A titanium plate production process

By introducing a laterally movable grinding and washing machine in the degreasing process of titanium plate processing, instead of the belt grinding machine, the defects and high cost problems in the oxide removal process on the surface of titanium plate are solved, and process shortening and automatic operation efficiency are improved .

CN114535292BActive Publication Date: 2024-12-03WUXI YINZHEN MATERIAL TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210032041.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-12
Publication Date
2024-12-03
Estimated Expiration
2042-01-12

AI Technical Summary

Technical Problem

In the existing titanium plate processing technology, oxides exist on the surface of the roughly rolled titanium plate, which needs to be polished through a belt grinder, but this process has defects such as different plate shapes, abrasions, burns, etc., and low production efficiency , high costs lead to increased equipment management and employment costs, making it difficult to achieve automated operations.

Method used

In the degreasing process, a laterally movable grinding brushing machine is introduced to replace the belt grinding machine. The oxide on the surface of the titanium plate is mechanically removed, and chemical degreasing is combined to eliminate the original grinding process, shorten the process, and improve production efficiency.

Benefits of technology

By adding a horizontally movable grinding and washing machine in the degreasing process, the processing process is shortened, production efficiency is improved, defect losses caused by the belt grinder are avoided, production costs are reduced, and the integration of automated operations is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114535292B_ABST
    Figure CN114535292B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nonferrous metal processing, and discloses a titanium plate production process, which comprises the following steps: raw material→mechanical dephosphorization→rough rolling→degreasing grinding→finishing rolling→continuous annealing. By adding a laterally movable grinding and brushing machine in the degreasing process, the grinding process in the prior art is merged into the degreasing process, and the entire grinding equipment line of the original grinding process is eliminated and replaced by a single laterally movable grinding and brushing machine, which greatly shortens the processing cycle and simplifies the processing process. At the same time, the grinding effect after roughing is greatly improved, so that a titanium plate with better surface quality can be obtained, and the integrity of the automated operation is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nonferrous metal processing technology, in particular to a titanium plate production process. Background Art

[0002] At present, in the titanium plate processing process at home and abroad, due to the presence of titanium oxide on the surface of the titanium plate after rough rolling, it needs to be polished in a grinding unit to eliminate it. Grinding after the rough rolling process to obtain titanium metal plates with excellent surface quality is very important for the production and preparation of titanium plates. The existing grinding process usually uses a belt grinder as the main grinding production line. The common defects of grinding with a belt grinder after roughing are: different plate surface shapes, scratches, burns, etc. At the same time, the existing conventional grinding unit is an independent offline unit with low production efficiency and high cost.

[0003] After the rough rolling of titanium plate raw materials, the production labor cost and equipment management cost of setting up a production line for the entire grinding process are greatly increased. The processing process is cumbersome and the ideal automated operation effect cannot be achieved. Therefore, how to shorten the titanium plate processing process while ensuring excellent product surface quality after the rough rolling process, streamline the processing equipment line, and improve the efficiency of automated processing operations are the main issues that domestic and foreign titanium plate producers consider. Summary of the invention

[0004] In view of the shortcomings of the above-mentioned existing production technology, the present application provides a titanium plate production process, thereby eliminating the original grinding process, replacing the entire equipment line of the original grinding process with a single device, and merging it into the degreasing process, shortening the process, improving processing quality, and improving production efficiency.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A titanium plate production process comprises the following steps:

[0007] Step 1: Raw materials: Use purchased hot-rolled titanium plates as raw materials, and the raw material specifications are 4.0*1000mm (thickness*width);

[0008] Step 2: Mechanical phosphorus removal, by spraying sand on the surface of the raw material titanium plate to mechanically remove some oxides on the surface of the titanium plate;

[0009] Step 3: Rough rolling, rough rolling the titanium plate after dephosphorization to reduce the thickness of the titanium plate;

[0010] Step 4: Degreasing and grinding: grinding the titanium plate after rough rolling to remove oxides, and then using organic alkali to chemically degrease it to clean the dirt and grease on the surface of the strip;

[0011] Step 5: Finish rolling, the titanium plate after degreasing and grinding is finished rolling, and the thickness of the titanium plate after finishing rolling ranges from 0.05 to 0.5 mm;

[0012] Step 6: Continuous annealing. The annealing process of the titanium plate after fine rolling is preheating → natural gas heating furnace → entering the slow cooling section → jet cooling device.

[0013] Preferably, the deformation amount after rough rolling is 50% of the raw material titanium plate.

[0014] Preferably, during degreasing and grinding, the action flow of the unit is: unwinder → tension roller → chemical cleaning → scrubber → rinsing → pickling → laterally movable grinding scrubber → pure water spray → hot air drying → tension roller → winding.

[0015] Preferably, during degreasing and grinding, the concentration of the degreasing medium organic base is 3-5%, and the temperature is 65±5°C.

[0016] Preferably, the finishing rolling production and the roughing rolling production are carried out in the same equipment, and the control requirements are equivalent.

[0017] Preferably, the maximum furnace temperature of the heat treatment furnace during continuous annealing is 1050°C, the control accuracy is ±5°C, and the protective atmosphere parameters are 100% Ar, residual O2≤3ppm, and the dew point after purification is -65°C.

[0018] Preferably, the rolling mill is a multi-roll reversible rolling mill during rough rolling, the pressing thickness of the rolling mill is controlled by hydraulic pressing thickness automatic control (AGC) technology, the deformation of each pass of the rolling mill is ≤15%, and the concentration of the emulsion is 4-6%. The beneficial effects of the present invention are as follows:

[0019] 1. Adding a horizontally movable grinding and scrubbing machine in the degreasing process can save the original "grinding" process, shorten the processing steps, improve production efficiency, and shorten the production cycle by 15% on the original basis;

[0020] 2. Use a laterally movable grinding and brushing machine to replace the belt grinder in the prior art to grind and remove the oxide on the surface of the titanium plate, avoiding the defect loss caused by the original belt grinder and increasing economic benefits;

[0021] 3. By adding a laterally movable grinding and brushing machine to the next degreasing process, the entire equipment line required for the original grinding process is eliminated. A single machine replaces the entire equipment line and is added to the degreasing process. The two are carried out simultaneously, which greatly improves the integrity of automated operations and saves production labor and equipment management costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a process flow chart of the present invention;

[0023] Figure 2It is a three-dimensional schematic diagram of a laterally movable grinding and scrubbing machine in the degreasing and grinding process of the present invention;

[0024] Figure 3 for Figure 2 A front view of

[0025] Figure 4 for Figure 2 A schematic diagram of the structure of the middle and lower brush roller assembly;

[0026] Figure 5 for Figure 4 Sectional view at AA in the middle;

[0027] Figure 6 for Figure 2 A schematic diagram of the structure of the middle and upper brush roller assembly;

[0028] Figure 7 for Figure 6 Cross-sectional view at the middle BB.

[0029] Among them, 1. frame; 2. brushing mechanism; 4. cylinder with spring; 6. screw jack; 7. gear motor; 8. cylinder; 9. first motor; 10. linear guide; 11. base; 12. titanium plate; 13. intermediate shaft; 14. motor bracket; 15. second motor; 20. upper brush roller assembly; 21. lower brush roller assembly; 201. bearing seat; 202. spherical roller bearing; 203. core shaft; 204. brush roller; 205. push ring; 206. retaining ring; 207. brush roller pressure plate; 208. first guide wheel shaft; 209. deep groove ball bearing; 210. first guide wheel; 211. herringbone frame; 212. second guide wheel shaft; 213. second guide wheel. DETAILED DESCRIPTION

[0030] The specific implementation of the present invention is described below in conjunction with the accompanying drawings.

[0031] A titanium plate production process, such as Figure 1 As shown, it includes the following steps:

[0032] Step 1: Raw materials: Use purchased hot-rolled titanium plates as raw materials, and the raw material specifications are 4.0*1000mm (thickness*width);

[0033] Step 2: Mechanical phosphorus removal, by spraying sand on the surface of the raw material titanium plate to mechanically remove some oxides on the surface of the titanium plate;

[0034] Step 3: Rough rolling, rough rolling the titanium plate after dephosphorization to reduce the thickness of the titanium plate;

[0035] Step 4: Degreasing and grinding: grinding the titanium plate after rough rolling to remove oxides, and then chemically degreasing it with organic alkali to clean the dirt and grease on the surface of the strip;

[0036] Step 5: Finish rolling, the titanium plate after degreasing and grinding is finished rolling, and the thickness of the titanium plate after finishing rolling ranges from 0.05 to 0.5 mm;

[0037] Step 6: Continuous annealing. The annealing process of the titanium plate after fine rolling is preheating → natural gas heating furnace → entering the slow cooling section → jet cooling device.

[0038] In the embodiment of the present invention, the deformation amount after rough rolling is 50% of the raw material titanium plate.

[0039] In the embodiment of the present invention, during degreasing and grinding, the action flow of the unit is: unwinder → tension roller → chemical cleaning → scrubber → rinsing → pickling → laterally movable grinding scrubber → pure water spray → hot air drying → tension roller → winding.

[0040] In the embodiment of the present invention, during degreasing and grinding, the concentration of the degreasing medium organic base is 3-5%, and the temperature is 65±5°C.

[0041] In the embodiment of the present invention, the finishing rolling production and the rough rolling production are carried out in the same equipment, and the control requirements are equivalent.

[0042] In the embodiment of the present invention, the maximum furnace temperature of the heat treatment furnace during continuous annealing is: 1050°C, the control accuracy is: ±5°C; the protective atmosphere parameters are: 100% Ar, residual O2≤3ppm, and the dew point after purification is -65°C.

[0043] In the embodiment of the present invention, the rolling mill is a multi-roll reversible rolling mill during rough rolling, the pressing thickness of the rolling mill is controlled by the hydraulic pressing thickness automatic control (AGC) technology, the deformation of each pass of the rolling mill is ≤15%, and the concentration of the emulsion is 4-6%. In the embodiment of the present invention, the finishing rolling production and the rough rolling production are carried out in the same equipment, and the control requirements are equivalent.

[0044] In the embodiment of the present invention, the maximum furnace temperature of the heat treatment furnace during continuous annealing is: 1050°C, the control accuracy is: ±5°C; the protective atmosphere parameters are: 100% Ar, residual O2≤3ppm, and the dew point after purification is -65°C.

[0045] In the embodiment of the present invention, the rolling mill is a multi-roll reversible rolling mill during rough rolling, the pressing thickness of the rolling mill is controlled by hydraulic pressing thickness automatic control (AGC) technology, the deformation of each pass of the rolling mill is ≤15%, and the concentration of the emulsion is 4-6%.

[0046] The processing process of the prior art is: raw materials → mechanical dephosphorization → rough rolling → grinding → degreasing → fine rolling → continuous annealing. After the rough rolling process, the surface of the titanium plate is ground by a belt grinder. Grinding with a belt grinder is prone to cause the following problems: 1. Residual sand; 2. Uneven grinding; 3. Inconvenient operation and difficult to control the grinding position; 4. When the plate shape is poor: excessive grinding and pressing down is prone to scratches, and the over-cleared position is not ground cleanly; 5. The consumption of the sand belt is large and the cost is too high.

[0047] like Figure 1 In the embodiment shown, the process flow of the present invention is: raw material → mechanical dephosphorization → rough rolling → degreasing grinding (adding a laterally movable grinding and brushing machine) → finishing rolling → continuous annealing. By adding a grinding and brushing machine to the degreasing process, degreasing and grinding are carried out simultaneously on the titanium plate after the rough rolling to reduce the thickness, which can save the original grinding process, shorten the processing steps, improve production efficiency, and shorten the production cycle by 15% on the original basis. At the same time, the addition of the laterally movable grinding and brushing machine avoids the defect loss caused by the original belt grinder and increases economic benefits.

[0048] like Figure 2 , Figure 3 , Figure 4 , Figure 5 , Figure 6 and Figure 7 In the illustrated embodiment, the specific structure of the laterally movable grinding and brushing machine is as follows: it includes a frame 1, in which a brushing mechanism 2 is symmetrically installed, the brushing mechanism 2 includes an upper brush roller assembly 20 located at the top and a lower brush roller assembly 21 located at the bottom, and a working gap is left between the upper brush roller assembly 20 and the lower brush roller assembly 21, and the working gap is used to insert the titanium plate 12 through the feed port, and the oxide on the surface of the titanium plate 12 is brushed by the cooperation of the upper brush roller assembly 20 and the lower brush roller assembly 21. The upper brush roller assembly 20 and the lower brush roller assembly 21 both include a pair of bearing seats 201 for supporting the body of the upper brush roller assembly 20. The mandrel 203 is rollingly mounted in the bearing seat 201 through a self-aligning roller bearing 202. A brush roller 204 is fixed in the middle of the mandrel 203. The brush roller 204 is axially fixed by setting a push ring 205 and a retaining ring 206 on both sides of the axial direction. The push ring 205 and the brush roller 204 are assisted by setting a brush roller 204 pressure plate. A pair of first guide wheel shafts 208 are also arranged at the bottom of the bearing seat 201. The first guide wheel shaft 208 is rollingly mounted with a first guide wheel 210 through a deep groove ball bearing 209. The upper brush roller assembly 20 also includes a herringbone frame 211 detachably arranged on the top of the bearing seat 201. A second guide wheel shaft 212 is arranged below the top two sides of the herringbone frame 211. A second guide wheel 213 is rollingly mounted on the second guide wheel shaft 212 through a deep groove ball bearing 209.

[0049] The left and right sides of the frame 1 are fixed with spring-loaded horizontal cylinders 8 to position and fix the brushing mechanism 2 in the horizontal direction. The driving end of the spring-loaded horizontal cylinder 8 and the bearing seat 201 are arranged at the same horizontal height, so that the bearing seat 201 can be pressed against and fixed, making the bearing seat 201 stable and reliable. After the brushing mechanism 2 is inserted into the frame 1, the spring-loaded horizontal cylinder 8 exhausts the air, and its driving end presses against the bearing seat 201 and fixes the bearing seat 201 only with the spring force. Screw jacks 6 are fixed on the upper and lower end surfaces on both sides of the front and rear sides of the frame 1, and the bearing seat 201 is positioned and fixed in the vertical direction by the screw jacks 6, thereby ensuring the support and fixation of the brushing mechanism 2 in the vertical direction; the driving section of the screw jack 6 is connected to the gear motor 7 arranged on one side of the screw jack 6, thereby driving the screw jack 6 to be pressed down or loosened.

[0050] like Figure 2 and Figure 3 In the illustrated embodiment, the screw jack 6 between the front end face and the rear end face of the frame 1 is connected by transmission via an intermediate shaft 13, thereby ensuring the accuracy and stability of the synchronous operation.

[0051] like Figure 2 and Figure 3 In the illustrated embodiment, four cylinders 8 are further provided on the top of the frame 1, and two cylinders 8 are fixedly arranged on both sides of the screw jack 6 above in a group, and the driving ends of the cylinders 8 cooperate with the outer contour of the top of the herringbone frame 5 to prevent the screw jack 6 from backlashing.

[0052] like Figure 2 and Figure 3 In the embodiment shown, a motor bracket 14 is further arranged at the rear of the frame 1. The motor bracket 14 is divided into two horizontal heights. A first motor 9 is arranged on the motor bracket 14 at a height parallel to the upper brush roller assembly 20. The first motor 9 is connected to the mandrel 203 by transmission. A second motor 15 is arranged on the motor bracket 14 at a height parallel to the lower brush roller assembly 21. The second motor 15 is connected to the mandrel by transmission. The upper brush roller assembly 20 and the lower brush roller assembly 21 are driven to roll by the first motor 9 and the second motor 15, so as to scrub the oxides on the upper and lower surfaces of the titanium plate 12.

[0053] like Figure 2 and Figure 3 In the shown embodiment, a base 11 is arranged under the frame 1, and a linear guide 10 is arranged between the base 11 and the frame 1 to adjust the linear displacement of the laterally movable grinding and brushing machine, so that the grinding and brushing machine can be perpendicular to the processing material and move laterally in the horizontal direction, thereby obtaining the following advantages: 1. The contact surface between the brushing mechanism 2 and the titanium plate 12 can be adjusted to obtain the required surface morphology; 2. The brushing mechanism 2 is fully utilized, and its service life is extended / the replacement cycle is reduced; 3. The lateral movement can make the bristles of the brushing mechanism 2 evenly distributed, and the surface quality of the processing material is more effectively guaranteed.

[0054] In the embodiment of the present invention, the motor parameters used are 75kW, 6P, and a frequency converter is used to make the brush roller speed adjustable. The brush roller load is controlled by the load current of the brush roller motor. The load current is automatically adjusted by multiplying the empirical coefficient by different plate widths (a bandwidth signal is required), and the brush roller load can be divided into eight modes for selection. The setting content of the brush roller load is modified by the indicator light on the B-Pack. In addition, up to three brush roller modes can be stored, and each brush roller mode can be selected by the selection switch on the operation panel.

[0055] In the embodiment of the present invention, each brushing mechanism 2 is a reverse grinding brush, which adopts the "brush to brush" technology to control the horizontal force and vertical force of the brushing, accurately control the brushing power, and set different "speed-pressure" modes. During the operation, a grinding equipment body that can be moved laterally has been developed to extend the service life of the brushing mechanism 2 and to obtain more effective cleaning of the board surface quality.

[0056] In the embodiment of the present invention, the brushing mechanism 2 provides a position memory function, so that the brushing mechanism 2 returns to the brushing position from the temporary retreat position of the welding point in the shortest time. Due to the wear of the brushing mechanism 2, the fixed high-speed pressing mode requires time to press down again, but the memory function enables the brushing mechanism 2 to shorten the high-speed pressing distance, and the brushing mechanism 2 can return to the brushing position in the shortest time, thereby minimizing the unbrushed part of the processed material.

[0057] By adding a transversely movable grinding and brushing machine in the degreasing unit after the rough rolling process of the present invention, the action sequence of: uncoiler - tension roller - chemical cleaning - brushing machine - rinsing - pickling - transversely movable grinding and brushing machine - pure water spray - hot air drying - tension roller - winding is achieved. Compared with the prior art, the original "grinding" process performed by the belt grinder can be omitted, the overall processing process is greatly shortened, the production efficiency is improved, and the production cycle is shortened by 15% on the original basis; at the same time, the transversely movable brushing machine can effectively avoid the defect loss caused by the original belt grinder. The transversely movable brushing machine is added to the degreasing process, and the two are carried out simultaneously, the processing and production quality is improved, the equipment line of the entire process is replaced by a single machine, and merged into the unit of the next process, which greatly improves the integration of automation and saves the costs of manual production, equipment management, etc.

[0058] The above description is an explanation of the present invention, not a limitation of the present invention. The scope of the present invention is defined in the claims. Any form of modification may be made within the scope of protection of the present invention.

Claims

1. A titanium plate production process, characterized in that: The process includes the following steps: Step 1: Raw materials: hot-rolled titanium plate is used as raw material, and the raw material specification is 4.0*1000mm (thickness*width); Step 2: Mechanical phosphorus removal, by spraying sand on the surface of the raw material titanium plate to mechanically remove some oxides on the surface of the titanium plate; Step 3: Rough rolling, rough rolling the titanium plate after dephosphorization to reduce the thickness of the titanium plate; Step 4: Degreasing and grinding: grinding the titanium plate after rough rolling to remove oxides, and then using organic alkali to chemically degrease it to clean the dirt and grease on the surface of the strip; Step 5: Finish rolling, the titanium plate after degreasing and grinding is finished rolling, and the thickness of the titanium plate after finishing rolling ranges from 0.05 to 0.5 mm; Step 6: Continuous annealing: the annealing process of the titanium plate after fine rolling is preheating → natural gas heating furnace → entering the slow cooling section → jet cooling device; It also includes a transversely movable grinding and brushing machine for implementing the titanium plate production process, the movable grinding and brushing machine includes a frame (1), a brushing mechanism (2) is installed in the frame (1) in a left-right symmetrical manner, the brushing mechanism (2) includes an upper brush roller assembly (20) located at the top and a lower brush roller assembly (21) located at the bottom, a working gap is left between the upper brush roller assembly (20) and the lower brush roller assembly (21), the working gap is used to insert the titanium plate (12) through the feed port, and the upper brush roller assembly (20) and the lower brush roller assembly (21) cooperate to brush the oxide on the surface of the titanium plate (12); the upper brush roller assembly (20) and the lower brush roller assembly (21) each include a pair of bearing seats (201) for supporting the body of the upper brush roller assembly (20), and a spherical roller bearing (202) is rollingly installed in the bearing seat (201). The shaft (203) is provided with a brush roller (204) fixed in the middle of the core shaft (203). The brush roller (204) is axially fixed by arranging push rings (205) and retaining rings (206) on both sides of the shaft. A brush roller pressure plate (207) is arranged between the push ring (205) and the brush roller (204) for auxiliary fixing. A pair of first guide wheel shafts (208) are also arranged at the bottom of the bearing seat (201). A first guide wheel (210) is rollably mounted on the first guide wheel shaft (208) via a deep groove ball bearing (209). The upper brush roller assembly (20) further comprises a herringbone frame (211) detachably arranged on the top of the bearing seat (201). Second guide wheel shafts (212) are arranged below both sides of the top of the herringbone frame (211). A second guide wheel (213) is rollably mounted on the second guide wheel shaft (212) via a deep groove ball bearing (209).

2. A titanium plate production process as claimed in claim 1, characterized in that: The deformation amount after the rough rolling is 50% of the raw material titanium plate.

3. A titanium plate production process as claimed in claim 1, characterized in that: During the degreasing and grinding, the action flow of the unit is: unwinder → tension roller → chemical cleaning → scrubber → rinsing → pickling → laterally movable grinding scrubber → pure water spraying → hot air drying → tension roller → winding.

4. A titanium plate production process as claimed in claim 1 or 3, characterized in that: During the degreasing and grinding, the concentration of the degreasing medium organic base is 3-5%, and the temperature is 65±5°C.

5. A titanium plate production process as claimed in claim 1, characterized in that: The finishing rolling production and the rough rolling production are carried out in the same equipment, and the control requirements are consistent.

6. A titanium plate production process as claimed in claim 1, characterized in that: The maximum furnace temperature of the heat treatment furnace during the continuous annealing is 1050°C, the control accuracy is ±5°C, and the protective atmosphere parameters are 100% Ar, residual O2≤3ppm, and the dew point after purification is -65°C.

7. A titanium plate production process as claimed in claim 1 or 2, characterized in that: The rolling mill during the rough rolling is a multi-roll reversible rolling mill, and the pressing thickness of the rolling mill is controlled by the hydraulic pressing thickness automatic control (AGC) technology. The deformation of each pass of the rolling mill is ≤15%, and the concentration of the emulsion is 4-6%.