efficiency of the entire welding process and increases the labor cost; b. Heating by a flame spray gun causes a large amount of oxide scale to form in the area to be welded, which seriously affects the fusion process of the weld structure and reduces the mechanical properties of the material, and is prone to cracking; c. Since the workpiece needs to be heat treated after welding, this limits the size of the workpiece. If the size is too large, the heat treatment process cannot be performed, and the heat treatment process will affect the microstructure of the entire workpiece and change the performance of the entire workpiece. d. The Mag welding process has high requirements for the welding speed. When the welding speed is high, undercutting and overburning often occur in the welding area, making it impossible for the welding wire to completely fill the V-shaped groove. The mechanical properties of the molten metal between passes are poor and it is very easy to crack. When the welding speed exceeds the critical value, periodic fluctuations will appear on the weld surface, which will destroy the strength and performance of the weld joint and cause low continuity of the weld metal.

[0005] Under the requirements of the industry, not only higher requirements are placed on welding organization, but more importantly, higher requirements are placed on welding equipment.

[0006] As a new process that can improve material structure and performance quickly and effectively, the current main work of high-energy electric pulse technology focuses on the following three aspects:

[0007] 1) High-energy electric pulse treatment of solid metals can control the microstructural evolution and performance of materials;

[0008] 2) High-energy electric pulse treatment is performed on the liquid metal solidification process. When the metal material is in the solid-liquid two-phase region, high-energy electric pulse treatment can significantly improve the cast structure of the material, accelerate the formation of crystal nuclei, and inhibit grain growth, thereby obtaining uniform and refined grains.

[0009] 3) High-energy electric pulse treatment of molten metal can effectively refine grains, reduce segregation, and change the microstructural morphology.

[0010] Its working principle is to apply high-energy pulse current on both sides of the metal material, that is, the pulse power supply inputs the pulse current into the powered area of ​​the metal material moving between the two electrodes through two electrodes, and the pulse current produces a coupling effect of Joule heating effect and non-thermal effect in the powered area of ​​the metal material. The pulse current can significantly promote the atomic diffusion in the material and the strong interaction with defects (vacancies, dislocations, grain boundaries), and can improve the material's organizational structure by quickly inducing recovery, recrystallization, phase change and other behaviors, control the solidification organization of the metal material, refine the grains, improve the diffusion capacity of the elements, and promote the uniform distribution of the hard phase in the metal material; at the same time, because the high-energy electric pulse is transmitted through the pulse current between the two electrodes, it can only regulate the mechanical properties and processing properties of the material in the target area.

[0011] Tig welding is a simple and flexible welding method. During the welding process, the weld area is protected by pure argon gas and contacts the welding wire to generate a welding arc to fill the weld area. This welding process has a wide range of applications and can be used for welding more complex parts. At the same time, due to the low energy density of the heat source generated during the welding process, the heat affected zone is larger. During the welding process, due to the influence of thermal cycles, the grain size of the parent material on both sides of the weld is larger, which reduces the mechanical properties of the welded joint.

[0012] At present, there are many process methods for welding the same metal materials, but there are few studies on welding methods for dissimilar metal materials. The patent application document with patent number CN103521887A discloses a welding process for 45 steel and 35CrMo cast steel. The process adopts a single Mag welding process method. During the welding process, a wind shovel is used to impact each weld to preliminarily eliminate the stress generated during the welding process, and finally the stress retained in the welding machine area during the welding process is further eliminated by post-welding insulation. The patent application document with patent number CN109396695B discloses a fastener and workpiece for MIG brazing and flame brazing and a method for making the same. The process proposes a welding process such as MAG welding, TIG welding, and MIG welding by continuously replacing the welding power supply and its corresponding welding gun. These process methods are cumbersome to operate and require manpower to manually change the welding gun head, which is not much different from multiple welding guns.

[0013] However, for heterogeneous alloy steels, a single welding method cannot guarantee the structure and performance of the weld area. Combined with the subsequent heat preservation treatment, a lot of heat preservation time is consumed, which increases the labor cost and the weld structure still cannot achieve the optimal result. Therefore, how to solve the series of problems existing in the existing heterogeneous metal pipe welding process equipment, improve the microstructure morphology and mechanical properties of the weld area, and reduce the cracking tendency of the material due to particle coarsening, segregation, inclusions and other phenomena, it is particularly important to develop an efficient, fast and intelligent welding equipment for the butt joint of homogeneous or heterogeneous metal pipes. Summary of the invention

[0014] In view of the shortcomings of the prior art, the present invention, in line with the goals of energy saving, efficiency improvement and carbon neutrality, provides a device and process for fully automatic electric pulse combined segmented welding of different metal pipes; to solve the problems of undercut and overburning caused by the instability of welding speed in Mag welding, Mig welding and Tig welding, reduce the cracking tendency of materials caused by particle coarsening, segregation, inclusions and other phenomena, and improve the working efficiency of existing welding processes and equipment during the welding process.

[0015] To achieve the above object, the present invention adopts the following technical solution:

[0016] The present invention discloses a device for fully automatic electric pulse combined segmented welding of different metal pipes for intelligent docking, comprising two spinning machines, a heating system, a welding system, an electric pulse system, and a quenching system; the spinning machine is used to fix a workpiece to be welded; the heating system comprises an eddy current coil, which is used to perform eddy current heating pretreatment on the workpiece to be welded; the welding system comprises a Tig welding gun, a Mag welding gun, a Mig welding gun, and a bearing rotating device, wherein the Tig welding gun, the Mag welding gun, and the Mig welding gun are installed on the bearing rotating device, and the bearing rotating device is used to automatically rotate and select the welding gun to weld the workpiece to be welded; the electric pulse system comprises a high-frequency pulse power supply and a graphite brush rod, and the graphite brush rod is used to connect the high-frequency pulse power supply to provide electric pulse current to the welded piece; the quenching system is used to quench the welded piece after the electric pulse treatment.

[0017] The fully automatic electric pulse combined segmented welding provided by the present invention mainly integrates the welding system and the electric pulse system, so that after the workpiece to be welded is welded, the electric pulse heat treatment can be directly performed, and the Joule heat effect of the high-energy electric pulse is used to improve the grain coarsening and segregation phenomena that occur during Mag welding, Mig welding, and Tig welding.

[0018] The heating system of the present invention includes an eddy current coil, and the surface of the material to be welded is heated uniformly to a high degree; and the heating rate and the holding time during the heating process are monitored by an infrared temperature measuring gun, and the temperature-time curve is transmitted to the PC control system in real time through an electrical signal. At the same time, after the preheating is completed, the PC control system is used to control the automatic control of the eddy current induction heating coil to perform translational movement and return to the initial position to prevent interference with the subsequent welding process and the electric pulse process.

[0019] In a preferred solution, the device further comprises a PC control system, and the PC control system is used to issue instructions for controlling other systems.

[0020] In a preferred solution, the device further comprises an electric control box, which comprises a DC power supply, an AC power supply and a transformer, and is used to supply power to the device.

[0021] In the actual operation process of the present invention, the electric control box is used to supply power to the PC control system, the spinning machine, the electric pulse system, the welding system, the support transmission system, the quenching system, the heating system, the temperature measurement system, and the rotating clamping fixed support seat, so that the instructions issued by the PC control system are transmitted to the corresponding components to control the rotational angular velocity of the spinning machine; the corresponding pulse current frequency, current density, power-on time, heating rate, heating time and other signals are provided to the electric pulse system; the corresponding welding gun muzzle and mixed gas are selected according to the instruction program, the welding stroke is determined according to the power-on time, and the welding current and welding voltage are controlled; the corresponding quenching medium and the injection cooling time are selected according to the instruction program; the voltage and current of the eddy current coil in the heating system are controlled according to the instruction program, and the heating temperature, heating rate, and insulation time are controlled, and instructions are issued at the same time to enable the temperature measurement system to perform real-time temperature monitoring of the weld.

[0022] The preferred solution is that the two spinning machines are divided into a left spinning machine 1 # And the spinning machine 2 on the right # , the spinning machine 1 # Used to fix the workpiece to be welded 1 # , Spinning Machine 2 # Used to fix the workpiece to be welded 2 # Any spinning machine includes a spindle, a chuck, a spinning core mold, a clamping device, and a spinning handle; the chuck is installed on the spindle, clamping the rotating core mold and combining the clamping device and the spinning handle to clamp and fix the workpiece to be welded.

[0023] In a preferred embodiment, the device further includes a support transmission system and a base; the support transmission system includes a support pulley located at the top, a guide pulley located at the bottom and a support rod, the top support pulley and the bottom guide pulley are fixed to the top and bottom ends of the support rod and placed in the guide groove of the base, the top support pulley cooperates with the spinning machine to rotate the workpiece 360°, and the bottom guide pulley is used to control the workpiece to be welded to be fixed on the spinning machine.

[0024] Preferably, the device further comprises a temperature measuring system, wherein the temperature measuring system comprises an external-line temperature measuring instrument, and the external-line temperature measuring instrument is a bidirectional gun head, facing respectively the graphite brush rod of the electric pulse system and the composite welding gun head in the welding system.

[0025] In actual operation, the guide pulley in the heating system is controlled to move forward to the heating area according to the instructions issued by the PC control system, and then energized. Eddy current heating is performed according to the set temperature, and an infrared thermometer is used to monitor the weld and the surrounding 30mm in real time.

[0026] Preferably, the welding system further comprises a mixed gas flow guiding device and a tungsten electrode.

[0027] The welding system of the present invention adopts "one electrode, three gun muzzles, and three nozzles" in a ring-shaped package, and uses a bearing rotating device to integrate the Mag welding gun, Mig welding gun, Tig welding gun and their corresponding protective gases. According to the corresponding instructions issued by the PC control system, the corresponding welding gun is selected to perform welding work.

[0028] During the welding process, the corresponding shielding gas is sprayed out in cooperation with the mixed gas guide device according to the welding gun used to protect the welding process.

[0029] According to a preferred embodiment, the device further comprises a rotating clamping and fixing support seat, which is used to clamp and fix the graphite brush rod of the electric pulse system, the composite welding gun of the welding system, the infrared temperature measuring gun of the temperature measuring system, and the quenching nozzle rotating device of the quenching system, wherein the electric pulse system and the welding system are distributed 180° in opposite directions, the infrared temperature measuring gun of the temperature measuring system is fixed at the center position of the rotating clamping and fixing support seat; the quenching system is fixed in the middle of the rotating clamping and fixing support seat.

[0030] In actual operation, the electric pulse system starts working after welding is completed. The connection process of the high-energy electric pulse electrode is initiated by the PC control system sending instructions to the rotating clamping support. When the graphite brush rod contacts the pipe to be welded, it stops rotating and then the pulse power supply is turned on. The pulse current frequency, current density, pulse width, power-on time, heating rate and other signals set by the PC control system are used to work on the energized area of ​​the pipe.

[0031] A preferred solution is that the quenching system includes a liquid guide tube, a distribution nozzle, a control valve, and a nozzle rotating device. The liquid guide tube, the distribution nozzle and the control valve are fixed in the nozzle rotating device. The rotating device is fixed in the middle of a rotating clamping fixed support seat. The distribution nozzle is a single-phase nozzle, facing the graphite brush rod of the electric pulse system.

[0032] In the actual operation process, according to the instructions issued by the PC control system, the nozzle equipped with the corresponding quenching medium is automatically selected for quenching.

[0033] The present invention provides a fully automatic electric pulse combined segmented welding process for intelligently butting different metal pipes, comprising the following steps:

[0034] The workpiece to be welded 1 # 、Workpiece to be welded 2 # The grooves are pre-cut, and then fixed on a spinning machine and positioned to form a welding area. The welding area is pre-treated by eddy current heating, and then welded to obtain the welding area. Finally, the welding area is subjected to electric pulse treatment and quenching treatment to obtain a welded product. The welding method is selected from at least one of Mag welding process, Tig welding process, and Mig welding process.

[0035] In a preferred embodiment, the workpiece to be welded 1 # With the workpiece to be welded 2 # The materials of the workpiece to be welded are different. # With the workpiece to be welded 2 # The material of the workpiece to be welded is selected from Q890 or 42CrMoA. # With the workpiece to be welded 2 # The thickness is ≤40mm, preferably the thickness is ≤30mm.

[0036] In a preferred embodiment, the workpiece to be welded 1 # With the workpiece to be welded 2 # The grooves are all pre-opened with a 10-25° groove, preferably a 15-20° groove.

[0037] The preferred solution is that the swing positioning is to place the workpiece 1 to be welded with a groove # With the workpiece to be welded 2 # The butt joint is made in a V-shaped groove, and the space gap of the butt joint is controlled within 5 mm, preferably within 3 mm.

[0038] In a preferred embodiment, the preheating temperature is 100-400° C., the preheating time is 5-20 min, and the heating rate is 30-70° C. / min.

[0039] The inventors found that placing the weldment in an eddy current heating coil for preheating and heating using the above procedure can ensure uniform heating, and the resulting welded product has an optimal microstructure and better performance. In actual operation, a temperature measuring gun is used to measure the temperature of the welding groove in real time, and the temperature is kept stable after it stabilizes, which is the preheating time.

[0040] Further preferably, the preheating temperature is 150-280° C., the preheating time is 10-15 min, and the heating rate is 50-70° C. / min.

[0041] Preferably, when the welding method is to adopt Mag welding process throughout the whole process, the parameters of the Mag welding process are: welding voltage is controlled at 10~30V, welding current is controlled at 10~400A, and welding speed is controlled at 0~5m / min.

[0042] Further preferably, during the Mag welding process, the protective atmosphere used includes a mixed atmosphere of argon and oxygen, wherein the volume ratio of argon to oxygen in the mixed atmosphere is 80:20, and the flow rate of the protective atmosphere is 16-18 L / min.

[0043] In actual operation, Mag welding uses HGS-80 welding wire, and the diameter of HGS80 welding wire is 1.2mm.

[0044] Preferably, when the welding method adopts Tig welding process throughout the whole process, the parameters of the Tig welding process are as follows: the welding voltage is controlled at 10~30V, the welding current is controlled at 10~350A, and the welding speed is controlled at 0~5m / min.

[0045] Further preferably, during the Tig welding process, the protective atmosphere used is argon gas, and the flow rate of argon gas is 16-18 L / min.

[0046] In actual operation, Tig welding uses HGS-80 welding wire, the diameter of HGS80 welding wire is 1.2mm and the shielding gas is argon.

[0047] In a preferred solution, the welding method is to use Tig welding technology to perform base welding, and then use Mag welding technology to fill the cover surface.

[0048] The inventors have found that for the welding of dissimilar alloys, the above-mentioned welding square is preferred, and the final material performance is optimal. The Tig welding process is first used on the workpiece to be welded 1 # With the workpiece to be welded 2 # The base welding is performed at the groove of the workpiece to be welded, and then the Mag welding process is used to weld the workpiece 1 # With the workpiece to be welded 2 #The groove is covered and filled in the same direction, and finally the microstructure is regulated at the groove by a high-energy electric pulse quenching device. The dissimilar alloy weld obtained by this process has fine grains and uniform structure, which eliminates the welding thermal stress generated during the welding process and has the best comprehensive mechanical properties and mechanical properties.

[0049] The segmented process combining Tig welding and Mag welding is adopted. The air tightness of Tig welding is better during welding, which can effectively reduce the pores in the weld during welding. And because the heat source energy density is low, the oxidation degree is low during welding, and no oxides are generated, so the welding quality of the bottom weld can be ensured. At the same time, Mag welding is used to fill the cover surface in the subsequent welding process. Not only does it reduce the cost, but it can also avoid the problem that the welding wire cannot completely fill the V-shaped groove, the mechanical properties of the molten metal between passes are poor, and it is very easy to crack. The welding method of the present invention improves the welding quality of the weld to a certain extent, improves the toughness of the welded joint, and reduces the tendency to crack.

[0050] According to a preferred embodiment, during the base welding, the base weld thickness is controlled to be 2-7 mm, and the Tig welding process parameters are: the welding current is controlled to be 150-250 A, the welding voltage is 15-30 V, and the argon gas flow rate is 16-18 L / min.

[0051] In the present invention, when segmented welding is used, the process parameters of the base welding need to be controlled within the above range to obtain a base weld with a thickness of 2 to 7 mm. The performance of the final material is optimal at the above thickness. If the base weld is too thick, the welding strength will deteriorate.

[0052] In addition, the inventors found that excessive welding current not only leads to excessive thickness, but also causes a large amount of particle splashing during the welding process. These particles, as second-phase impurities, directly cause the brittleness of the molten pool area to increase, thereby affecting the performance. At the same time, due to the excessive current, the amount of heat input to the molten pool at the same time will increase, resulting in an increase in the grain size of the entire fusion zone and the heat-affected zone, which will also make the mechanical properties of the material worse.

[0053] Further preferably, during the base welding, the base weld thickness is controlled to be 2-5 mm, and the Tig welding process parameters are: the welding current is controlled to be 150-180 A, and the welding voltage is 15-23 V.

[0054] In actual operation, before Tig base welding, the tungsten pole of the welding gun is first aligned with the V-shaped groove, and pure argon gas is introduced into the area at the same time. After the air in the V-shaped groove is completely removed, the arc is started. HGS-80 welding wire is used in the welding process.

[0055] In a preferred embodiment, when filling the cover, the protective atmosphere used is a mixed atmosphere containing argon and oxygen, wherein the volume ratio of argon to oxygen in the mixed atmosphere is 95-98:2-5.

[0056] In a preferred embodiment, the parameters of the Mag welding process are as follows: the welding current is controlled at 150-300A, the welding voltage is 18-30V, and the gas flow rate is 16-18L / min.

[0057] In actual operation, after the base welding is completed, the surface welding slag and end protrusions are immediately polished and removed. After polishing, the protective gas is passed into the V-shaped groove with a Mag welding gun for about 10 seconds. After the air in the welding area is completely removed, the Mag welding filling and capping are started. HGS-80 welding wire is used during the welding process.

[0058] In a preferred embodiment, the Mag welding adopts a multi-layer and multi-pass welding process, the welds overlap each other, and the weld width at the overlapping part is ≥ 1 / 3 of the width of the previous weld, the welding direction of any one pass is consistent, and the inter-pass temperature is maintained at 140~280℃, preferably 160~220℃.

[0059] In the present invention, Mag welding adopts multi-layer and multi-pass welding until the complete covering is completed.

[0060] In actual operation, when using multi-layer and multi-pass welding technology, a temperature measuring gun is required to measure the temperature within 10mm around the welding groove after each filling.

[0061] In a preferred embodiment, the process parameters of the electric pulse treatment are: the pulse current frequency is controlled at 200-800 Hz, and the current density is controlled at 1×10 4 ~6×10 5 A / cm 2 , so that the local area of ​​the weldment is heated to 800-1000°C within 20-120 seconds, and the treatment time of the electric pulse is 1-10 minutes. In the present invention, the local area refers to the welding area and the surrounding area of ​​30-50 cm, and the heating time is controlled to be 20-120 seconds.

[0062] In the present invention, the performance of the material finally obtained by electric pulse treatment under the above-mentioned process parameters is optimal. This is because the current during electric pulse treatment has a great influence on the grain size of the processing area. If the current is too large, it is easy to cause coarse grains, while if the current is too small, the segregation between the grains cannot be eliminated.

[0063] Further preferably, the process parameters of the electric pulse treatment are: the pulse current frequency is controlled at 200-600 Hz, the local area heating temperature is controlled at 800-900° C., and the power-on time is about 1-5 min.

[0064] In actual operation, the power supply is immediately cut off after the electric pulse treatment for about 1 to 10 minutes, and quenching treatment is performed to obtain fine grains with high solid solubility.

[0065] In a preferred embodiment, the quenching process is to heat the welding area of ​​the welded part to 800-900°C, keep the temperature for 1-10 minutes, and then flush the welding area with a coolant to cool it down to room temperature.

[0066] Compared with the prior art, the present invention has the following beneficial effects:

[0067] 1) Compared with the traditional dissimilar metal welding process (single welding technology + post-weld heat treatment), the present invention provides a fully automatic electric pulse combined segmented welding device for intelligent docking of different metal pipes, which combines Mag welding gun, Mig welding gun and Tig welding gun into a comprehensive welding gun, and uses the Joule heat effect of high-energy electric pulse to improve the grain coarsening and segregation phenomena that occur in the welding process of Mag welding, Mig welding and Tig welding; at the same time, the PC control system is intelligently, digitally and automatically controlled to quickly and effectively control the selection of welding guns, the rotation angular velocity of the weld, the eddy current heating rate, the insulation time, the pulse current, the voltage, the frequency, the pulse width and other important parameters of the pipe in the welding process, and the welding process and the high-energy electric pulse process are monitored in real time, so as to solve the problems of undercutting and overburning caused by the instability of welding speed in Mag welding process, Mig welding process and Tig welding process, improve the microstructure morphology and mechanical properties of the weld area, reduce the cracking tendency caused by the particle coarsening, segregation and inclusion caused by the influence of welding heat, and improve the welding efficiency and reduce the welding cost under the premise of ensuring the welding yield.

[0068] 2) In addition, the present invention also provides a welding and electric pulse processing process suitable for dissimilar alloys. The process adopted by the Tig welding + Mag welding + high-energy electric pulse combined segmented welding method of the present invention is two welding technologies plus electric pulse processing. The segmented process of Tig welding + Mag welding is adopted, which can reduce the welding cost while ensuring the welding quality. The Tig welding + Mag welding + high-energy electric pulse combined segmented welding method of the present invention adopts a high-energy electric pulse treatment to regulate the microstructure at the welding joint, and improves the mechanical properties of the welding joint by refining the grains, eliminating segregation in the microstructure, crushing the network carbide, and eliminating welding thermal stress, thereby improving the plasticity, toughness, strength, etc. of the welding joint and reducing the cracking tendency of the material. Compared with the existing dissimilar metal welding process, this welding process does not require a long heat treatment and insulation time after welding, saving a lot of welding costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0069] Figure 1This is a front view and right view of the structural schematic diagram of a fully automatic electric pulse joint segmented welding device for intelligently connecting different metal pipes of the present invention. 1 is a PC control system; 2 is an electric control box; 3 is a spinning machine 1 # ; 4 is the pipe to be welded 1 # ; 5 is the electric pulse system; 6 is the welding system; 7 is the pipe to be welded 2 # ; 8 is a spinning machine 2 # ; 9 is the supporting transmission system; 10 is the quenching system; 11 is the heating system; 12 is the temperature measuring system; 13 is the base.

[0070] Figure 2 It is a right view of the structural schematic diagram of a fully automatic electric pulse combined segmented welding device for intelligently connecting different metal pipes of the present invention, in which 14 is a rotating clamping and fixing support seat.

[0071] Figure 3 It is a structural diagram of the welding system, wherein 61, 65, and 66 are three mixed gas delivery channels; 62, 64, and 67 are welding gun channels for three welding processes; 63 is a tungsten electrode rod for the Tig welding process; and 68 is a bearing rotating device.

[0072] Figure 4 It is a schematic diagram of the installation of a rotary clamping fixed support seat, a quenching system, a temperature measuring system, an electric pulse system, and a welding system, wherein 5 is an electric pulse system loaded with a graphite brush rod; 121 is an infrared temperature measuring gun in the temperature measuring system; 101 is a quenching spray gun in the quenching system; 141 is a connecting rod in the rotary clamping fixed support seat; 69 is a composite welding gun in the welding system; and 142 is a support seat in the rotary clamping fixed support seat.

[0073] Figure 5 This is the metallographic structure diagram of the 42CrMoA base material at 30 mm from the center in Example 3;

[0074] Figure 6 This is the metallographic structure diagram of the Q890 base material at 30 mm from the center in Example 3;

[0075] Figure 7 is the metallographic structure diagram of the base welding seam in Example 3;

[0076] Figure 8 This is the metallographic structure diagram of the base welding seam in Comparative Example 1;

[0077] Fig. 9 This is the metallographic structure diagram of the base weld in Comparative Example 2. DETAILED DESCRIPTION

[0078] The present invention is described in detail below with reference to the accompanying drawings.

[0079] like Figure 1 , Figure 2 As shown in the figure, the fully automatic electric pulse joint segmented welding device for intelligently connecting different metal pipes in this specific embodiment mainly consists of a PC control system 1, an electric control box 2, and a # Spinning machine 3, 1 # Pipe to be welded 4, electric pulse system 5, welding system 6, 2 # Pipe to be welded 7, 2 # The spinning machine tool 8, a supporting transmission system 9, a quenching system 10, a heating system 11, a temperature measuring system 12, a base 13, a rotating clamping and fixing support seat 14 and the like are composed of the following parts.

[0080] The electric control box includes a DC power supply, an AC power supply, a transformer, etc. (not shown in the figure), and the electric control box is used to supply power to the PC control system, the spinning machine, the electric pulse system, the welding system, the support transmission system, the quenching system, the heating system, the temperature measurement system, and the rotating clamping fixed support seat, so that the instructions issued by the PC control system are transmitted to the corresponding components to control the rotation angular velocity (1-1000 r / min) of the spinning machine; the electric pulse system is provided with corresponding pulse current frequency (10-8000 Hz), pulse width (10-30000 μs), current density (10 3 ~10 6 A / cm 2 ), power-on time, heating rate (10~100 ℃ / min), heating time and other signals; select the corresponding welding gun nozzle and mixed gas according to the instruction program, determine the welding stroke according to the power-on time, control the welding current (80~500A) and welding voltage (10~40V); select the corresponding quenching medium (cooling water, oil) and spray cooling time according to the instruction program; control the voltage and current of the eddy current coil in the heating system according to the instruction program, control the heating temperature, heating rate, and insulation time, and issue instructions to enable the temperature measurement system to perform real-time temperature monitoring of the weld (1~999℃).

[0081] The specific operation includes the following steps:

[0082] 1) Use a clamp to hoist two grooved pipes to be welded and place them in the groove at the top of the support transmission system. Use the handle to adjust the height of the support rod so that the center line of the pipe is aligned with the center line of the rotating core mold of the spinning machine. Move the guide pulley at the bottom of the support transmission system to fix the ungrooved end of the pipe on the chuck. After adjusting the distance between the butt pipes, it is usually controlled at 30~50mm, and use the spinning handle to fix the pipe through the clamping device.

[0083] 2) After fixing the two grooved pipes to be welded on the spinning machine, the heating system receives the command from the PC control system and moves to the vicinity of the corresponding welding area to start energizing the eddy current coil, and performs eddy current heating according to the heating speed, insulation temperature, and insulation time set by the PC control system. When the insulation setting time is reached, the power supply ends, the heating stops, and the guide pulley at the bottom retreats to the original position. The pipes to be welded do not need to be moved during the preheating process, and the eddy current coil provides heat radiation to achieve this.

[0084] 3) After the preheating treatment of the pipe to be welded is completed, the PC control system immediately issues a command to control the welding system to start working. According to the selected welding process parameters, the corresponding welding gun is automatically rotated and selected, and the corresponding mixed gas flows out from the guide device, and the corresponding protective gas is sprayed at the weld to protect the welding process. The process adopts a multi-layer and multi-pass welding process, and each pass is monitored in real time by the infrared thermometer in the temperature measurement system for the weld and the surrounding 30mm. The temperature of each weld and the surrounding area must be controlled within the set temperature range before welding can be carried out, and the welding will stop after the weld is completely covered. The control of the welding speed in the welding process is mainly provided by the rotation angular velocity of the spindle in the spinning machine, and is transmitted by the support pulley on the top of the supporting transmission device; and the temperature of the weld and the surrounding 30mm is monitored in real time by the infrared thermometer during the entire welding process.

[0085] 4) After the segmented welding of the pipe to be welded is completed, the PC control system immediately sends instructions to the electric pulse system to control the rotating clamping control support to perform three-dimensional rotational movement, and uses the rotating bearing in the center to make the graphite brush rod contact the pipe to be welded. After the trigger point is controlled at 50mm around the pipe to be welded, the high-frequency pulse power supply will be automatically turned on. The electric pulse organization of the pipe energization area will be adjusted according to the pulse current frequency, current density, pulse width, power-on time, heating rate and other signals set by the PC control system.

[0086] 5) After the pipe to be welded is treated with high-frequency electric pulses, the PC control system issues instructions to control the rotating clamping control support to perform three-dimensional rotational motion, so that the graphite electrode rod returns to its initial position. Then, instructions are issued to the quenching system, and the nozzle rotating device of the quenching system is controlled to quench according to the required quenching medium and cooling speed.

[0087] like Figure 3 The figure shows the structure of the welding system in the fully automatic electric pulse joint segmented welding device for intelligently connecting different metal pipes in this specific embodiment, which is mainly composed of a mixed gas delivery channel, a welding gun pass, a tungsten electrode rod and a bearing rotating device. 61, 65, and 66 are three types of mixed gas delivery channels; 62, 64, and 67 are three types of welding gun passes; 63 is a tungsten electrode rod for the Tig welding process; 68 is a bearing rotating device

[0088] Install components 61, 62, 63, 64, 65, 66 and 67 as shown in the figure, and use "one electrode, three muzzles and three nozzles" to install them in a ring shape in component 68. The electrode and the top of the muzzle are connected to the electric control box, the core of the muzzle is the welding wire (not marked in the figure), the top of the nozzle is connected to the mixed gas pipeline and is equipped with an electric control valve, and the muzzle and the mixed gas are selected according to the signal transmitted by the PC control system.

[0089] like Figure 4 As shown, it is a schematic diagram of the installation of the rotary clamping system, quenching system, temperature measurement system, electric pulse system and welding system in the fully automatic electric pulse combined segmented welding device for intelligent docking of different metal pipes according to this specific embodiment, wherein 5 is the electric pulse system loaded with graphite brush rod; 121 is the infrared temperature measuring gun in the temperature measurement system; 101 is the quenching spray gun in the quenching system; 141 is the connecting rod in the rotary clamping system; 69 is the composite welding gun in the welding system; 142 is the support seat in the rotary clamping system.

[0090] The present invention also provides a process for welding and electric pulse treatment of dissimilar alloys using the above device: the following is further described in detail in conjunction with specific embodiments. Example

[0091] A Mag welding + high energy electric pulse combined segmented welding method for dissimilar alloys such as Q890 and 42CrMoA, comprising the following steps:

[0092] a. Prepare materials: Make a 20° groove on Q890 and 42CrMoA materials. The corresponding alloy chemical element composition and mass fraction are: Q890: C: 0.15%; Si: 0.28%; Mn: 1.33%; P: 0.011%; S: 0.01%; Al: 0.041%; Cu: 0.02%; Cr: 0.45%; Ni: 0.325%; Mo: 0.326%; V: 0.035%; Ti: 0.02%. 42CrMoA: C: 0.41%; Si: 0.24%; Mn: 0.62%; P: 0.015%; S: 0.006%; Cr: 1.02%; Ni: 0.1%; Mo: 0.21%. The thickness of the alloy materials is 30mm. Grind and remove iron filings, oil stains, oxides and other impurities on the groove surface and the surrounding 30mm.

[0093] b. Positioning: Butt the Q890 and 42CrMoA with grooves cut in V-shaped grooves, and control the space gap of the butt joint within 5mm.

[0094] c. Preheating treatment: Place the butt-jointed materials in the eddy current heating coil, set the heating rate to 60℃ / min after power on, preheat the butt-jointed materials to 220℃, and keep warm for 5 minutes.

[0095] d. Base welding: Q890 and 42CrMoA alloys with 10~25° single-sided grooves are butt-jointed in a V-shaped manner, and the Mag welding process is used to base the V-groove. The thickness of the base weld is 6mm. Before base welding, align the tungsten pole of the welding gun with the V-groove, and at the same time, introduce shielding gas to the area for about 10 seconds. After removing all the air in the V-groove, start to strike the arc. After base welding is completed, immediately grind and remove the surface welding slag and end protrusions. After grinding clean, use a Mag welding gun to introduce shielding gas towards the V-groove for about 10 seconds. After removing all the air in the welding area, start Mag welding to fill the cover. HGS-80 welding wire is used during the welding process, and the shielding gas is 80%Ar+20%O by volume. 2 The mixed gas is required. At the same time, the Mag welding direction is required to be consistent with the previous welding direction. The process adopts a multi-layer and multi-pass welding process. After each pass of filling, a temperature measuring gun is required to measure the temperature within 10mm around the welding groove. The temperature between passes is required to be maintained at 250℃. HGS-80 welding wire is used in the welding process. The parameters in the welding process are: HGS80 welding wire diameter is 1.2mm, welding current is controlled at 150~250A, welding voltage is adjusted to 25V, and gas flow is 16L / min.

[0096] e. Electric pulse grain refinement treatment: After the Mag welding cap is completed, the two ends of the weldment are clamped at the two ends of the electric pulse electrode, and the power is turned on to pass a high-density pulse current through the weldment. The pulse current frequency is controlled at 600 Hz and the current density is controlled at 1×10 4 ~6×10 5 A / cm 2 , so that the local area of ​​the weldment is quickly heated to 900°C. After about 10 minutes of electric pulse treatment, the power supply is immediately cut off, and the outer 30mm of both ends of the welding area is quenched to obtain fine grains with high solid solubility.

[0097] After testing, the performance of the center and surrounding of the welding area was obtained:

[0098] (1) Impact performance (impact temperature is 233.15K):

[0099] 1) Impact energy at weld: 32.4J

[0100] 2) Impact energy at the fusion line on the Q890 side: 34.9J

[0101] 3) Impact energy at the fusion line of 42CrMoA side: 40.7J

[0102] (2) Tensile strength: 916.3MPa

[0103] (3) Elongation: 17.2%

[0104] (4) Hardness: 296HV Example

[0105] A Tig welding + high-energy electric pulse combined segmented welding method for dissimilar alloys such as Q890 and 42CrMoA, comprising the following steps:

[0106] a. Prepare materials: Make a groove of 10~20° on Q890 and 42CrMoA materials. The corresponding alloy chemical element composition and mass fraction are as follows: Q890: C: 0.15%; Si: 0.28%; Mn: 1.33%; P: 0.011%; S: 0.01%; Al: 0.041%; Cu: 0.02%; Cr: 0.45%; Ni: 0.325%; Mo: 0.326%; V: 0.035%; Ti: 0.02%. 42CrMoA: C: 0.41%; Si: 0.24%; Mn: 0.62%; P: 0.015%; S: 0.006%; Cr: 1.02%; Ni: 0.1%; Mo: 0.21%. The thickness of the alloy materials is 30mm. Grind and remove iron filings, oil stains, oxides and other impurities on the surface of the groove and the surrounding 20~30mm.

[0107] b. Positioning: Butt the Q890 and 42CrMoA with grooves cut in V-shaped grooves, and control the space gap of the butt joint within 3mm.

[0108] c. Preheating treatment: Place the butt-jointed materials in the eddy current heating coil, set the heating rate to 60℃ / min after power on, preheat the butt-jointed materials to 250℃, and keep warm for 5 minutes.

[0109] d. Base welding: The Q890 and 42CrMoA alloys with 20° single-sided grooves are butt-jointed in a V-shaped manner, and the base welding is performed in the V-shaped groove using the Tig welding process. The thickness of the base welding bead is 5mm. Before Tig base welding, the tungsten pole of the welding gun is first aligned with the V-shaped groove, and pure argon shielding gas is introduced into the area for about 10 seconds. After the air in the V-shaped groove is completely removed, the arc is started. After the base welding is completed, the surface welding slag and end protrusions are immediately polished and removed. After polishing, the protective gas is introduced into the V-shaped groove with a Tig welding gun for about 10 seconds. After the air in the welding area is completely removed, the Tig welding is started to fill the cover. HGS-80 welding wire is used during the welding process, and the Tig welding direction is required to be consistent with the previous welding direction. The process adopts a multi-layer and multi-pass welding process. After each pass of filling, a temperature measuring gun is required to measure the temperature within 10mm around the welding groove. The temperature between passes is required to be maintained at 220℃. HGS-80 welding wire is used during the welding process. The parameters during welding are: HGS80 welding wire diameter is 1.2 mm, welding current is controlled at 150~230 A, welding voltage is adjusted to 23 V, and gas flow rate is 16 L / min.

[0110] e. Electric pulse grain refinement treatment: After the Tig welding cap is completed, the two ends of the weldment are clamped at the two ends of the electric pulse electrode, and the power is turned on to pass the high-density pulse current through the weldment. The pulse current frequency is controlled at 500 Hz and the current density is controlled at 1×10 4 ~6×10 5 A / cm 2 , so that the local area of ​​the weldment is quickly heated to 900°C. After about 7 minutes of electric pulse treatment, the power supply is immediately cut off, and the outer 30mm of both ends of the welding area is quenched to obtain fine grains with high solid solubility.

[0111] After testing, the performance of the center and surrounding of the welding area was obtained:

[0112] (1) Impact performance (impact temperature is 233.15K):

[0113] 1) Impact energy at weld: 40.3J

[0114] 2) Impact energy at the fusion line on the Q890 side: 52.4J

[0115] 3) Impact energy at the fusion line of 42CrMoA side: 56.7J

[0116] (2) Tensile strength: 988.9MPa

[0117] (3) Elongation: Tig weld: 20.7%

[0118] (4) Hardness: 317HV Example

[0119] A Tig welding + Mag welding + high-energy electric pulse combined segmented welding method for dissimilar alloys such as Q890 and 42CrMoA, comprising the following steps:

[0120] a. Prepare materials: Make a 20° groove on Q890 and 42CrMoA materials. The corresponding alloy chemical element composition and mass fraction are: Q890: C: 0.15%; Si: 0.28%; Mn: 1.33%; P: 0.011%; S: 0.01%; Al: 0.041%; Cu: 0.02%; Cr: 0.45%; Ni: 0.325%; Mo: 0.326%; V: 0.035%; Ti: 0.02%. 42CrMoA: C: 0.41%; Si: 0.24%; Mn: 0.62%; P: 0.015%; S: 0.006%; Cr: 1.02%; Ni: 0.1%; Mo: 0.21%. The thickness of the alloy materials is 30mm. Grind and remove iron filings, oil stains, oxides and other impurities on the groove surface and the surrounding 30mm.

[0121] b. Positioning: Butt the Q890 and 42CrMoA with grooves cut in V-shaped grooves, and control the space gap of the butt joint within 3mm.

[0122] c. Preheating treatment: Place the butted materials in the eddy current heating coil, set the heating rate to 60℃ / min after power on, preheat the butted materials to 220℃, and keep warm for 10 minutes.

[0123] d. Base welding: The Q890 and 42CrMoA alloys with 20° single-sided grooves are butt-jointed in a V-shaped manner, and the base is made in the V-shaped groove using the Tig welding process. The thickness of the base weld is 3 mm. Before Tig base welding, the tungsten pole of the welding gun is first aligned with the V-shaped groove, and pure argon shielding gas is introduced into the area for about 10 seconds. After the air in the V-shaped groove is completely removed, the arc is started. The HGS-80 welding wire is used in the welding process. The parameters in the welding process are: the diameter of the HGS80 welding wire is 1.2 mm, the welding current is controlled at 150~180A, the welding voltage is adjusted to 18V, and the gas flow rate is 16 L / min.

[0124] e. Filling and capping: After the base welding is completed, grind and remove the surface welding slag and end protrusions immediately. After grinding, use the Mag welding gun to pass the protective gas towards the V-shaped groove for about 10 seconds, and start the Mag welding filling and capping after removing all the air in the welding area. HGS-80 welding wire is used during the welding process, and the protective gas is 98% argon + 2% oxygen. At the same time, the Mag welding direction is required to be consistent with the previous welding direction. The parameters during the welding process are: the diameter of the HGS80 welding wire is 1.2mm, the welding current is controlled at 150~180A, and the welding voltage is adjusted to 18V. The process adopts a multi-layer and multi-pass welding process. After each filling, a temperature measuring gun is required to measure the temperature within 10mm around the welding groove. The interpass temperature is required to be maintained at 200℃ and the gas flow rate is 16L / min.

[0125] f. Electric pulse grain refinement treatment: After the Mag welding cap is completed, the two ends of the weldment are clamped at the two ends of the electric pulse electrode, and the power is turned on to pass the high-density pulse current through the weldment. The pulse current frequency is controlled at 450Hz and the current density is controlled at 1×10 4 ~6×10 5 A / cm 2 , so that the local area of ​​the weldment is quickly heated to 850°C. After about 3 minutes of electric pulse treatment, the power supply is immediately cut off, and the outer 30mm of both ends of the welding area is quenched to obtain fine grains with high solid solubility.

[0126] Figures 5 to 7 This is the tissue photo corresponding to Example 3.

[0127] in Figure 5 This is the metallographic structure diagram of the 42CrMoA base material at 30 mm from the center in Example 3, and its microstructure is composed of uniform troostite and a small amount of ferrite. Figure 6 This is the metallographic structure diagram of the Q890 base material at 30 mm from the center in Example 3, and its microstructure is composed of martensite and granular carbide. Figure 7 3 is the metallographic structure diagram of the base welding seam in Example 3, and its microstructure consists of low-carbon lath martensite and lath bainite.

[0128] After testing, the performance of the center and surrounding of the welding area was obtained:

[0129] (1) Impact performance (impact temperature is 233.15K):

[0130] 1) Impact energy at weld: 49.7J

[0131] 2) Impact energy at the fusion line on the Q890 side: 55.6J

[0132] 3) Impact energy at the fusion line on the 42CrMoA side: 58.8J

[0133] (2) Tensile strength:

[0134] 1) Tig weld: 996.1MPa

[0135] 2) Mag weld: 948.1MPa

[0136] (3) Elongation:

[0137] 1) Tig weld: 21.4%

[0138] 2) Mag weld: 20.2%

[0139] (4) Hardness: 327HV

[0140] Comparative Example 1

[0141] The commonly used welding method for dissimilar metals is a single Tig welding + tempering heat treatment welding method, which includes the following steps:

[0142] a. Prepare materials: Make a 20° groove on Q890 and 42CrMoA materials. The corresponding alloy chemical element composition and mass fraction are: Q890: C: 0.15%; Si: 0.28%; Mn: 1.33%; P: 0.011%; S: 0.01%; Al: 0.041%; Cu: 0.02%; Cr: 0.45%; Ni: 0.325%; Mo: 0.326%; V: 0.035%; Ti: 0.02%. 42CrMoA: C: 0.41%; Si: 0.24%; Mn: 0.62%; P: 0.015%; S: 0.006%; Cr: 1.02%; Ni: 0.1%; Mo: 0.21%. The thickness of the alloy materials is 40mm. Grind and clean the surface of the groove and the surrounding 30mm iron filings, oil stains, oxides and other impurities.

[0143] b. Positioning: Butt the Q890 and 42CrMoA with grooves cut in V-shaped grooves, and control the space gap of the butt joint within 5mm.

[0144] c. Preheating treatment: Use an acetylene oxygen open flame heater to heat the docked materials to 250°C and measure the temperature with a temperature gun.

[0145] d. Welding: The Q890 and 42CrMoA alloys with 20° single-sided grooves are butt-jointed in a V-shaped manner, and the Tig welding process is used to perform the base welding in the V-shaped groove. The welding is performed after the shielding gas is introduced, and the thickness of the base weld is 6mm. After the base welding is completed, the filling and capping are carried out in the same direction. HGS-80 welding wire is used in the welding process, and the shielding gas is argon. The parameters in the welding process are: the diameter of the HGS80 welding wire is 1.2mm, the welding current is controlled at 150~250A, the welding voltage is adjusted to 23V, and the gas flow rate is 18L / min.

[0146] e. Post-weld heat treatment: After filling, air cool immediately. After the weld joint is completely cooled, place the material in a holding furnace for tempering heat treatment. During the heat treatment process, the furnace is heated to 350℃ at a rate of 5℃ / min and kept for 2h before cooling to room temperature with the furnace.

[0147] Figure 8 This is the metallographic structure diagram of the base welding seam in comparative example 1, and its microstructure is composed of low-carbon lath martensite and lath bainite. Figure 7 and Figure 8 It can be found that Figure 8 The low-carbon lath martensite and lath bainite in the steel are both coarse. This is because, during the electric pulse treatment, the welding area is locally heated to the solid solution temperature, causing the segregation and second phase to re-austenize during the welding process. The welding area is quickly cooled by quenching at the end, forming fine grains with high solid solubility.

[0148] After testing, the performance of the center and surrounding of the welding area was obtained:

[0149] (1) Impact performance (impact temperature is 233.15K):

[0150] 1) Impact energy at weld: 27.7J

[0151] 2) Impact energy at the fusion line on the Q890 side: 30.3J

[0152] 3) Impact energy at the fusion line of 42CrMoA side: 34.7J

[0153] (2) Tensile strength: 894.1MPa

[0154] (3) Elongation: 16.2%

[0155] (4) Hardness: 269 HV.

[0156] Comparative Example 2

[0157] The commonly used welding method for dissimilar metals is a single Mag welding + tempering heat treatment welding method, which includes the following steps:

[0158] a. Prepare materials: Make a 20° groove on Q890 and 42CrMoA materials. The corresponding alloy chemical element composition and mass fraction are: Q890: C: 0.15%; Si: 0.28%; Mn: 1.33%; P: 0.011%; S: 0.01%; Al: 0.041%; Cu: 0.02%; Cr: 0.45%; Ni: 0.325%; Mo: 0.326%; V: 0.035%; Ti: 0.02%. 42CrMoA: C: 0.41%; Si: 0.24%; Mn: 0.62%; P: 0.015%; S: 0.006%; Cr: 1.02%; Ni: 0.1%; Mo: 0.21%. The thickness of the alloy materials is 30mm. Grind and remove iron filings, oil stains, oxides and other impurities on the groove surface and the surrounding 30mm.

[0159] b. Positioning: Butt the Q890 and 42CrMoA with grooves cut in V-shaped grooves, and control the space gap of the butt joint within 5mm.

[0160] c. Preheating treatment: Use an acetylene oxygen open flame heater to heat the docked materials to 250°C and measure the temperature with a temperature gun.

[0161] d. Welding: The Q890 and 42CrMoA alloys with 20° single-sided grooves are butt-jointed in a V-shaped manner, and the Mag welding process is used to perform the base welding in the V-shaped groove. The welding is performed after the shielding gas is introduced, and the thickness of the base weld is 5mm. After the base welding is completed, the filling and capping are carried out in the same direction. HGS-80 welding wire is used in the welding process, and the shielding gas is 80% argon + 20% oxygen. The parameters in the welding process are: the diameter of the HGS80 welding wire is 1.2mm, the welding current is controlled at 150~250A, the welding voltage is adjusted to 23V, and the gas flow rate is 18L / min.

[0162] e. Post-weld heat treatment: After filling, air cool immediately. After the weld joint is completely cooled, place the material in a holding furnace for tempering heat treatment. During the heat treatment process, the furnace is heated to 300°C at a rate of 5°C / min and kept at that temperature for 2 hours before cooling to room temperature with the furnace.

[0163] Fig. 9 It is the metallographic structure diagram of the base welding seam in comparative example 2, and its microstructure consists of low-carbon lath martensite and lath bainite.

[0164] After testing, the performance of the center and surrounding of the welding area was obtained:

[0165] (1) Impact performance (impact temperature is 233.15K):

[0166] 1) Impact energy at weld: 25.4J

[0167] 2) Impact energy at the fusion line on the Q890 side: 28.2J

[0168] 3) Impact energy at the fusion line of 42CrMoA side: 32.5J

[0169] (2) Tensile strength: 883.2MPa

[0170] (3) Elongation: 15.8%

[0171] (4) Hardness: 264 HV.

Claims

1. A process for fully automatic electric pulse combined segmented welding of intelligently connected different metal pipes, characterized in that: The steps include: placing a workpiece to be welded 1 # 、Workpiece to be welded 2 # The grooves are pre-cut, and then fixed on the spinning machine and positioned to form the area to be welded. The area to be welded is pre-treated by eddy current heating, and then welded to obtain the welding area. Finally, the welding area is treated by electric pulse and quenching to obtain the welded product. The workpiece to be welded 1 # With the workpiece to be welded 2 # The materials are different. The welding method is to use Tig welding process for base welding, and then use Mag welding process to fill the cover surface; During the base welding, the base weld thickness is controlled to be 2-7 mm, and the Tig welding process parameters are: the welding current is controlled at 150-250 A, the welding voltage is 15-30 V, and the argon gas flow rate is 16-18 L / min; The parameters of the Mag welding process are as follows: the welding current is controlled at 150~300A, the welding voltage is 18~30V, and the gas flow rate is 16~18L / min; The process parameters of the electric pulse treatment are: the pulse current frequency is controlled at 200-800 Hz, the current density is controlled at 1×10 4 ~6×10 5 A / cm 2 , so that the local area of ​​the weldment is heated to 800~1000℃ within 20~120s, and the treatment time of the electric pulse is 1~10min; The quenching process is to heat the welding area of ​​the welded part to 800-900°C, keep the temperature for 1-10 minutes, and then flush the welding area with a coolant to cool it down to room temperature; The devices used in the process include two spinning machines, a heating system, a welding system, an electric pulse system, and a quenching system; the spinning machine is used to fix the workpiece to be welded; the heating system includes an eddy current coil, which is used to perform eddy current heating pretreatment on the workpiece to be welded; the welding system includes a Tig welding gun, a Mag welding gun, a Mig welding gun, and a bearing rotating device, wherein the Tig welding gun, the Mag welding gun, and the Mig welding gun are installed on the bearing rotating device, and the bearing rotating device is used to automatically rotate and select the welding gun to weld the workpiece to be welded; the electric pulse system includes a high-frequency pulse power supply and a graphite brush rod, and the graphite brush rod is connected to the high-frequency pulse power supply to provide electric pulse current to the welded part; the quenching system is used to quench the welded part after the electric pulse treatment.

2. According to claim 1, a process for fully automatic electric pulse combined segmented welding of intelligently connected different metal pipes is characterized by: The workpiece to be welded 1 # With the workpiece to be welded 2 # The materials of the workpiece to be welded are all selected from Q890 or 42CrMoA. # With the workpiece to be welded 2 # The thickness is ≤40mm; The workpiece to be welded 1 # With the workpiece to be welded 2 # The grooves are pre-opened at 10~25°; The swing positioning is to open the groove of the workpiece to be welded 1 # With the workpiece to be welded 2 # The butt joint is made by V-shaped groove, and the space gap of the butt joint is controlled within 5mm; The temperature of the eddy current heating pretreatment is 100-400° C., the time of the eddy current heating pretreatment is 5-20 min, and the heating rate is 30-70° C. / min.

3. The process of fully automatic electric pulse combined segmented welding for intelligent butt joint of different metal pipes according to claim 1 is characterized by: When filling the cover, the protective atmosphere used is a mixed atmosphere containing argon and oxygen, wherein the volume ratio of argon to oxygen in the mixed atmosphere is 95-98:2-5; The Mag welding adopts a multi-layer and multi-pass welding process, the welds overlap each other, and the weld width at the overlapping part is ≥ 1 / 3 of the width of the previous weld, the welding direction of any one pass is consistent, and the inter-pass temperature is maintained at 140~280℃.

4. The process of fully automatic electric pulse combined segmented welding for intelligent butt joint of different metal pipes according to claim 1 is characterized by: The device further comprises a PC control system, wherein the PC control system is used to issue instructions to control other systems; The device also includes an electric control box, which includes a DC power supply, an AC power supply, and a transformer, and is used to supply power to the device.

5. The process of fully automatic electric pulse combined segmented welding for intelligent butt joint of different metal pipes according to claim 1 is characterized by: The 2 spinning machines are divided into the left spinning machine 1 # And the spinning machine 2 on the right # , the spinning machine 1 # Used to fix the workpiece to be welded 1 # , Spinning Machine 2 # Used to fix the workpiece to be welded 2 # Any spinning machine includes a spindle, a chuck, a spinning core mold, a clamping device, and a spinning handle; the chuck is installed on the spindle, clamping the rotating core mold and combining the clamping device and the spinning handle to clamp and fix the workpiece to be welded.

6. The process of fully automatic electric pulse combined segmented welding for intelligent butt joint of different metal pipes according to claim 1 is characterized by: The device also includes a support transmission system and a base; the support transmission system includes a support pulley at the top, a guide pulley at the bottom and a support rod, the top support pulley and the bottom guide pulley are fixed to the top and bottom ends of the support rod and placed in the guide groove of the base, the top support pulley cooperates with the spinning machine to rotate the workpiece 360 ​​degrees, and the bottom guide pulley is used to control the workpiece to be welded to be fixed on the spinning machine; The device further comprises a temperature measuring system, wherein the temperature measuring system comprises an external line temperature measuring instrument, wherein the external line temperature measuring instrument is a bidirectional gun head, facing respectively the graphite brush rod of the electric pulse system and the composite welding gun head in the welding system; The device also includes a rotating clamping and fixing support seat, which is used to clamp and fix the graphite brush rod of the electric pulse system, the composite welding gun of the welding system, the infrared temperature measuring gun of the temperature measuring system, and the quenching nozzle rotating device of the quenching system, wherein the electric pulse system and the welding system are distributed in opposite directions at 180°, the infrared temperature measuring gun of the temperature measuring system is fixed at the center position of the rotating clamping and fixing support seat; the quenching system is fixed in the middle of the rotating clamping and fixing support seat.

7. The process of fully automatic electric pulse combined segmented welding for intelligent butt joint of different metal pipes according to claim 1 is characterized by: The welding system also includes a mixed gas flow guide device, a tungsten electrode; The quenching system includes a liquid guide tube, a distribution nozzle, a control valve, and a nozzle rotating device. The liquid guide tube, the distribution nozzle and the control valve are fixed in the nozzle rotating device. The rotating device is fixed in the middle of a rotating clamping fixed support seat. The distribution nozzle is a single-phase nozzle, facing the graphite brush rod of the electric pulse system.