Polyimide nanoparticles, preparation method thereof and application thereof
Polyimide nanoparticles prepared through hydrothermal synthesis are blended with polyimide or its precursor polyamic acid, which solves the problem of insufficient compatibility of polyimide materials and improves the mechanical and heat resistance of the materials , achieving comprehensive performance optimization.
Patent Information
- Application Number
- CN202011144166.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-10-23
AI Technical Summary
Polyimide materials are insufficient in the blending process of nanoparticles and substrates, resulting in poor dispersion and limited improvement in material performance.
Polyimide nanoparticles are prepared by selecting a combination of dianhydride and polyamine and a diamine with polar groups, and blending them with polyimide or its precursor polyamic acid solution, and by forming Processing improves material performance.
The mechanical properties and heat resistance of polyimide materials have been significantly improved, the problem of insufficient compatibility has been solved, and materials with excellent comprehensive performance have been obtained.
Smart Images

Figure CN114479071B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of polyimide materials, in particular to a polyimide nanoparticle and a preparation method and application thereof, which are used to achieve blending modification of polyimide materials with good compatibility to improve various properties of the materials. Background Art
[0002] Nanoparticle blending is a common technology for improving material performance in modern times, which can significantly improve mechanical properties (reinforcement, toughening), thermal properties (glass transition temperature, thermal decomposition temperature), electrical properties (conductivity, dielectric properties), etc. However, in the process of blending nanoparticles with substrates, there is often a problem of insufficient compatibility, which leads to poor dispersion of nanoparticles in the matrix, and even material defects due to nanoparticle agglomeration. Therefore, improving the compatibility of nanoparticles and the matrix is the key to improving this deficiency.
[0003] Polyimide is a special high-performance polymer. Since its synthesis process can be prepared by a two-step method and the intermediate polyamic acid has good solubility, polyimide can be subjected to different types of molding processes such as film forming, spinning and resin matrix. However, in the application process, the required performance optimization cannot be fully achieved through the selection and adjustment of copolymerization units. Therefore, in order to improve certain properties of the material, blended nanomaterials are selected to achieve this purpose. Based on the similar and compatible characteristics of polymer materials, the present invention proposes a polyimide nanoparticle and a controllable preparation method and application thereof. The obtained polyimide nanoparticle is blended with other polyimides or polyimide precursor polyamic acid solution and then molded, which can improve the mechanical properties and heat resistance of the material. The development and application of this type of material provides a new idea and method for realizing the blending modification of polyimide materials. Summary of the invention
[0004] The present invention relates to a polyimide nanoparticle and a preparation method and application thereof, which mainly solves the problem of insufficient compatibility when polyimide materials and nanoparticles are blended, so that the material has the advantages of both bulk material and nanoparticle material performance.
[0005] The technical idea of the preparation method of polyimide nanoparticles of the present invention is mainly to select a combination of dianhydride, polyamine and diamine with polar groups to form salt, and then hydrothermally synthesize to prepare polyimide nanoparticles, wherein the combination of dianhydride and polyamine is mainly a rigid symmetrical structure, and the skeleton structure of nanoparticles is obtained. The diamine with polar groups participates in the skeleton formation and also adjusts the size of nanoparticles through the hydrophilic and hydrophobic effects in the aqueous solution, so that the size of nanoparticles can be controlled. The obtained nanoparticles are blended and modified with polyimide or its precursor polyamic acid solution, and a material with excellent comprehensive performance can be obtained after molding and processing.
[0006] One of the purposes of the present invention is to provide a polyimide nanoparticle comprising a structural unit derived from at least one of a triamine or a tetraamine, a structural unit derived from a diamine with a polar hydrophilic group, and a structural unit derived from a dianhydride.
[0007] The dianhydride is selected from dianhydrides with a rigid structure, preferably at least one of pyromellitic dianhydride, 3,3,4,4-biphenyltetracarboxylic dianhydride, 2,3,3,4-biphenyltetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, cyclobutanetetracarboxylic dianhydride, and bicyclo[2.2.1]heptane-2,3,5,6-tetracarboxylic dianhydride.
[0008] The triamine or tetraamine is selected from at least one of tris(4-aminophenyl)amine, 1,3,5-tris(aminophenyl)benzene, 1,3,5-tris(4-aminophenoxy)benzene, 4,4',4"-(1,3,5-triazine-2,4,6-triyl)triphenylamine, 4,4',4"-(1,3,5-triazine-2,4,6-triyl)tris(1,10-biphenyl)amine, 1,3,5,7-tetraaminoadamantane, and tetrakis(4-aminophenyl)methane.
[0009] The diamine with polar hydrophilic group is selected from at least one of 3,5-diaminobenzoic acid, 3,4-diaminobenzoic acid, 2,4-diaminobenzenesulfonic acid, 2,5-diaminobenzenesulfonic acid and 3,4-diaminobenzenesulfonic acid.
[0010] The molar ratio of the amino functional groups of the triamine or / and tetraamine to the total amino functional groups is 60-90%, preferably 75-85%; the molar ratio of the amino functional groups of the diamine with polar hydrophilic groups to the total amino functional groups is 10-40%, preferably 15-25%.
[0011] The particle size of the polyimide nanoparticles of the present invention is 0.1-5 μm.
[0012] The second object of the present invention is to provide a method for preparing polyimide nanoparticles, comprising reacting dianhydride with amine to form salt, then dispersing the obtained salt in water, and hydrothermally synthesizing the polyimide nanoparticles, wherein the amine is a mixture of at least one of a triamine or a tetraamine and a diamine with a polar hydrophilic group.
[0013] In the preparation method of the present invention, the dianhydride is selected from monomers with a rigid structure, preferably one or more of pyromellitic dianhydride (PMDA), 3,3,4,4-biphenyltetracarboxylic dianhydride (BPDA), 2,3,3,4-biphenyltetracarboxylic dianhydride (α-BPDA), 2,3,6,7-naphthalenetetracarboxylic dianhydride, cyclobutanetetracarboxylic dianhydride (CBDA), bicyclo[2.2.1]heptane-2,3,5,6-tetracarboxylic dianhydride (BHDA), etc. Among them, the more preferred dianhydride monomer is an aromatic symmetrical structure dianhydride, one or more of pyromellitic dianhydride, 3,3,4,4-biphenyltetracarboxylic dianhydride, and 2,3,6,7-naphthalenetetracarboxylic dianhydride.
[0014] In the preparation method of the present invention, the triamine or tetraamine is one or more of tris(4-aminophenyl)amine (TAPA), 1,3,5-tris(aminophenyl)benzene (TAPB), 1,3,5-tris(4-aminophenoxy)benzene (TAPOB), 4,4',4"-(1,3,5-triazine-2,4,6-triyl)triphenylamine (Tta), 4,4',4"-(1,3,5-triazine-2,4,6-triyl)tris(1,10-biphenyl)amine, 1,3,5,7-tetraaminoadamantane, tetrakis(4-aminophenyl)methane, etc. Among them, more preferred are rigid triamines or tetraamines with a relatively large spatial symmetric structure, such as one or more of tris(4-aminophenyl)amine, 1,3,5-tris(aminophenyl)benzene, and 1,3,5,7-tetraaminoadamantane.
[0015] In the preparation method of the present invention, the diamine with a polar hydrophilic group is one or more of 3,5-diaminobenzoic acid, 3,4-diaminobenzoic acid, 2,4-diaminobenzenesulfonic acid, 2,5-diaminobenzenesulfonic acid, and 3,4-diaminobenzenesulfonic acid, wherein preferably the diamine in the molecule is located at the meta or para position, such as at least one or more of 3,5-diaminobenzoic acid, 2,5-diaminobenzenesulfonic acid, and 2,4-diaminobenzenesulfonic acid.
[0016] In the preparation method of the present invention, the molar ratio of the amino functional group of the amine to the anhydride functional group of the dianhydride is (0.95-1.05):1.
[0017] In the amines, the molar ratio of the amino functional groups of triamines and / or tetraamines to the total amino functional groups is 60-90%, preferably 75-85%; the molar ratio of the amino functional groups of diamines with polar hydrophilic groups to the total amino functional groups is 10-40%, preferably 15-25%.
[0018] Preferably, the preparation method comprises the following steps:
[0019] (1) dissolving a dianhydride in water, hydrolyzing the dianhydride to obtain a tetraacid solution, and optionally adding an alcohol to the tetraacid solution;
[0020] (2) dissolving an amine in water or a mixed solvent of water and alcohol, and adding the mixture to a tetraacid solution to react and obtain a salt;
[0021] (3) dispersing the obtained salt in water and performing hydrothermal synthesis to obtain the polyimide nanoparticles.
[0022] In the preparation method of the present invention, in step (1), the solid content of the dianhydride is less than 5wt%, preferably 0.5-3wt%;
[0023] The hydrolysis temperature is 60 to 90° C., preferably 70 to 80° C.; the hydrolysis time is 1 to 4 hours, preferably 2 to 3 hours.
[0024] In step (1), optionally, an alcohol is added after hydrolysis, wherein the alcohol is a short-chain alcohol, preferably at least one of methanol and ethanol, in order to improve the solubility of the obtained tetraacid;
[0025] The alcohol content of the tetra-acid solution is less than 20 wt %, preferably 5 to 15 wt %.
[0026] In the preparation method of the present invention, in step (2), the alcohol is at least one of methanol, ethanol, isopropanol and tert-butanol.
[0027] After the salt is obtained by reaction in step (2), the salt may be filtered, dried, and other common steps.
[0028] In the preparation method of the present invention, in step (3), the solid content of the salt is 0.05 to 2 wt%, preferably 0.1 to 1 wt%;
[0029] The temperature of the hydrothermal synthesis is 160 to 220° C., preferably 180 to 200° C.; the time of the hydrothermal synthesis is 4 to 48 hours, preferably 6 to 24 hours.
[0030] After the polyimide nanoparticles are obtained in step (3), common steps such as washing, filtering, and drying may be performed.
[0031] According to a preferred embodiment of the present invention, the preparation method may include the following steps:
[0032] (1) dissolving the dianhydride in an aqueous solution and hydrolyzing it to obtain the corresponding tetraacid;
[0033] (2) dissolving the corresponding amine and adding it to the tetraacid solution to form salt, filtering, and washing;
[0034] (3) The salt is dispersed in an aqueous solution at a certain weight, and polyimide nanoparticles are hydrothermally synthesized;
[0035] (4) washing, filtering, and drying to obtain polyimide nanoparticles;
[0036] In the step (1), the dianhydride is dissolved in an aqueous solution, and the solid content of the added dianhydride monomer is controlled to be less than 5wt%, preferably 0.5wt% to 3wt%. After the monomer is added, the solution is heated and stirred, and the temperature is set at 60-90°C and the reaction time is 1-4h to allow the dianhydride monomer to fully react with water to obtain the corresponding tetraacid, and the process is as follows:
[0037]
[0038] The dianhydride is hydrolyzed by heat to give the tetraacid of the corresponding structure
[0039] The dianhydride is dissolved in aqueous solution. After the reaction, in order to improve the solubility of the tetraacid in water, some alcohol solvent can be added to dissolve the monomer. The alcohol solvent is selected to be methanol or ethanol, and the content of the added alcohol is less than 20% of the aqueous solution.
[0040] In the step (2), the corresponding amine is dissolved and then added to the tetraacid solution to form salt, filter and wash. The selected amine is a combination of a triamine or a tetraamine and a diamine with a polar hydrophilic group, wherein the polyamine is the main component, the molar ratio of the functional group accounts for 60% to 90%, and the preferred functional group accounts for 75% to 85%. The diamine with a polar hydrophilic group is a nanoparticle size regulator, and the molar ratio of its functional group accounts for 10% to 40%, and the preferred functional group is 15% to 25%.
[0041] The amine is dissolved in water or a mixed solvent of water and alcohol, wherein the molar ratio of the amino functional group in the added monomer to the anhydride functional group in the dianhydride is (0.95-1.05):1.
[0042] In the salt formation, filtration and washing process in step (2), ethanol is selected as the washing solution to dissolve and wash away the unreacted monomers.
[0043] In the step (3), a salt is dispersed in an aqueous solution with a certain weight, and polyimide nanoparticles are hydrothermally synthesized; wherein the salt is dispersed in water with a solid content of 0.05% to 2wt%, preferably with a solid content of 0.1 to 1wt%.
[0044] The hydrothermal synthesis temperature range is 160℃~220℃, preferably 180℃~200℃. The hydrothermal reactor can be used in a static non-stirring form or a stirring form, preferably a stirring form. The reaction time is 4h to 48h, preferably 6h to 24h. The structural process and product structural characteristic formula of the polyimide material obtained after the reaction are as follows:
[0045]
[0046] The above is the reaction structure formula of polyimide nanoparticles, wherein R1 represents different dianhydride groups, R2 represents different triamine groups, R3 represents different tetraamine groups, and R4 represents different diamine regulator structures.
[0047] In the step (4), the polyimide nanoparticles are washed, filtered and dried; a water / ethanol mixed solvent is used for washing, and then the solvent is gradually replaced with an ethanol solvent for washing and filtering to obtain a powder sample, and the polyimide nanoparticles are obtained by vacuum drying at room temperature.
[0048] The controllable preparation property of the nanoparticles is reflected in that, by adding a size regulator, nanoparticle spheres with a size between 0.1 and 5 μm can be obtained, and the nanoparticles have good size distribution.
[0049] The third object of the present invention is to provide the use of the polyimide nanoparticles or the polyimide nanoparticles obtained by the preparation method in modified polyimide materials.
[0050] The fourth object of the present invention is to provide a modified polyimide material, which is prepared by the following steps:
[0051] The polyimide nanoparticles or the polyimide nanoparticles obtained by the preparation method are dispersed in a solvent, mixed with polyamic acid or soluble polyimide, and then molded after being evenly dispersed.
[0052] The polyamic acid or polyimide may be in the form of a solution, a powder, or the like.
[0053] The solvent is the same as or has similar solubility to the solvent of the polyamic acid solution or the solution of the polyimide matrix to be modified, and does not cause phase separation or precipitation after being added.
[0054] The amount of the polyimide nanoparticles is 0.1 to 5 wt % of the amount of the polyamic acid or polyimide, preferably 0.5 to 2 wt %.
[0055] The forming process includes film coating, spinning and molding.
[0056] Preferably, the polyimide nanoparticles are ultrasonically dispersed in a solvent, and then added to a polyamic acid solution or a soluble polyimide solution to be modified, and then subjected to corresponding molding processing after being evenly dispersed.
[0057] The nanoparticles are dispersed in the solvent at 0.1wt% to 5wt% relative to the solid content of the solution to be modified, preferably at a solid content of 0.5wt% to 2wt%, and then blended with the solution to be modified after ultrasonic vibration for 0.2 to 2h, stirred and dispersed evenly, and then subjected to corresponding molding processing, including coating, spinning and molding.
[0058] The present invention solves the problem of insufficient compatibility and uneven dispersion when nanoparticles are used to modify polyimide materials. The performance of polyimide materials can be effectively improved by selecting similarly compatible polyimide nanoparticles and utilizing the performance advantages brought by the selected corresponding structures.
[0059] The present invention will be further described below by way of examples. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 .The electron microscope image of the polyimide nanoparticles in Example 1 shows a size distribution of 3 to 5 um.
[0061] Figure 2 .The electron microscope image of the polyimide nanoparticles of Example 2 shows a size distribution of 0.1 to 0.5 um.
[0062] Figure 3 .Infrared FTIR spectra of polyimide nanoparticles and precursor salts of Example 1.
[0063] Figure 4 Example 1: Thermal weight loss diagram of polyimide nanoparticles and dynamic weight change diagram of precursor salt during the test.
[0064] Figure 5 .Electron microscopy image of the polyimide nanoparticles of Comparative Example 1.
[0065] Figure 6 .Electron microscopy image of the polyimide nanoparticles of Comparative Example 2.
[0066] Figure 7 Comparative Example 2: Thermal weight loss diagram of polyimide nanoparticles and the dynamic change diagram of the weight of the precursor salt during the test with temperature. DETAILED DESCRIPTION
[0067] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0068] The raw materials used in the specific implementation manner of the present invention are commercially available.
[0069] The test equipment and test conditions used in the present invention are:
[0070] Porosity and average pore size of polyimide nanoparticles: The relevant data were obtained using a BET surface adsorption tester to statistically analyze the average pore size distribution and specific surface area of the nanoparticles.
[0071] Characterization of characteristic groups of polyimide nanoparticles: Determine the imidization of polyimide. Select Fourier infrared tester to calculate the characteristic peaks of imide group and amide group, and clarify the imidization degree. The wave number of CN stretching vibration peak in imide structure is greater than 1750cm -1 The peak wave number of CO stretching vibration in the structure formed by the carboxyl group in the salt and the amine is between 1700cm -1 Up to 1750cm -1 between.
[0072] Characterization of thermal properties of polyimide nanoparticles: Use thermal gravimetric test to calculate the weight loss of nanoparticles, examine whether there are some unimidized structures, and observe the temperature corresponding to when the thermal gravimetric loss reaches 5%. If weight loss occurs at around 200°C, it means that some unimidized structures are undergoing dehydration and imidization. Tests on nanoparticle precursor salts can be used to analyze and determine the reaction temperature corresponding to the start of water loss when the salt reacts.
[0073] Characterization of mechanical properties of blended materials: A universal tensile tester was used to characterize the mechanical properties of blended materials.
[0074] Characterization of thermal properties of blended materials: Thermal gravimetric test is used to characterize material stability, and thermomechanical analysis is used to calculate the material's glass transition temperature and thermal expansion coefficient.
[0075] Material wettability test: measured by contact angle tester. Water and diiodomethane were selected as test solutions, and the contact angle was measured and calculated to obtain the surface energy of the modified film.
[0076] Example 1
[0077] 1. Disperse 2.00 g of pyromellitic anhydride (9.16 mmol) into 98.00 g of water, heat the solution to 80°C and stir for 2 h until all the monomers are dissolved. At this time, the solution is a pyromellitic acid aqueous solution.
[0078] 2. Dissolve 1.51 g of tri(4-aminophenyl)amine (5.19 mmol) and 0.21 g of 3,5-diaminobenzoic acid (1.38 mmol) in water. After dissolution and dispersion, slowly add them to the pyromellitic acid solution to form a salt. After stirring, filter to obtain a powder solid. Select ethanol solvent for washing and filtration. After vacuum drying, obtain a salt monomer composed of acid and amine.
[0079] 3. Disperse 1.00 g of salt into 99.00 g of water, then transfer it to a hydrothermal reactor with stirring, set the reaction temperature to 180°C, and stir the reaction for 6 hours.
[0080] 4. The product was dispersed in a water / ethanol solution for washing, filtered, and the water / ethanol solution was gradually replaced with an ethanol solution. The final product was vacuum dried to obtain a powder sample. Spherical nanoparticles with a size distribution of 3 to 5 μm were obtained by electron microscopy. Figure 1 As shown. According to infrared test analysis, hydrothermal synthesis completely transforms the salt groups into imide, and no polyamide structure is observed, such as Figure 3 As shown, combined with the thermogravimetric analysis, the nanoparticles have good heat resistance, and the 5wt% weight loss temperature is 490℃, indicating that there are no unreacted groups in the particles, such as Figure 4 shown.
[0081] 5. Add 0.05g of powder sample to a certain mass of dimethylacetamide solution, ultrasonically disperse it for 1h, then add it to a solution containing 10g of polyamic acid, stir it thoroughly and cast the solution into a film, and further imidize it into a polyimide composite film.
[0082] 6. After composite modification, the tensile strength of the polyimide composite film increased from 151.3MPa to 178.8MPa, and the thermal expansion coefficient decreased from 35.6ppm / K to 28.9ppm / K.
[0083] Example 2
[0084] 1. Prepare pyromellitic acid solution as in step 1 of Example 1.
[0085] 2. Disperse 0.68 g of 1,3,5,7-tetraaminoadamantane (3.44 mmol) and 0.35 g of 3,5-diaminobenzoic acid (2.29 mmol) in an ethanol solution. After dissolving and dispersing, slowly add them to a pyromellitic acid solution to form a salt. Stir and filter to obtain a powder solid. Use an ethanol solvent for washing and filtration. After vacuum drying, obtain a salt monomer composed of an acid and an amine.
[0086] 3. Carry out hydrothermal reaction as in step 3 of Example 1.
[0087] 4. The sample was cleaned and dried as in step 4 of Example 1, and spherical nanoparticles with a size distribution of 0.1 to 0.5 μm were obtained by electron microscopy. Figure 2 shown.
[0088] 5. Carry out blending coating as in step 5 of Example 1 to prepare a polyimide composite film.
[0089] 6. After modification, the surface wettability of the polyimide composite membrane was improved, the water droplet contact angle decreased from 75° to 60°, and the composite membrane had better adsorption capacity for positively charged dye molecules in the solution.
[0090] Example 3
[0091] 1. Disperse 1.00 g of pyromellitic anhydride (4.58 mmol) and 1.35 g of 3,3,4,4-biphenyltetracarboxylic anhydride (4.58 mmol) into 97.65 g of water, heat the solution to 80°C and stir for 4 hours to react, add 10 g of ethanol to completely dissolve the two tetraacid monomers in the solution.
[0092] 2. Dissolve 1.51 g of tri(4-aminophenyl)amine (5.19 mmol) and 0.21 g of 3,5-diaminobenzoic acid (1.38 mmol) in water. After dissolution and dispersion, slowly add them to the pyromellitic acid solution to form a salt. After stirring, filter to obtain a powder solid. Select ethanol solvent for washing and filtration. After vacuum drying, obtain a salt monomer composed of acid and amine.
[0093] 3. Carry out hydrothermal reaction as in step 3 of Example 1.
[0094] 4. The sample was cleaned and dried as in step 4 of Example 1, and spherical nanoparticles with a size distribution of 2 to 4 μm were obtained by electron microscopy.
[0095] 5. The polyimide nanoparticles and polyimide molding powder are uniformly mixed and dispersed in a corresponding solvent, and a polyimide-based resin composite material can be obtained by molding.
[0096] 6. After mixing and modification, the glass transition temperature of polyimide resin increases from 250℃ to 265℃.
[0097] Example 4
[0098] 1. Carry out the hydrolysis reaction of anhydride as in step 1 of Example 1.
[0099] 2. Dissolve 1.51 g of tri(4-aminophenyl)amine (5.19 mmol) and 0.26 g of 2,5-diaminobenzenesulfonic acid (1.38 mmol) in water. After dissolution and dispersion, slowly add them to the pyromellitic acid solution to form a salt. After stirring, filter to obtain a powder solid. Select ethanol solvent for washing and filtration. After vacuum drying, obtain a salt monomer composed of acid and amine.
[0100] 3. Disperse 0.10 g of salt into 99.00 g of water, then transfer it to a hydrothermal reactor with stirring, set the reaction temperature to 180°C, and stir the reaction for 6 hours.
[0101] 4. The product was dispersed in a water / ethanol solution for washing, filtered, and the water / ethanol solution was gradually replaced with an ethanol solution. The final product was vacuum dried to obtain a powder sample. Spherical nanoparticles with a size distribution of 0.2 to 1 μm were obtained by electron microscopy characterization and statistics.
[0102] 5. Add 5 g of powder sample into a certain mass of dimethylacetamide solution, ultrasonically disperse it for 1 hour, then add it into a solution containing 1000 g of polyamic acid, stir it thoroughly and evenly to obtain polyamic acid fiber by solution spinning, and then obtain polyimide fiber by thermal imidization.
[0103] 6. Polyimide fiber is woven into filter bags after composite modification, which can adsorb and separate positively charged substances.
[0104] Comparative Example 1
[0105] 1. Carry out the hydrolysis reaction of anhydride as in step 1 of Example 1.
[0106] 2. Dissolve 1.78 g of tris(4-aminophenyl)amine (6.11 mmol) in water, and after dissolution and dispersion, slowly add it to the pyromellitic acid solution to form a salt, stir and filter to obtain a powder solid, select ethanol solvent for washing and filtration, and vacuum dry to obtain a salt monomer composed of acid and amine.
[0107] 3. Carry out hydrothermal reaction as in step 3 of Example 1 to obtain polyimide nanoparticles.
[0108] 4. The product was dispersed in a water / ethanol solution for washing, filtered, and the water / ethanol solution was gradually replaced with an ethanol solution. The final product was vacuum dried to obtain a powder sample. Electron microscopy showed that the obtained powder contained spherical nanoparticles and aggregates of fused nanoparticles, which may be aggregates that grew continuously during the molding process, such as Figure 5 shown.
[0109] 5. The product is ultrasonically dispersed in the solution and will settle after standing for a period of time, indicating that its aggregate dispersion is poor and may agglomerate and become incompatible after blending with the matrix material.
[0110] Comparative Example 2
[0111] 1. Carry out the hydrolysis reaction of anhydride as in step 1 of Example 1.
[0112] 2. Dissolve 1.39 g of 3,5-diaminobenzoic acid (9.16 mmol) in water, and after dissolution and dispersion, slowly add it to the pyromellitic acid solution to form a salt, stir and filter to obtain a powder solid, select ethanol solvent for washing and filtration, and vacuum dry to obtain a salt monomer composed of an acid and an amine.
[0113] 3. Carry out hydrothermal reaction as in step 3 of Example 1 to obtain polyimide nanoparticles.
[0114] 4. The product was dispersed in a water / ethanol solution for washing, filtered, and the water / ethanol solution was gradually replaced with an ethanol solution. The final product was vacuum dried to obtain a powder sample. Electron microscopy showed that the obtained nanoparticles were irregular particles with a size of less than 0.5 μm. Figure 6 shown.
[0115] 5. Since the selected anhydride amine monomers are relatively rigid and the selected diamine is a meta-structure, the molecular weight of the nanoparticles corresponding to the PI polymerization may not grow to a higher level, so the thermal stability of the nanoparticles is poor, and the thermal weight loss at 336°C has reached 5wt% (such as Figure 7 As shown), it is not suitable for improving the heat resistance of composite materials.
Claims
1. A polyimide nanoparticle, comprising a structural unit derived from at least one of a triamine or a tetraamine, a structural unit derived from a diamine with a polar hydrophilic group, and a structural unit derived from a dianhydride; the diamine with a polar hydrophilic group is selected from at least one of 3,5-diaminobenzoic acid, 3,4-diaminobenzoic acid, 2,4-diaminobenzenesulfonic acid, 2,5-diaminobenzenesulfonic acid, and 3,4-diaminobenzenesulfonic acid.
2. The polyimide nanoparticles according to claim 1, characterized in that: The dianhydride is selected from dianhydrides having a rigid structure; and / or, The triamine or tetraamine is selected from at least one of tris(4-aminophenyl)amine, 1,3,5-tris(aminophenyl)benzene, 1,3,5-tris(4-aminophenoxy)benzene, 4,4',4"-(1,3,5-triazine-2,4,6-triyl)triphenylamine, 4,4',4"-(1,3,5-triazine-2,4,6-triyl)tris(1,10-biphenyl)amine, 1,3,5,7-tetraaminoadamantane, and tetrakis(4-aminophenyl)methane.
3. The polyimide nanoparticles according to claim 2, characterized in that: The dianhydride is selected from at least one of pyromellitic dianhydride, 3,3,4,4-biphenyltetracarboxylic dianhydride, 2,3,3,4-biphenyltetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, cyclobutanetetracarboxylic dianhydride, and bicyclo[2.2.1]heptane-2,3,5,6-tetracarboxylic dianhydride.
4. The polyimide nanoparticle according to claim 1 or 2, characterized in that: The particle size of the polyimide nanoparticles is 0.1-5 μm.
5. A method for preparing the polyimide nanoparticles according to any one of claims 1 to 4, comprising reacting a dianhydride with an amine to form a salt, then dispersing the resulting salt in water, and hydrothermally synthesizing the polyimide nanoparticles, wherein the amine is a mixture of at least one of a triamine or a tetraamine and a diamine with a polar hydrophilic group.
6. The method for preparing polyimide nanoparticles according to claim 5, characterized in that: The molar ratio of the amino functional group of the amine to the anhydride functional group of the dianhydride is (0.95-1.05):1, and / or, In the amine, the molar ratio of the amino functional groups of the triamine and / or tetraamine to the total amino functional groups is 60-90%; the molar ratio of the amino functional groups of the diamine with polar hydrophilic groups to the total amino functional groups is 10-40%.
7. The method for preparing polyimide nanoparticles according to claim 5, characterized in that: The molar ratio of the amino functional groups of the triamine and / or tetraamine to the total amino functional groups is 75-85%; the molar ratio of the amino functional groups of the diamine with polar hydrophilic groups to the total amino functional groups is 15-25%.
8. The method for preparing the polyimide nanoparticles according to claim 5 or 6, comprising the following steps: (1) dissolving a dianhydride in water, hydrolyzing the dianhydride to obtain a tetraacid solution, and optionally adding an alcohol to the tetraacid solution; (2) dissolving an amine in water or a mixed solvent of water and alcohol, adding a tetraacid solution and stirring to react to obtain a salt; (3) dispersing the obtained salt in water and performing hydrothermal synthesis to obtain the polyimide nanoparticles.
9. The method for preparing polyimide nanoparticles according to claim 8, characterized in that: In step (1), the solid content of the dianhydride is less than 5 wt %; and / or, The hydrolysis temperature is 60-90° C. and the hydrolysis time is 1-4 hours.
10. The method for preparing polyimide nanoparticles according to claim 9, characterized in that: The solid content of the dianhydride is 0.5 to 3 wt %; and / or, The hydrolysis temperature is 70-80° C. and the hydrolysis time is 2-3 hours.
11. The method for preparing polyimide nanoparticles according to claim 8, characterized in that: In step (1), the alcohol is a short-chain alcohol; The alcohol content in the tetra-acid solution is less than 20 wt %.
12. The method for preparing polyimide nanoparticles according to claim 11, characterized in that: The alcohol is at least one of methanol and ethanol; The alcohol content in the tetra-acid solution is 5-15 wt %.
13. The method for preparing polyimide nanoparticles according to claim 8, characterized in that: In step (2), the alcohol is at least one of methanol, ethanol, isopropanol and tert-butanol.
14. The method for preparing polyimide nanoparticles according to claim 8, characterized in that: In step (3), the solid content of the salt is 0.05 to 2 wt %; and / or, The temperature of the hydrothermal synthesis is 160-220°C; the time of the hydrothermal synthesis is 4-48h.
15. The method for preparing polyimide nanoparticles according to claim 14, characterized in that: The solid content of the salt is 0.1 to 1 wt %; and / or, The temperature of the hydrothermal synthesis is 180-200°C; the time of the hydrothermal synthesis is 6-24h.
16. Use of the polyimide nanoparticles according to any one of claims 1 to 5 or the polyimide nanoparticles obtained by the preparation method according to any one of claims 5 to 15 in modifying polyimide materials.
17. A modified polyimide material is prepared by the following steps: The polyimide nanoparticles according to any one of claims 1 to 5 or the polyimide nanoparticles obtained by the preparation method according to any one of claims 5 to 15 are dispersed in a solvent, mixed with polyamic acid or soluble polyimide, and then molded after being uniformly dispersed.
18. The modified polyimide material according to claim 17, characterized in that: The amount of the polyimide nanoparticles is 0.1 to 5 wt % of the amount of the polyamic acid or polyimide; and / or, The forming process includes film coating, spinning and molding.
19. The modified polyimide material according to claim 18, characterized in that: The amount of the polyimide nanoparticles used is 0.5-2 wt % of the amount of the polyamic acid or polyimide used.