Packaging film
By forming a multi-layer encapsulation film on the surface of the organic electronic device, using the particle size adjustment and adsorption energy calculation of the hygroscopic agent and bright spot inhibitor, the problem of moisture and oxygen intrusion and bright spots is solved, and an efficient moisture barrier and bright spot prevention is achieved, improving the Durability and stability of the device.
Patent Information
- Application Number
- CN202080072894.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-10-28
AI Technical Summary
Organic electronic devices, such as OLEDs, are susceptible to moisture and oxidation factors, leading to durability issues and bright spot problems. It is difficult for existing technologies to effectively block external moisture and oxygen intrusion while preventing bright spots caused by internal exhaust.
Using an encapsulation film, including an encapsulation layer, by forming a multi-layer structure on the surface of the organic electronic device, using hygroscopic agents and bright spot inhibitors to adjust the particle size distribution and particle size ratio, and combining density functional theory to calculate adsorption energy to achieve moisture barriers and bright spots. prevent.
Effectively blocks external moisture and oxygen intrusion, prevents internal bright spots, improves the long-term durability and reliability of organic electronic devices, and ensures stability in harsh environments.
Smart Images

Figure CN114555358B_ABST
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2019-0134808, filed on October 28, 2019, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0004] The present application relates to an encapsulation film, an organic electronic device including the same, and a method for manufacturing the organic electronic device. Background Art
[0005] An organic electronic device (OED) means a device including an organic material layer that generates alternating current of charges using holes and electrons, and examples thereof may include a photovoltaic device, a rectifier, an emitter, an organic light emitting diode (OLED), and the like.
[0006] Organic light emitting diodes (OLEDs) in the above organic electronic devices have lower power consumption and faster response speed than existing light sources, and are conducive to making display devices or lighting equipment thinner. In addition, OLEDs have space availability and are therefore expected to be applied to various fields including various portable devices, monitors, notebook computers, and TVs.
[0007] In the commercialization and application expansion of OLED, the most important issue is the durability issue. The organic materials and metal electrodes contained in OLED are very easily oxidized by external factors such as moisture. In addition, there is also the problem of bright spots of OLED caused by the exhaust gas that may occur inside the OLED device. That is, products including OLED are very sensitive to environmental factors. Therefore, various methods have been proposed to suppress the exhaust gas generated inside while effectively blocking oxygen or moisture from penetrating into organic electronic devices such as OLED from the outside.
[0008] Public Content
[0009] Technical issues
[0010] The present application provides an encapsulation film that allows formation of a structure capable of blocking moisture or oxygen from entering an organic electronic device from the outside and can prevent bright spots from being generated in the organic electronic device.
[0011] Technical Solution
[0012] The present application relates to a packaging film, which can be used as a packaging layer or to package an organic electronic device such as an OLED.
[0013] In this specification, the term "organic electronic device" means a product or device having a structure including an organic material layer that generates an alternating current of charges using holes and electrons between a pair of electrodes facing each other, and examples thereof may include but are not limited to photovoltaic devices, rectifiers, emitters, and organic light emitting diodes (OLEDs), etc. In one example of the present application, the organic electronic device may be an OLED.
[0014] The encapsulation film of the exemplary organic electronic element may include an encapsulation layer. The encapsulation layer may encapsulate the entire surface of the organic electronic element formed on the substrate. In one example, the encapsulation layer may include a hygroscopic agent, a bright spot inhibitor, and an encapsulation resin. In addition, in the present application, as a result of analyzing the particle size of the hygroscopic agent and bright spot inhibitor contained in the sample passed by dissolving the encapsulation layer in an organic solvent and then filtering it through a 300-mesh nylon filter, the value according to the following general formula 1 can satisfy the range of 2.4 to 3.6. That is, for the following general formula 1, first, the encapsulation layer is dissolved in an organic solvent. Thereafter, the dissolved encapsulation layer composition is filtered through a 300-mesh nylon filter, and the encapsulation layer composition passed is sampled. The hygroscopic agent and bright spot inhibitor contained in the sampled sample are subjected to particle size analysis. As a result of the particle size analysis, D10, D50, and D90 are calculated and substituted into the following general formula 1. The lower limit of the value calculated according to the following general formula 1 may be, for example, 2.4, 2.5, 2.6, 2.7, 2.75, 2.8, 2.85, 2.9, 2.95, 3.0, 3.05, 3.1, 3.15 or 3.17 or more, and the upper limit may be, for example, 3.6, 3.5, 3.4, 3.3, 3.28, 3.25, 3.2, 3.0, 2.95, 2.9, 2.85, or 2.8 or less.
[0015] [General formula 1]
[0016]
[0017] In the above general formula 1, D10 is the average particle size according to the particle size analysis result D10, D50 is the average particle size according to the particle size analysis result D50, and D90 is the average particle size according to the particle size analysis result D90. The unit is μm. The particle size analysis can be a particle size distribution measured according to ISO13320:2009. The definitions of D10, D50 and D90 are as defined in the particle size analysis. As a result of the particle size analysis, relative to the maximum value in the cumulative distribution of the particle size, D10, D50 and D90 may mean the sizes corresponding to 10%, 50% and 90%, respectively. Conventionally, the size of the particles contained in the encapsulation layer is simply controlled by the average particle size, but the present application adjusts the absolute value of D50 (which corresponds to the particle size of 50% of the volume accumulation in the cumulative distribution of the particles) and the appropriate ratio between the particles having a small particle size and the particles having a large particle size. By doing so, the present application can prevent bright spots by hydrogen adsorption while achieving moisture barrier properties, and achieve long-term durable reliability of organic electronic devices even in harsh environments because curing properties are not deteriorated.
[0018] In one example, the ratio of the average particle size according to D50 of the moisture absorbent and the bright spot inhibitor to the average particle size according to the particle size analysis result D10 may be in the range of 2.0 to 4.0. The lower limit of the ratio may be, for example, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, or 2.7 or more, and the upper limit may be, for example, 4.0, 3.9, 3.8, 3.7, 3.6, 3.5, 3.4, 3.3, 3.2, 3.1, 3.0, 2.95 or 2.93.
[0019] In one embodiment, the type of organic solvent is not particularly limited, but may be, for example, toluene, and the sample may be, for example, a sample cut into 1.5 cm × 1.5 cm samples and measured. In addition, in the present specification, the unit mesh may be a unit of the American ASTM standard. When the encapsulation layer is attached to a glass substrate and / or a metal layer, the encapsulation layer may be separated from the metal layer by decapsulating it from the glass substrate and then immersing it in liquid nitrogen, wherein the decapsulation method is not limited thereto, and known methods may be used. The present application can quantitatively calculate the particle size distribution by particle size analysis. In addition, the filtration of the encapsulation layer by filtration is to remove impurity particles such as dust introduced during the re-dissolution process.
[0020] In one example, the ratio of the average particle size of the bright spot inhibitor to the average particle size of the moisture absorbent can be 2.0 or less according to D50 particle size analysis. The lower limit of the particle size ratio can be 0.01, 0.1, 0.15, 0.18, 0.2, 0.23, 0.25, 0.3, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, or 1.1 or more, and the upper limit can be 1.9, 1.8, 1.7, 1.6, 1.5, 1.4, 1.3, 1.2, 1.1, 1.0, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, or 0.3 or less. The original purpose of the packaging film of the present application is to block moisture from the outside, wherein a bright spot inhibitor is newly introduced to solve another technical problem of hydrogen adsorption, but there is a technical problem that it is not easy to maintain the initial moisture barrier effect while including the bright spot inhibitor. The present invention achieves excellent bright spot prevention performance while maintaining the original moisture barrier effect by adjusting the particle size distribution and / or particle size ratio of the moisture absorbent and the bright spot inhibitor.
[0021] In the present specification, the term "moisture absorbent" may mean a chemically reactive adsorbent as described below that is capable of removing moisture or moisture, for example, by chemically reacting with moisture or moisture that penetrates into a packaging film.
[0022] For example, the hygroscopic agent may be present in the encapsulation layer or the encapsulation film in a uniformly dispersed state. Here, the uniformly dispersed state may mean that the hygroscopic agent exists in the same or substantially the same density even in any part of the encapsulation layer or the encapsulation film. The hygroscopic agent that can be used for the above may include, for example, metal oxides, sulfates or organic metal oxides, etc. Specifically, examples of sulfates may include magnesium sulfate, sodium sulfate or nickel sulfate, etc., and examples of organic metal oxides may include aluminum oxide octanoate, etc. Here, specific examples of metal oxides may include phosphorus pentoxide (P2O5), lithium oxide (Li2O), sodium oxide (Na2O), barium oxide (BaO), calcium oxide (CaO) or magnesium oxide (MgO), etc., examples of metal salts may include sulfates, such as lithium sulfate (Li2SO4), sodium sulfate (Na2SO4), calcium sulfate (CaSO4), magnesium sulfate (MgSO4), cobalt sulfate (CoSO4), gallium sulfate (Ga2(SO4)3), titanium sulfate (Ti(SO4)2) or nickel sulfate (NiSO4), metal halides such as calcium chloride (CaCl 2), magnesium chloride (MgCl2), strontium chloride (SrCl2), yttrium chloride (YCl3), copper chloride (CuCl2), cesium fluoride (CsF), tantalum fluoride (TaF5), niobium fluoride (NbF5), lithium bromide (LiBr), calcium bromide (CaBr2), cesium bromide (CeBr3), selenium bromide (SeBr4), vanadium bromide (VBr3), magnesium bromide (MgBr2), barium iodide (BaI2) or magnesium iodide (MgI2), or metal chlorates such as barium perchlorate (Ba(ClO4)2) or magnesium perchlorate (Mg(ClO4)2), etc., but not limited to these. As a desiccant that can be included in the encapsulation layer, one or two or more of the above-mentioned components can also be used. In one example, when two or more are used as desiccant, calcined dolomite, etc. can be used.
[0023] Such a hygroscopic agent can be controlled to a suitable size according to the application. In one example, the average particle size of the hygroscopic agent can be controlled to be 100nm to 15000nm, 500nm to 10000nm, 800nm to 8000nm, 1μm to 7μm, 1.5μm to 5μm or 1.8μm to 3μm. The hygroscopic agent with a size within the above range is easy to store because the reaction rate with moisture is not too fast, does not damage the components to be packaged, and can effectively remove moisture without interfering with the hydrogen adsorption process associated with the above-mentioned bright spot inhibitor. In this specification, unless otherwise specified, the particle size may mean the average particle size, and may be the particle size measured by a known method with a D50 particle size analyzer.
[0024] The content of the desiccant is not particularly limited, and it can be appropriately selected in consideration of the desired barrier properties. In one example, the weight ratio of the bright spot inhibitor to the desiccant of the encapsulation film of the present application can be in the range of 0.001 to 0.5 or 0.01 to 0.1. In the present application, the bright spot inhibitor is dispersed in the film to prevent bright spots, but considering the moisture barrier properties and reliability of the element that realizes the original function as the encapsulation film, the bright spot inhibitor added to prevent bright spots can be included with the desiccant in a specific content ratio. The desiccant is included in the range of 5 to 250 parts by weight relative to 100 parts by weight of the encapsulation resin.
[0025] As described above, the encapsulation layer of the present application may include a bright spot inhibitor. The adsorption energy of the bright spot inhibitor for exhaust gas as calculated by the approximate method of density functional theory may be 0 eV or less. The lower limit of the adsorption energy is not particularly limited, but may be -20 eV. The type of exhaust gas is not particularly limited, but may include oxygen, H atoms, H2 molecules and / or NH3. Since the encapsulation film includes a bright spot inhibitor, the present application can prevent bright spots caused by exhaust gas generated in an organic electronic device.
[0026] In one embodiment of the present application, the adsorption energy between the bright spot inhibitor and the atoms or molecules that cause the bright spot can be calculated by electronic structure calculations based on density functional theory. The above calculations can be performed by methods known in the art. For example, in the present application, a two-dimensional flat plate structure in which the densest packed surface of the bright spot inhibitor having a crystal structure is exposed on the surface is constructed, and then the structure is optimized, and the structure in which the molecules that cause the bright spots are adsorbed on the surface in the vacuum state is structurally optimized, the value obtained by subtracting the total energy of the molecules that cause the bright spots from the total energy difference of the two systems is defined as the adsorption energy. For the total energy calculation of each system, a modified PBE function as a function of the GGA (Generalized Gradient Approximation) series is used as an exchange-correlation to simulate the interaction between electrons, and the cutoff value of the electron kinetic energy used is 500eV, and only the gamma point corresponding to the origin of the reciprocal space is included and calculated. The conjugate gradient method is used to optimize the atomic structure of each system and iterative calculations are performed until the interatomic force is or smaller. A series of calculations were performed by VASP which is a commercially available code.
[0027] The material of the bright spot suppressor is not limited as long as the material has the effect of preventing bright spots on the panel of the organic electronic device when the encapsulation film is applied to the organic electronic device. For example, the bright spot suppressor can be a material that can absorb the following materials: for example, oxygen, H2 gas, ammonia (NH3) gas, H + NH 2+ , NHR2 or NH2R. Here, R may be an organic group, and for example, may be exemplified by an alkyl group, an alkenyl group, an alkynyl group, etc., but is not limited thereto.
[0028] In one example, the material of the bright spot inhibitor is not limited, as long as it meets the above adsorption energy value, and it can be a metal or a non-metal. The bright spot inhibitor can include, for example, Li, Ni, Ti, Rb, Be, Mg, Ca, Sr, Ba, Al, Zn, In, Pt, Pd, Fe, Cr, Si, or a combination thereof, can include oxides or nitrides of the materials, and can include alloys of the materials. In one example, the bright spot inhibitor can include nickel particles, nickel oxide particles, titanium nitride, titanium-based iron-titanium alloy particles, manganese-based iron-manganese alloy particles, magnesium-based magnesium-nickel alloy particles, rare earth-based alloy particles, zeolite particles, silica particles, carbon nanotubes, graphite, aluminum phosphate molecular sieve particles, or mesoporous silica particles. Relative to 100 parts by weight of the encapsulation resin, the bright spot inhibitor may be included in an amount of 1 to 150 parts by weight, 1.5 to 100 parts by weight, 2 to 80 parts by weight, 2.5 to 50 parts by weight, 3 to 40 parts by weight, 3.5 to 20 parts by weight, 4 to 10 parts by weight, or 4.5 to 8 parts by weight. The present application can achieve bright spot prevention of organic electronic devices while improving the adhesion and durability of the film within the above content range. In addition, the particle size of the bright spot inhibitor may be in the range of 10nm to 30μm, 50nm to 21μm, 105nm to 18μm, 110nm to 12μm, 120nm to 9μm, 140nm to 4μm, 150nm to 2μm, 180nm to 900nm, 230nm to 700nm, or 270nm to 550nm. The particle size can be analyzed according to the D50 particle size. By including the bright spot inhibitor, the present application can achieve moisture barrier properties and durable reliability of the encapsulation film while effectively adsorbing hydrogen generated in the organic electronic device. In the present specification, the term resin component may be an encapsulation resin and / or a binder resin described below.
[0029] In one embodiment, when the surface or cross section of the encapsulation layer in the present application is determined by a backscattered electron image at an acceleration voltage of 15 kV by SEM, the hygroscopic agent and the bright spot inhibitor with a particle size of 100 nm to 20 μm can be within the range of 10% or more, 15% or more, or 20% or more of the area of the entire surface or cross section. The upper limit can be 95% or less, 80% or less, 70% or less, or 50% or less. In addition, when the surface or cross section of the encapsulation layer in the present application is determined by a backscattered electron image at an acceleration voltage of 15 kV by SEM, the area occupied by the bright spot inhibitor can be smaller than the area occupied by the hygroscopic agent. By adjusting the area ratio of the backscattered electron image, the present application can not only achieve a moisture barrier effect and a bright spot prevention effect, but also allow light to fully reach the resin matrix during UV curing, thereby achieving curing characteristics and durable reliability under high temperature and high humidity. The area ratio can be adjusted according to the cumulative particle size distribution, particle size or particle size ratio of the aforementioned hygroscopic agent and bright spot inhibitor.
[0030] In one example, the encapsulation layer of the present application may have a multilayer structure including at least two or more encapsulation layers as a single layer. In the case of including two or more encapsulation layers, the encapsulation layer may include a first layer facing the element when encapsulating the organic electronic element, and a second layer located on a surface opposite to the surface of the first layer facing the element. Figure 1 As shown in (a), the encapsulation film includes at least two or more encapsulation layers, wherein the encapsulation layer may include a first layer 2 facing the organic electronic element during encapsulation and a second layer 4 not facing the organic electronic element. In addition, the second layer 4 may contain a bright spot inhibitor 3, the adsorption energy of the bright spot inhibitor 3 for exhaust gas as calculated by the approximate method of density functional theory is 0 eV or less. In addition, the encapsulation film of the present application contains a bright spot inhibitor in the second layer located on the surface opposite to the element attachment surface of the first layer facing the organic electronic element during encapsulation, so that damage to the organic electronic element due to stress concentration caused by the bright spot inhibitor can be prevented. From such a point of view, based on the mass of all bright spot inhibitors in the encapsulation film, the first layer may contain a bright spot inhibitor at 15% or less or may not contain a bright spot inhibitor. In addition, based on the mass of all bright spot inhibitors in the encapsulation film, the layer other than the first layer that does not contact the organic electronic element may contain 85% or more of the bright spot inhibitor. That is, in the present application, when encapsulating the element, the other encapsulation layers that do not contact the organic electronic element can contain a larger amount of bright spot inhibitor compared to the first layer facing the organic electronic element, thereby preventing physical damage to the element while achieving the moisture barrier properties and bright spot prevention properties of the film.
[0031] As described above, the encapsulation layer may have a multilayer structure of two or more layers. When two or more layers constitute the encapsulation layer, the composition of each layer in the encapsulation layer may be the same or different. In one example, the encapsulation layer may include an encapsulation resin and / or a moisture absorbent, and the encapsulation layer may be a pressure-sensitive adhesive layer or an adhesive layer.
[0032] like Figure 1 As shown, the encapsulation layers 2, 4 may include a first layer 2 and a second layer 4, and the second layer 4 of the encapsulation layer may include a bright spot inhibitor 3. In addition, as shown Figure 1 As shown in (b), the second layer may contain both a bright spot inhibitor 3 and a desiccant 5. In addition, without limitation to the above, the encapsulation layer may be formed into a three-layer structure. In the encapsulation film of the present application, when the encapsulation layer has a three-layer structure, at least one encapsulation layer may contain a bright spot inhibitor and / or a desiccant. For example, the bright spot inhibitor and the desiccant may also be contained in one encapsulation layer at the same time or may each exist in a separate encapsulation layer. However, when the encapsulation film is applied to an organic electronic component, the first layer 2 as the encapsulation layer facing the organic electronic component may not contain a bright spot inhibitor and a desiccant, or even if it contains a bright spot inhibitor and a desiccant, it may only contain a small amount.
[0033] In one embodiment of the present invention, the encapsulation layer may include an encapsulation resin, and the encapsulation resin may be a curable resin or a cross-linkable resin. The glass transition temperature of the encapsulation resin may be less than 0°C, less than -10°C, or less than -30°C, less than -50°C, or less than -60°C. The lower limit is not particularly limited, and it may be -150°C or higher. Here, the glass transition temperature may be the glass transition temperature after curing, and in one embodiment, it may mean the glass transition temperature after curing with an irradiation level of about 1 J / cm 2 The glass transition temperature after the encapsulation resin is irradiated with ultraviolet rays of 1000 nm or greater; or the glass transition temperature after ultraviolet irradiation and further thermal curing.
[0034] In one example, the encapsulation resin may include styrene resin or elastomer, polyolefin resin or elastomer, other elastomers, polyoxyalkylene resin or elastomer, polyester resin or elastomer, polyvinyl chloride resin or elastomer, polycarbonate resin or elastomer, polyphenylene sulfide resin or elastomer, a mixture of hydrocarbons, polyamide resin or elastomer, acrylate resin or elastomer, epoxy resin or elastomer, silicone resin or elastomer, fluororesin or elastomer, or a mixture thereof, etc.
[0035] Here, as styrene resin or elastomer, for example, styrene-ethylene-butadiene-styrene block copolymer (SEBS), styrene-isoprene-styrene block copolymer (SIS), acrylonitrile-butadiene-styrene block copolymer (ABS), acrylonitrile-styrene-acrylate block copolymer (ASA), styrene-butadiene-styrene block copolymer (SBS), styrene homopolymer, or a mixture thereof can be exemplified. As olefin resin or elastomer, for example, high-density polyethylene resin or elastomer, low-density polyethylene resin or elastomer, polypropylene resin or elastomer, or a mixture thereof can be exemplified. As elastomer, for example, ester thermoplastic elastomer, olefin elastomer, silicone elastomer, acrylic elastomer, or a mixture thereof can be used. In particular, as olefin thermoplastic elastomer, polybutadiene resin or elastomer or polyisobutylene resin or elastomer can be used. As polyoxyalkylene resin or elastomer, for example, polyoxymethylene resin or elastomer, polyethylene oxide resin or elastomer, or a mixture thereof can be exemplified. As polyester resins or elastomers, for example, polyethylene terephthalate resins or elastomers, polybutylene terephthalate resins or elastomers, or mixtures thereof, etc. can be exemplified. As polyvinyl chloride resins or elastomers, for example, polyvinylidene chloride, etc. can be exemplified. As mixtures of hydrocarbons, for example, hexatriacontane or paraffin, etc. can be exemplified. As polyamide resins or elastomers, for example, nylon, etc. can be exemplified. As acrylate resins or elastomers, for example, polybutyl (meth)acrylate, etc. can be exemplified. As the epoxy resin or elastomer, for example, there can be exemplified bisphenol type, such as bisphenol A type, bisphenol F type, bisphenol S type and hydrogenated products thereof; novolac type, such as phenol novolac type or cresol novolac type; nitrogen-containing ring type, such as triglycidyl isocyanurate type or hydantoin type; alicyclic type; aliphatic type; aromatic type, such as naphthalene type and biphenyl type; glycidyl type, such as glycidyl ether type, glycidyl amine type and glycidyl ester type; dicyclic type, such as dicyclopentadiene type; ester type; ether ester type; or a mixture thereof; etc. As the silicone resin or elastomer, for example, there can be exemplified polydimethylsiloxane and the like. Examples of the fluororesin or elastomer include polytrifluoroethylene resin or elastomer, polytetrafluoroethylene resin or elastomer, polychlorotrifluoroethylene resin or elastomer, polyhexafluoropropylene resin or elastomer, polyvinylidene fluoride, polyvinyl fluoride, polyethylene fluoride, or mixtures thereof.
[0036] The resins or elastomers listed above can also be used, for example, by grafting with maleic anhydride or the like, by copolymerizing with other resins or elastomers via monomers used to produce the resins or elastomers, and by modification with other compounds. Examples of the above other compounds can include carboxyl-terminated butadiene-acrylonitrile copolymers, and the like.
[0037] In one example, the encapsulation layer may include, but is not limited to, olefin elastomers, silicone elastomers, acrylic elastomers, etc. among the above types as the encapsulation resin.
[0038] In one embodiment of the present invention, the encapsulating resin may be an olefin-based resin. In one example, the olefin-based resin may be a homopolymer of a butene monomer; a copolymer obtained by copolymerizing a butene monomer with another polymerizable monomer; a reactive oligomer using a butene monomer; or a mixture thereof. The butene monomer may include, for example, 1-butene, 2-butene, or isobutylene.
[0039] Other monomers polymerizable with the butene monomer or derivative may include, for example, isoprene, styrene, or butadiene, etc. By using a copolymer, physical properties such as processability and crosslinking degree can be maintained, and thus heat resistance of the adhesive itself can be ensured when applied to an organic electronic device.
[0040] In addition, the reactive oligomer using butene monomer can include butene polymers with reactive functional groups. The weight average molecular weight of the oligomer can be in the range of 500 to 5000. In addition, butene polymers can be combined with other polymers with reactive functional groups. Other polymers can be but are not limited to (meth) alkyl acrylates. The reactive functional group can be hydroxyl, carboxyl, isocyanate or nitrogen-containing groups. In addition, reactive oligomers and other polymers can be cross-linked by a multifunctional crosslinking agent, and the multifunctional crosslinking agent can be selected from at least one of isocyanate crosslinking agents, epoxide crosslinking agents, aziridine crosslinking agents and metal chelate crosslinking agents.
[0041] In one example, the encapsulation resin of the present application can be a copolymer of a diene and an olefinic compound containing a carbon-carbon double bond. Here, the olefinic compound can include butene, etc., and the diene can be a monomer that can be polymerized with the olefinic compound, and can include, for example, isoprene or butadiene, etc. For example, the copolymer of an olefinic compound containing a carbon-carbon double bond and a diene can be butyl rubber.
[0042] In the encapsulation layer, the resin or elastomer component can have a weight average molecular weight (Mw) reaching the degree that the pressure-sensitive adhesive composition can be formed into a film shape. For example, the weight average molecular weight of the resin or elastomer can be about 100,000g / mol to 2,000,000g / mol, 120,000g / mol to 1,500,000g / mol or 150,000g / mol to 1,000,000g / mol or so. In this specification, the term weight average molecular weight means the value of being converted into standard polystyrene measured by GPC (gel permeation chromatography). However, resin or elastomer do not necessarily have the above-mentioned weight average molecular weight. For example, in the case where the molecular weight of the resin or elastomer component is not at a level sufficient to form a film, a separate binder resin can be blended into the pressure-sensitive adhesive composition.
[0043] In another embodiment, the encapsulation resin according to the present application may be a curable resin. When the encapsulation resin is a curable resin, the encapsulation resin may be a resin having a glass transition temperature of 85°C or higher and 200°C or lower after curing. The glass transition temperature may be the glass transition temperature after photocuring or thermally curing the encapsulation resin. The specific types of curable resins available in the present invention are not particularly limited, and for example, various thermosetting resins or photocurable resins known in the art may be used. The term "thermosetting resin" means a resin that can be cured by appropriate heat application or aging process, and the term "photocurable resin" means a resin that can be cured by irradiation with electromagnetic waves. In addition, the curable resin may be a dual-curing resin including both thermal curing properties and photocuring properties.
[0044] The specific type of curable resin in the present application is not particularly limited, as long as it has the above-mentioned characteristics. For example, the curable resin can be cured to show adhesive properties, which may include such a resin: the resin contains one or more thermosetting functional groups (such as glycidyl, isocyanate, hydroxyl, carboxyl or amide) or contains one or more functional groups that can be cured by irradiation with electromagnetic waves (such as epoxy, cyclic ether, sulfide, acetal or lactone). Specific examples of such resins may include acrylic resins, polyester resins, isocyanate resins or epoxy resins, etc., but are not limited thereto.
[0045] In the present application, as curable resin, aromatic or aliphatic, or linear or branched epoxy resin can be used. In one embodiment of the present invention, an epoxy resin having an epoxy equivalent of 180g / equivalent to 1,000g / equivalent containing two or more functional groups can be used. By using an epoxy resin with an epoxy equivalent in the above range, characteristics such as the adhesive properties and glass transition temperature of the cured product can be effectively maintained. Examples of such epoxy resins can include a mixture of one or two or more of the following: cresol novolac epoxy resin, bisphenol A type epoxy resin, bisphenol A type novolac epoxy resin, phenol novolac epoxy resin, tetrafunctional epoxy resin, biphenyl type epoxy resin, trisphenol methane type epoxy resin, alkyl-modified trisphenol methane epoxy resin, naphthalene type epoxy resin, dicyclopentadiene type epoxy resin or dicyclopentadiene modified phenol type epoxy resin.
[0046] In the present application, as curable resin, epoxy resin containing cyclic structure in molecular structure can be used, and epoxy resin containing aromatic group (for example, phenyl) can be used.When epoxy resin contains aromatic group, cured product has excellent thermal stability and chemical stability, and shows low moisture absorption at the same time, so that the reliability of organic electronic device packaging structure can be improved.The specific example of epoxy resin containing aromatic group that can be used in the present invention can be one of the following or a mixture of two or more: biphenyl type epoxy resin, dicyclopentadiene type epoxy resin, naphthalene type epoxy resin, dicyclopentadiene modified phenol type epoxy resin, epoxy resin based on cresol, epoxy resin based on bisphenol, epoxy resin based on xylene, multifunctional epoxy resin, phenol novolac epoxy resin, trisphenol methane type epoxy resin and alkyl modified trisphenol methane epoxy resin etc., but not limited thereto.
[0047] In addition, in one example, the encapsulation layer of the present application may include an active energy ray-polymerizable compound that is highly compatible with the encapsulation resin and can form a specific crosslinked structure with the encapsulation resin. In this case, the encapsulation resin may be a crosslinkable resin.
[0048] For example, the encapsulation layer of the present application may contain a multifunctional or monofunctional active energy ray polymerizable compound that can be polymerized together with the encapsulation resin by irradiating active energy rays. The active energy ray polymerizable compound may refer to a compound that contains two or more functional groups that can participate in a polymerization reaction by irradiating active energy rays, such as a functional group containing an ethylenically unsaturated double bond (e.g., an acryloyl group or a methacryloyl group) or a functional group such as an epoxy group or an oxetane group.
[0049] As the multifunctional active energy ray-polymerizable compound, for example, multifunctional acrylate (MFA) can be used.
[0050] In addition, the multifunctional active energy ray polymerizable compound may be contained in an amount of 3 to 30 parts by weight, 5 to 25 parts by weight, 8 to 20 parts by weight, 10 to 18 parts by weight, or 12 to 18 parts by weight relative to 100 parts by weight of the encapsulation resin. In the case of a monofunctional active energy ray polymerizable compound, it may also be contained alone in the above content range. The present application provides an encapsulation film having excellent durable reliability even under harsh conditions such as high temperature and high humidity within the above range.
[0051] A multifunctional active energy ray polymerizable compound that can be polymerized by irradiating active energy rays can be used without any limitation. For example, the compound may include 1,4-butanediol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,8-octanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, dicyclopentyl di(meth)acrylate, cyclohexane-1,4-diol di(meth)acrylate, tricyclodecane dimethanol (meth)diacrylate, dimethylol dicyclopentane di(meth)acrylate, neopentyl glycol-modified trimethylolpropane di(meth)acrylate, adamantane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, or a mixture thereof.
[0052] As a multifunctional active energy ray polymerizable compound, for example, a compound having a molecular weight of 100 g / mol or more and less than 1,000 g / mol and containing two or more functional groups can be used. As a monofunctional active energy ray polymerizable compound, for example, a compound having a molecular weight of 100 g / mol or more and less than 1,000 g / mol and containing one functional group can be used. In this case, the molecular weight may mean a weight average molecular weight (GPC measurement) or a typical molecular weight. The ring structure contained in the multifunctional active energy ray polymerizable compound may be a carbocyclic structure or a heterocyclic structure, or a monocyclic structure or a polycyclic structure.
[0053] In one embodiment of the present application, the encapsulation layer may further include a free radical initiator. The free radical initiator may be a photoinitiator or a thermal initiator. The specific type of the photoinitiator may be appropriately selected in consideration of the curing rate and the possibility of yellowing. For example, a benzoin-based photoinitiator, a hydroxyketone-based photoinitiator, an aminoketone-based photoinitiator, or a phosphine oxide-based photoinitiator may be used, and specifically, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propane-1-one, 4-(2-hydroxy 1-[4-(1-methylvinyl)phenyl]propanone], 2-[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone], 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, and the like.
[0054] The free radical initiator may be included in a ratio of 0.2 to 20 parts by weight, 0.5 to 18 parts by weight, 1 to 15 parts by weight, or 2 to 13 parts by weight relative to 100 parts by weight of the active energy ray polymerizable compound. Therefore, the reaction of the active energy ray polymerizable compound can be effectively induced and the degradation of the physical properties of the encapsulation layer composition due to the residual components after curing can also be prevented.
[0055] In a specific example of the present application, the encapsulation layer of the encapsulation film may further include a curing agent, depending on the type of resin component included. For example, it may further include a curing agent capable of reacting with the above-mentioned encapsulation resin to form a cross-linked structure, etc. In this specification, the term encapsulation resin and / or binder resin may be used with the same meaning as the resin component.
[0056] The kind of the curing agent may be appropriately selected and used according to the resin component or the type of functional group contained in the resin.
[0057] In one example, when the resin component is an epoxy resin, the curing agent is a curing agent for epoxy resin known in the art, and for example, one or two or more of the following can be used: an amine curing agent, an imidazole curing agent, a phenol curing agent, a phosphorus curing agent or an anhydride curing agent, etc., but not limited thereto.
[0058] In one example, as a curing agent, an imidazole compound which is solid at room temperature and has a melting point or decomposition temperature of 80° C. or higher can be used. As such a compound, for example, 2-methylimidazole, 2-heptadecylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, or 1-cyanoethyl-2-phenylimidazole can be exemplified, but it is not limited thereto.
[0059] The content of the curing agent can be selected according to the composition of the composition (e.g., the type or ratio of the encapsulating resin). For example, relative to 100 parts by weight of the resin component, the curing agent can be included in an amount of 1 to 20 parts by weight, 1 to 10 parts by weight, or 1 to 5 parts by weight. However, the weight ratio can be changed according to the type and ratio of the functional groups of the encapsulating resin or the resin, or the crosslinking density to be achieved, etc.
[0060] When the resin component is a resin that can be cured by irradiation with active energy rays, for example, a cationic photopolymerization initiator can be used as the initiator.
[0061] As the cationic photopolymerization initiator, As an ionizing cationic initiator of a salt, an organic metal salt series, or a non-ionizing cationic photopolymerization initiator of an organic silane or latent sulfonic acid series. The salt-based initiator can be exemplified by diaryliodonium Salt, triaryl Examples of the initiator of the organic metal salt series include iron arenes, examples of the initiator of the organic silane series include o-nitrobenzyl triarylsilyl ether, triarylsilyl peroxide or acyl silane, and examples of the initiator of the latent sulfonic acid series include α-sulfonyloxy ketone or α-hydroxymethyl benzoin sulfonate, but are not limited thereto.
[0062] In one example, as the cationic initiator, an ionizing cationic photopolymerization initiator may be used.
[0063] In one example, the encapsulation layer may also include a tackifier, wherein the tackifier may preferably be a hydrogenated cycloolefin polymer. As a tackifier, for example, a hydrogenated petroleum resin obtained by hydrogenating a petroleum resin may be used. The hydrogenated petroleum resin may be partially or completely hydrogenated, and may also be a mixture of such resins. Such a tackifier may be selected to have good compatibility with the pressure-sensitive adhesive composition, excellent moisture barrier properties, and low organic volatile components. Specific examples of hydrogenated petroleum resins may include hydrogenated terpene resins, hydrogenated ester resins, or hydrogenated dicyclopentadiene resins, etc. The weight average molecular weight of the tackifier may be about 200 g / mol to 5,000 g / mol. The content of the tackifier may be appropriately adjusted as needed. For example, according to one example, relative to 100 parts by weight of the encapsulation resin, the content of the tackifier may be included in a ratio of 5 parts by weight to 100 parts by weight, 8 parts by weight to 95 parts by weight, 10 parts by weight to 93 parts by weight, or 15 parts by weight to 90 parts by weight.
[0064] If necessary, the encapsulation layer may also include a moisture blocker. In this specification, the term "moisture blocker" may refer to a material that is not reactive with moisture or has low reactivity with moisture, but can physically block or hinder the movement of moisture or humidity in the film. As a moisture blocker, for example, one or two or more of the following may be used: clay, talc, spherical silica, needle-shaped silica, flaky silica, porous silica, zeolite, titanium dioxide or zirconium oxide. In addition, the moisture blocker may be surface treated with an organic modifier to promote the penetration of organic substances. As such an organic modifier, for example, dimethylbenzyl hydrogenated tallow quaternary ammonium, dimethyl hydrogenated tallow quaternary ammonium, methyl tallow bis-2-hydroxyethyl quaternary ammonium, dimethyl hydrogenated tallow 2-ethylhexyl quaternary ammonium, dimethyl dehydrogenated tallow quaternary ammonium, or a mixture thereof may be used.
[0065] The content of the water blocking agent is not particularly limited and may be appropriately selected in consideration of desired barrier properties.
[0066] In addition to the above-mentioned constitution, the encapsulation layer may further include various additives according to the application and manufacturing process of the encapsulation film described below. For example, according to the expected physical properties, the encapsulation layer may include a curable material, a crosslinking agent, a filler, etc. in an appropriate content range.
[0067] When the encapsulation layer is formed of two or more layers, the second layer that does not contact the organic electronic element may contain a hygroscopic agent. For example, when the encapsulation layer is formed of two or more layers, the layer in contact with the organic electronic element in the encapsulation layer may not contain a hygroscopic agent, or contain a hygroscopic agent in a small amount of less than 5 parts by weight or less than 4 parts by weight relative to 100 parts by weight of the encapsulation resin.
[0068] Specifically, considering that the encapsulation film is applied to the encapsulation of organic electronic components, the content of the hygroscopic agent can be controlled in consideration of damage to the components. For example, the first layer facing the component during encapsulation may contain a small amount of hygroscopic agent, or may not contain a hygroscopic agent. In one example, the first layer of the encapsulation layer facing the component during encapsulation may contain 0% to 20% of hygroscopic agent relative to the total mass of the hygroscopic agent contained in the encapsulation film. In addition, the encapsulation layer that does not contact the component may contain 80% to 100% of hygroscopic agent relative to the total mass of the hygroscopic agent contained in the encapsulation film.
[0069] In a specific example of the present application, the encapsulation film may further include a metal layer formed on one side of the encapsulation layer. The thermal conductivity of the metal layer of the present application may be 15 W / m·K or greater, 18 W / m·K or greater, 20 W / m·K or greater, 25 W / m·K or greater, 30 W / m·K or greater, 40 W / m K or greater, 50 W / m K or greater, 60 W / m K or greater, 70 W / m K or greater, 80 W / m K or greater, 90 W / m K or greater, 100 W / m K or greater, 110 W / m·K or greater, 120 W / m·K or greater, 130 W / m·K or greater, 140 W / m·K or greater, 150 W / m·K or greater, 200 W / m·K or greater, or 210 W / m·K or greater. The upper limit of thermal conductivity is not particularly limited, and it may be 800 W / m·K or less. By having such a high thermal conductivity, the heat generated at the bonding interface during the metal layer bonding process can be released more quickly. In addition, the heat accumulated during the operation of the organic electronic device is quickly released due to the high thermal conductivity, so that the temperature of the organic electronic device itself can be kept low and the occurrence of cracks and defects is reduced. The thermal conductivity can be measured at any temperature within the temperature range of 15°C to 30°C.
[0070] The term "thermal conductivity" herein refers to the degree to which a material is able to transfer heat by conduction, wherein the unit may be expressed by W / m·K. This unit indicates the degree to which a material transfers heat at the same temperature and distance, which means a heat unit (Watt) relative to a distance unit (meter) and a temperature unit (Kelvin).
[0071] In one embodiment of the present application, the metal layer of the encapsulation film can be transparent and opaque. The thickness of the metal layer can be in the range of 3 μm to 200 μm, 10 μm to 100 μm, 20 μm to 90 μm, 30 μm to 80 μm, or 40 μm to 75 μm. The present application can provide a thin film encapsulation film while achieving sufficient heat release effect by controlling the thickness of the metal layer. The metal layer can be a thin metal foil or a polymer base layer deposited with a metal. The metal layer is not particularly limited as long as it is a material that satisfies the above-mentioned thermal conductivity and contains a metal. The metal layer may include any one of metals, metal oxides, metal nitrides, metal carbides, metal oxynitrides, metal boron oxides, and combinations thereof. For example, the metal layer may include an alloy in which one or more metal elements or non-metallic elements are added to one of the metals, and may include, for example, stainless steel (SUS). In addition, in one example, the metal layer can include iron, chromium, copper, aluminum, nickel, iron oxide, chromium oxide, silicon oxide, aluminum oxide, titanium oxide, indium oxide, tin oxide, indium tin oxide, tantalum oxide, zirconium oxide, niobium oxide and combinations thereof. The metal layer can be deposited by electrolysis, rolling, thermal evaporation, electron beam evaporation, sputtering, reactive sputtering, chemical vapor deposition, plasma chemical vapor deposition or electron cyclotron resonance source plasma chemical vapor deposition. In one example of the present application, the metal layer can be deposited by reactive sputtering.
[0072] Conventionally, nickel-iron alloy (Invar alloy) is generally used as an encapsulation film, but nickel-iron alloy has the disadvantages of being expensive, having low thermal conductivity and having poor cutting characteristics. The present application provides an encapsulation film that prevents the generation of bright spots in an organic electronic device, has excellent heat release characteristics and realizes processing convenience due to magnetism without using nickel-iron alloy as a metal layer.
[0073] The encapsulation film may further include a base film or a release film (hereinafter, may be referred to as a "first film"), and the encapsulation film may have a structure in which an encapsulation layer is formed on the base film or the release film. In addition, the structure may further include a base film or a release film (hereinafter, may be referred to as a "second film") formed on the metal layer.
[0074] The specific type of the first film that can be used in the present application is not particularly limited. In the present application, for example, a general polymer film in the art can be used as the first film. In the present application, for example, as a base film or a release film, a polyethylene terephthalate film, a polytetrafluoroethylene film, a polyethylene film, a polypropylene film, a polybutylene film, a polybutadiene film, a polyvinyl chloride film, a polyurethane film, an ethylene-vinyl acetate film, an ethylene-propylene copolymer film, an ethylene-ethyl acrylate copolymer film, an ethylene-methyl acrylate copolymer film or a polyimide film etc. can be used. In addition, a suitable demoulding process can be carried out on one or both sides of the base film or the release film of the present application. As an example of a release agent in the demoulding process for the base film, an alkyd series, a silicone series, a fluorine series, an unsaturated ester series, a polyolefin series or a wax series etc. can be used, wherein, in terms of heat resistance, a release agent of an alkyd series, a silicone series or a fluorine series is preferably used, but is not limited thereto.
[0075] In the present application, the thickness of the base film or release film (first film) as above is not particularly limited, and it can be appropriately selected according to the application to which the base film or release film is applied. For example, in the present application, the thickness of the first film can be 10 μm to 500 μm, preferably about 20 μm to 200 μm. If the thickness is less than 10 μm, deformation of the base film may easily occur during the manufacturing process, and if the thickness exceeds 500 μm, the economic benefit is low.
[0076] The thickness of the encapsulation layer included in the encapsulation film of the present application is not particularly limited, and it can be appropriately selected according to the following conditions in consideration of the application to which the film is applied. The thickness of the encapsulation layer can be 5 μm to 200 μm, preferably about 5 μm to 100 μm. The thickness of the encapsulation layer can be the entire thickness of the multi-layer encapsulation layer. If the thickness of the encapsulation layer is less than 5 μm, it may not be able to exhibit sufficient moisture barrier capability, and if it exceeds 200 μm, it is difficult to ensure processability, and the thickness expansion caused by moisture reactivity is large, so that the deposited film of the organic light-emitting element may be damaged, and the economic benefit is low.
[0077] The present application also relates to organic electronic devices. Figure 2As shown in , the organic electronic device may include a substrate 21; an organic electronic element 22 formed on the substrate 21; and the above-mentioned encapsulation film for encapsulating the organic electronic element 22. The encapsulation film can encapsulate the entire surface of the organic electronic element formed on the substrate, such as the entire upper part and the side. The encapsulation film may include an encapsulation layer containing a pressure-sensitive adhesive composition or an adhesive composition in a cross-linked or cured state. In addition, the organic electronic device can be formed by sealing the encapsulation layer to contact the entire surface of the organic electronic element formed on the substrate. A covering substrate 13 may be formed on the encapsulation layer 12. The covering substrate 13 may be glass, a plastic film, or the aforementioned metal layer. In one example, the covering substrate 13 may be integrally included with the encapsulation layer 12 to form an encapsulation film. In one example, the encapsulation film of the present application may be a film having a multilayer structure integrally including an encapsulation layer 12 and a metal layer 13.
[0078] In one embodiment of the present application, the organic electronic element may include a pair of electrodes, an organic layer including at least a light-emitting layer, and a passivation film. Specifically, the organic electronic element may include a first electrode layer, an organic layer formed on the first electrode layer and including at least a light-emitting layer, and a second electrode layer formed on the organic layer, and may include a passivation film for protecting the electrodes on the organic layer and the second electrode layer. The first electrode layer may be a transparent electrode layer or a reflective electrode layer, and the second electrode layer may also be a transparent electrode layer or a reflective electrode layer. More specifically, the organic electronic element may include a transparent electrode layer formed on a substrate, an organic layer formed on the transparent electrode layer and including at least a light-emitting layer, and a reflective electrode layer formed on the organic layer.
[0079] Here, the organic electronic element may be, for example, an organic light emitting element.
[0080] The passivation film may include an inorganic film and an organic film. In one embodiment, the inorganic film may be a metal oxide or nitride selected from one or more of Al, Zr, Ti, Hf, Ta, In, Sn, Zn and Si. The thickness of the inorganic film may be 0.01 μm to 50 μm, or 0.1 μm to 20 μm, or 1 μm to 10 μm. In an example, the inorganic film of the present application may be an inorganic material not comprising a dopant, or may be an inorganic material comprising a dopant. The dopant that may be doped may be one or more elements selected from Ga, Si, Ge, Al, Sn, Ge, B, In, Tl, Sc, V, Cr, Mn, Fe, Co and Ni, or an oxide of the element, but is not limited thereto. The difference between an organic film and an organic layer comprising at least a light-emitting layer is that it does not include a light-emitting layer, and may be an organic deposition layer comprising an epoxy compound.
[0081] The inorganic film or the organic film may be formed by chemical vapor deposition (CVD). For example, as the inorganic film, silicon nitride (SiNx) may be used. In one example, silicon nitride (SiNx) used as an inorganic film may be deposited to a thickness of 0.01 μm to 50 μm. In one example, the thickness of the organic film may be in the range of 2 μm to 20 μm, 2.5 μm to 15 μm, or 2.8 μm to 9 μm.
[0082] The present application also provides a method for manufacturing an organic electronic device. The manufacturing method may include the step of applying the above-mentioned encapsulation film to a substrate on which an organic electronic element is formed to cover the organic electronic element. In addition, the manufacturing method may include the step of curing the encapsulation film. The curing step of the encapsulation film may refer to the curing of the encapsulation layer, which may be performed before or after the encapsulation film covers the organic electronic element.
[0083] In the present specification, the term "curing" may mean that the pressure-sensitive adhesive composition of the present invention forms a cross-linked structure by heating or UV irradiation process, etc., thereby being produced in the form of a pressure-sensitive adhesive. Alternatively, it may mean that the adhesive composition is cured and attached as an adhesive.
[0084] Specifically, the organic electronic element can be formed by forming a transparent electrode on a glass or polymer film used as a substrate by a method such as vacuum evaporation or sputtering, forming a light-emitting organic material layer composed of, for example, a hole transport layer, a light-emitting layer, and an electron transport layer on the transparent electrode, and then further forming an electrode layer on the light-emitting organic material layer. Subsequently, an encapsulation layer of an encapsulation film is placed to cover the entire surface of the organic electronic element of the substrate subjected to the above process.
[0085] Beneficial Effects
[0086] The encapsulation film of the present application can be applied to seal or encapsulate organic electronic devices such as OLEDs. The film allows the formation of a structure capable of blocking moisture or oxygen from being introduced into the organic electronic device from the outside, and can prevent the organic electronic device from having bright spots. BRIEF DESCRIPTION OF THE DRAWINGS
[0087] Figure 1 is a cross-sectional view showing a packaging film according to one example of the present application.
[0088] Figure 2 is a cross-sectional view showing an organic electronic device according to one example of the present application.
[0089] [Explanation of Reference Numerals]
[0090] 1: Encapsulation film
[0091] 2, 4: Encapsulation layer
[0092] 3: Bright spot inhibitor
[0093] 5: Desiccant
[0094] 21: Base
[0095] 22: Organic electronic components
[0096] 12: Encapsulation layer
[0097] 13: Metal layer DETAILED DESCRIPTION
[0098] Hereinafter, the present invention will be described in more detail through Examples according to the present invention and Comparative Examples not according to the present invention, but the scope of the present invention is not limited by the following Examples.
[0099] Example 1
[0100] Production of encapsulation layer
[0101] In order to prepare the first layer solution, 250 kg of butyl rubber resin (BR268, EXXON, solid content 20%) dissolved in toluene and 50 kg of dicyclopentadiene hydrogenated resin (SU525, Kolon, solid content 70%) dissolved in toluene were homogenized. 15 kg of multifunctional acrylate (trimethylolpropane triacrylate, Miwon, solid content 50%) dissolved in toluene and 5 kg of photoinitiator (Irgacure651, Ciba, solid content 20%) dissolved in toluene were introduced into the homogenized solution, and 15 kg of 2-(2-ethoxyethoxy)ethyl acrylate and 137 kg of toluene as another solvent were introduced therein, homogenized, and then stirred at high speed for 1 hour to prepare the first layer solution.
[0102] In order to prepare the second layer solution, 265 kg of butyl rubber resin (BR268, EXXON, solid content 20%) dissolved in toluene and 67 kg of dicyclopentadiene hydrogenated resin (SU525, Kolon, solid content 70%) dissolved in toluene, and 3 kg of nickel (average particle size 500 nm) as a bright spot inhibitor were homogenized. 16 kg of multifunctional acrylate (trimethylolpropane triacrylate, Miwon, solid content 50%) dissolved in toluene and 8 kg of photoinitiator (Irgacure651, Ciba, solid content 20%) dissolved in toluene were introduced into the homogenized solution, and 288 kg of calcium oxide (CaO, raw material average particle size 2 μm) solution (solid content 50%) dispersed in toluene was introduced therein. 66 kg of toluene was introduced into the solution, homogenized, and then stirred at high speed for 1 hour to prepare the second layer solution.
[0103] After filtering the encapsulation layer solution prepared above through a 400-mesh nylon filter, the first layer (thickness 10 μm) and the second layer (thickness 50 μm) were each applied to the release surface of the release PET using a lip coater, dried in a dryer at 110° C. for 2 minutes and 4 minutes, respectively, and irradiated with ultraviolet light at 0.8 J / cm 2 and 2J / cm 2 Irradiation is performed to form an encapsulation layer, and then the two layers are laminated. The thickness means the thickness after drying is completed.
[0104] Production of packaging films
[0105] On the previously prepared metal layer (SUS430, thickness 80 μm), the release-treated PET of the second layer attached to the encapsulation layer was peeled off and laminated by a roll-to-roll process at 70° C., whereby an encapsulation film was produced such that the second layer was in contact with the metal layer.
[0106] The produced encapsulation film was cut into a size of 65 inches to produce a film for encapsulating an organic electronic element in a sheet state. Physical properties of the produced film were measured.
[0107] Example 2
[0108] A film for encapsulating an organic electronic element was produced in the same manner as in Example 1, except that the content of the CaO particles was changed to 290 kg.
[0109] Example 3
[0110] A film for encapsulating an organic electronic element was produced in the same manner as in Example 1, except that the average particle diameter of the CaO particles was changed to 2.5 μm.
[0111] Example 4
[0112] A film for encapsulating an organic electronic element was produced in the same manner as in Example 1, except that the average particle diameter of the CaO particles was changed to 1.5 μm.
[0113] Example 5
[0114] A film for encapsulating an organic electronic element was produced in the same manner as in Example 1, except that the average particle diameter of the Ni particles was changed to 600 nm.
[0115] Comparative Example 1
[0116] A film for encapsulating an organic electronic element was produced in the same manner as in Example 1, except that the average particle diameter of the CaO particles was changed to 6 μm.
[0117] Comparative Example 2
[0118] A film for encapsulating an organic electronic element was produced in the same manner as in Example 1, except that the average particle diameter of the Ni particles was changed to 2 μm.
[0119] Comparative Example 3
[0120] A film for encapsulating an organic electronic element was produced in the same manner as in Example 1, except that the content of the CaO particles was changed to 1 kg.
[0121] Experimental Example 1- Calculation of adsorption energy
[0122] The adsorption energy of the bright spot suppressors used in the embodiments and comparative examples to exhaust gas is calculated by electronic structure calculation based on density functional theory. After constructing a two-dimensional flat plate structure in which the densest packed surface of the bright spot suppressors having a crystal structure is exposed on the surface, and then performing structural optimization, and optimizing the structure in which the molecules causing bright spots are adsorbed on the surface in the vacuum state, the value obtained by subtracting the total energy of the molecules causing bright spots from the total energy difference of the two systems is defined as the adsorption energy. For the total energy calculation for each system, a modified PBE function as a function of the GGA (generalized gradient approximation) series is used as an exchange correlation to simulate the interaction between electrons and electrons, the electron kinetic energy cutoff used is 500eV, and only the gamma point corresponding to the origin of the reciprocal space is included and calculated. The conjugate gradient method is used to optimize the atomic structure of each system and iterative calculations are performed until the interatomic force is or less. A series of calculations were performed by VASP which is a commercially available code. The adsorption energies of Ni used as a bright spot suppressor in Examples and Comparative Examples for NH3 and H were -0.54 and -2.624, respectively.
[0123] Experimental Example 2 - Particle Size Distribution Results
[0124] For the encapsulation film produced in the embodiment, the encapsulation layer was cut into 1.5 cm × 1.5 cm, prepared into a sample, and then dissolved in 3 g of toluene (sonic treatment for 20 minutes, 50 ° C). After filtering it through a 300 mesh nylon filter, the particle size of the solution passing through the filter was measured. In the particle size measurement method, Mastersizer (Malvern Panalytical Ltd) was used as a device that applied technology certified by ISO 13320: 2009. In the setting of the software, the particle type was entered as non-spherical, the solvent was then entered as toluene, and the liquid level sensor threshold was entered as 20. Thereafter, the background measurement time and the sample measurement time were entered as 10 seconds and 5 seconds, respectively, and the lower and upper limits of the measurement obscuration were entered as 1% and 20%, respectively, and then the measurement was entered to be performed at least 3 times, thereby completing the setting. After introducing a toluene solvent into the device and circulating it at 2000RPM to 3000RPM, initialization and background value measurement are performed, and a filtered dispersion solution of a bright spot inhibitor and a moisture absorber is introduced therein, and the shielding rate value on the software screen is set to 3% to 7%, and then measurement is performed. During the measurement process, peaks that appear as irregular frequencies and signals in a region with a particle size of 30μm or more are determined as noise caused by dust, etc., and are removed, and then the result value is obtained.
[0125] The calculated value was calculated according to the following general formula 1. The unit of the average particle size is μm.
[0126] [General formula 1]
[0127]
[0128] [Table 1]
[0129] Dx(10) Dx(50) Dx(90) Dx(99) Formula 1 Example 1 0.7 2.04 4.12 5.62 2.93 Example 2 0.767 2.08 4.15 5.63 2.91 Example 3 0.991 2.79 6.6 10.7 3.19 Example 4 0.835 1.87 3.36 4.52 2.72 Example 5 0.942 2.87 5.47 7.53 3.18 Comparative Example 1 1.53 4.72 10.9 18 3.73 Comparative Example 2 2.77 9.24 16.2 30.4 4.66 Comparative Example 3 0.564 0.968 1.66 2.35 2.27
[0130] Experimental Example 3-Panel Defect Measurement
[0131] After depositing the organic electronic element on the thin film transistor glass substrate, the encapsulation films produced in the embodiment and the comparative example were each laminated to the element using a vacuum bonding machine at 25°C, a vacuum level of 50 mTorr and 0.4 MPa to have an effective bezel length of 3 mm to 4 mm, thereby manufacturing an organic electronic panel with a size of 65 inches. The effective bezel means the distance between the outside and the inside of the edge area where the encapsulation layer is in direct contact with the glass substrate when there is no organic electronic element on the edge of the glass substrate. After the manufactured panel was driven for 1000 hours at 85°C and 85% relative humidity, it was turned on in a dark room and it was determined with the naked eye whether a defective pixel appeared. For defective pixels, a bright spot brighter than the surrounding or a dark spot darker than the surrounding was determined as a defective pixel. In the case of 3 or fewer defective pixels, it was classified as O; in the case of less than 10 defective pixels, it was classified as Δ; when 10 or more defective pixels appeared, it was classified as X.
[0132] Experimental Example 4 - Moisture Barrier Length Measurement
[0133] As the moisture penetration length in the edge area of the panel for completing the measurement of Experimental Example 3, the distance between the outside and the inside of the area where the transparency increased was measured. Regarding the moisture absorbent, the area where moisture penetrated when the transparency increased due to the reaction with moisture and the area where moisture did not penetrate were divided by the boundary point of the transparency difference. When the moisture barrier distance was 2 mm or less, it was classified as O, and when the high temperature and high humidity durability reliability was poor due to the moisture barrier distance exceeding 2 mm, it was classified as X.
[0134] In the case of poor durability (degree of cure) when evaluated at high temperature and high humidity, the moisture barrier distance deteriorates. Therefore, the moisture barrier distance can be a measure of durability and hardening.
[0135] [Table 2]
[0136] Panel defects Moisture barrier properties Example 1 O O Example 2 O O Example 3 O O Example 4 O O Example 5 O O Comparative Example 1 O X Comparative Example 2 O X Comparative Example 3 O X
Claims
1. A packaging film, comprising a packaging layer, wherein the packaging layer comprises a moisture absorbent, a bright spot inhibitor and a packaging resin, Wherein, as a result of analyzing the particle sizes of the moisture absorbent and the bright spot inhibitor contained in a sample passed by dissolving the encapsulation layer in an organic solvent and then filtering it through a 300-mesh nylon filter, the value according to the following Formula 1 satisfies the range of 2.4 to 3.6: [General formula 1] in, D10 is the average particle size of D10 according to the particle size analysis result, D50 is the average particle size of D50 according to the particle size analysis result, and D90 is the average particle size of D90 according to the particle size analysis result, wherein the particle size analysis is the particle size distribution measured according to ISO13320:2009, According to the D50 particle size analysis, the ratio of the average particle size of the bright spot inhibitor to the average particle size of the moisture absorbent is 0.15 to 2.0, The particle size of the hygroscopic agent is in the range of 100 nm to 15000 nm. The particle size of the bright spot inhibitor is in the range of 10 nm to 30 μm. wherein the moisture absorbent is contained in the range of 5 parts by weight to 250 parts by weight relative to 100 parts by weight of the encapsulating resin, and The bright spot inhibitor is included in an amount of 1 part by weight to 150 parts by weight relative to 100 parts by weight of the encapsulating resin. 2 . The packaging film according to claim 1 , wherein a particle size of the moisture absorbent is in the range of 500 nm to 10000 nm. 3 . The packaging film according to claim 1 , wherein a particle size of the bright spot inhibitor is in a range of 50 nm to 21 μm. 4 . The packaging film according to claim 1 , wherein the bright spot suppressor has an adsorption energy to outgassing calculated by an approximate method of density functional theory of 0 eV or less.
5. The packaging film according to claim 4, wherein the exhaust gas comprises oxygen, H atoms, H 2 Molecule or NH 3 . The packaging film of claim 1 , wherein the moisture absorbent comprises a chemically reactive adsorbent. 7 . The encapsulation film according to claim 1 , wherein the bright spot inhibitor is included in an amount of 1.5 parts by weight to 100 parts by weight relative to 100 parts by weight of the encapsulation resin. 8 . The encapsulation film according to claim 1 , wherein the encapsulation resin is a curable resin or a cross-linkable resin. 9 . The encapsulation film of claim 1 , wherein the encapsulation layer further comprises an adhesion promoter. 10 . The encapsulation film according to claim 1 , wherein the encapsulation layer further comprises an active energy ray-polymerizable compound.
11. The packaging film according to claim 1, wherein when the surface or cross section of the packaging layer is determined by SEM with a backscattered electron image at an accelerating voltage of 15 kV, the moisture absorbent and the bright spot inhibitor having a particle size of 100 nm to 20 μm are within 10% or more of the area of the entire surface or cross section. 12 . The encapsulation film according to claim 1 , wherein when a surface or a cross section of the encapsulation layer is determined by a backscattered electron image by SEM at an accelerating voltage of 15 kV, an area occupied by the bright spot inhibitor is smaller than an area occupied by the moisture absorbent. 13 . The encapsulation film according to claim 1 , wherein the encapsulation layer encapsulates an entire surface of an organic electronic element formed on a substrate. 14 . The encapsulation film of claim 1 , further comprising a metal layer formed on one side of the encapsulation layer.
15. An organic electronic device, include: substrate; an organic electronic element formed on the substrate; and the encapsulation film according to claim 1 encapsulating the organic electronic element.
16. The organic electronic device according to claim 15, wherein the organic electronic element include: A pair of electrodes, an organic layer including at least a light-emitting layer, and a passivation film. 17 . A method for manufacturing an organic electronic device, comprising the step of applying the encapsulation film according to claim 1 to a substrate having an organic electronic element formed thereon to cover the organic electronic element.
Citation Information
Patent Citations
Configuration of random access channels for wireless communication