A bio-based flame-retardant polyurethane elastomer and preparation method thereof
By using tannic acid as a flame retardant and cross-linking agent in polyurethane elastomer, its flame retardant and mechanical properties are improved, and the problems of poor flame retardant performance of polyurethane elastomer and non-environmental protection of petroleum-based reactive flame retardants are solved. , realizing the preparation of high-performance, environmentally friendly bio-based flame-retardant polyurethane elastomer.
Patent Information
- Application Number
- CN202210362231.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-04-07
AI Technical Summary
Polyurethane elastomers have poor flame retardant properties and petroleum-based reactive flame retardants are not environmentally friendly, causing them to release toxic gases and smoke when burning, affecting human health and the environment.
Tannic acid is used as a reactive flame retardant and cross-linking agent, and a bio-based flame retardant polyurethane elastomer and its preparation method are designed through reversible cross-linking of hydroxyl groups and isocyanate groups to improve its flame retardancy and mechanical properties.
The flame retardant performance of polyurethane elastomer is improved and the mechanical properties are maintained. The use of non-toxic and easily degradable tannic acid simplifies the preparation process, expands the application fields of the material, and reduces environmental pollution.
Smart Images

Figure CN114573777B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of materials, and particularly relates to a bio-based flame-retardant polyurethane elastomer using tannic acid as a cross-linking agent and a preparation method thereof. Background Art
[0002] Polyurethane elastomer (PU) is a new type of polymer material with excellent properties, including high strength, high toughness, good shock absorption, wear resistance, oil and water resistance, acid and alkali resistance, etc. It has good storage stability and a wide range of toughness. Therefore, PU materials have penetrated into our lives and various industrial fields, and are widely used in coatings, construction, medical care, automobiles, railways, aviation and other fields. However, PU without flame retardant treatment is flammable in the air, and its limiting oxygen index (LOI) is only about 17%. Toxic gases such as HCN and CO will be released during the combustion process, which can easily cause suffocation and death. In addition, the combustion of PU will produce a large amount of molten droplets and smoke, which can easily cause harm to the human body, so it is of great significance to improve the flame retardancy of PU.
[0003] The flame retardancy of PU is mainly achieved by adding flame retardants, which are divided into "additive" flame retardants and "reactive" flame retardants according to the combination of flame retardants and PU. Additive flame retardants are physically incorporated into polyurethane, but in order to achieve the desired flame retardant properties, a large amount of flame retardants are often required to be added. Since most flame retardants have poor compatibility with the material matrix, the mechanical properties of the elastomer will inevitably deteriorate. At the same time, its overflow phenomenon will also have a negative impact on the human body and the environment, so it is restricted by environmental protection directives of various countries. Reactive flame retardants have good compatibility with PU and can play a flame retardant role without significantly affecting the mechanical properties, and their overall performance is better. Therefore, reactive flame retardants are undoubtedly the ideal choice for achieving flame retardancy of PU.
[0004] At present, most of the PU on the market comes from petrochemical products. Although the flame retardant and mechanical properties of PU prepared with petroleum-based reactive flame retardants are good, there are also obvious problems. Petroleum-based reactive flame retardants generally require multi-step synthesis, which is costly and will produce a large amount of toxic and harmful "three wastes". Based on the concept of sustainable development, using low-toxic, renewable, and easily degradable biomass raw materials instead of petrochemical products to produce plastic products, and researching and developing new reactive flame retardants such as bio-based reactive flame retardants will be conducive to promoting the development of high-performance flame-retardant polyurethane elastomer preparation technology. Summary of the invention
[0005] Technical problem to be solved: In order to solve the problem that polyurethane elastomer has poor flame retardancy and petroleum-based reactive flame retardants are not environmentally friendly, the present invention selects tannic acid widely present in plants such as bark and fruit as a reactive flame retardant and crosslinking agent, and utilizes hydroxyl and isocyanate groups for reversible crosslinking to design a bio-based flame retardant polyurethane elastomer and a preparation method thereof, which can improve the flame retardancy of polyurethane elastomer and maintain certain mechanical properties. The preparation process of the method is simple and easy to operate, and the obtained polyurethane elastomer has good flame retardancy and mechanical properties.
[0006] Technical solution: A method for preparing a bio-based flame-retardant polyurethane elastomer, which is prepared by the following steps in proportion: the first step is to dissolve tannic acid in tetrahydrofuran to obtain a tetrahydrofuran solution of tannic acid; the second step is to weigh prepolymer E95C and add it to the tetrahydrofuran solution of tannic acid, raise the temperature to 35-45°C and stir until the prepolymer E95C is completely dissolved, and the mass ratio of tannic acid to prepolymer E95C is 1:(5-20); the third step is to rotary evaporate the mixed solution obtained in the previous step under the conditions of -0.1MPa and 40-45°C to remove tetrahydrofuran and generate a viscous liquid; the viscous liquid is then poured into a tetrafluoroethylene mold, put into an oven, reacted at 75-85°C for 3-5h to remove the unevaporated tetrahydrofuran, and heated to 110-130°C for 11-13h to solidify it to generate an elastomer.
[0007] Preferably, the mass ratio of the tannic acid to the prepolymer E95C is 1:20, 1:10 or 1:5.
[0008] Preferably, the temperature of the heating and stirring is 40°C.
[0009] Preferably, the rotary evaporation temperature is 45°C.
[0010] Preferably, the curing conditions are: reacting at 80° C. for 4 hours, and then heating to 120° C. for 12 hours.
[0011] The bio-based flame-retardant polyurethane elastomer prepared by the preparation method.
[0012] Beneficial effects: 1. The bio-based polyurethane elastomer prepared by the method of the present invention uses tannic acid, which is widely available, biocompatible and non-toxic, as its raw material, which improves the performance and value of traditional products of biomass resources and expands the research direction of biomass resources. 2. The flame retardant properties of the bio-based polyurethane elastomer prepared by the method of the present invention are greatly improved compared with the polyurethane elastomer using 1,4-butanediol as a cross-linking agent, which broadens the application field of polyurethane elastomer. 3. The bio-based polyurethane elastomer prepared by the method of the present invention uses non-toxic and pollution-free tannic acid as a cross-linking agent, has a clearer molecular structure, higher and reversible cross-linking activity, and gives the polyurethane elastomer better mechanical properties, which broadens the application field of polyurethane elastomer. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 The infrared spectra of tannic acid and bio-based flame-retardant polyurethane elastomer with tannic acid as crosslinker are shown in Figure 1. The disappearance of the characteristic peak of tannic acid hydroxyl group, the disappearance of the characteristic peak of isocyanate group in prepolymer E95C, and the formation of carbamate in polyurethane can be seen, indicating that tannic acid and prepolymer E95C react fully. DETAILED DESCRIPTION
[0014] Example 1
[0015] The first step is to weigh 1,4-butanediol and add it to a reaction container according to a mass ratio of 1,4-butanediol to prepolymer E95C of 1:20, measure 20 mL of tetrahydrofuran and pour it into the reaction container, and continue stirring for 10 minutes until 1,4-butanediol is completely dissolved to obtain a tetrahydrofuran solution of 1,4-butanediol; the second step is to weigh prepolymer E95C and add it to the tetrahydrofuran solution of 1,4-butanediol according to a mass ratio of 1,4-butanediol to prepolymer E95C of 1:20, raise the reaction temperature to 40°C, and continue stirring for 10 minutes until prepolymer E95C is completely dissolved in the tetrahydrofuran solution of 1,4-butanediol to obtain a reaction mixed solution; the third step is to rotary evaporate the reaction mixed solution at a pressure of -0.1 MPa and a temperature of 45°C for 20 minutes to remove tetrahydrofuran and generate a viscous liquid. The viscous liquid was then poured into a tetrafluoroethylene mold, reacted at 80°C for 4 hours to remove all unevaporated tetrahydrofuran, and then heated to 120°C for 12 hours to solidify it into a polyurethane elastomer, thereby obtaining a polyurethane elastomer with a mass ratio of 1,4-butanediol to prepolymer E95C of 1:20.
[0016] Example 2
[0017] The first step is to weigh gallic acid and add it to a reaction container at a mass ratio of 1:20 between gallic acid and prepolymer E95C, measure 20 mL of tetrahydrofuran and pour it into the reaction container, and continue stirring for 10 minutes until the gallic acid is completely dissolved to obtain a tetrahydrofuran solution of gallic acid; the second step is to weigh prepolymer E95C and add it to the tetrahydrofuran solution of gallic acid at a mass ratio of 1:20 between gallic acid and prepolymer E95C, raise the reaction temperature to 40°C, and continue stirring for 10 minutes until the prepolymer E95C is completely dissolved in the tetrahydrofuran solution of gallic acid to obtain a reaction mixed solution; the third step is to rotary evaporate the reaction mixed solution at a pressure of -0.1 MPa and a temperature of 45°C for 20 minutes to remove tetrahydrofuran and generate a viscous liquid. The viscous liquid was then poured into a tetrafluoroethylene mold, reacted at 80°C for 4 hours to remove the unevaporated tetrahydrofuran, and then heated to 120°C for 12 hours to solidify it into a polyurethane elastomer, thereby obtaining a polyurethane elastomer with a mass ratio of gallic acid to prepolymer E95C of 1:20.
[0018] Example 3
[0019] The first step is to weigh tannic acid and add it to a reaction container according to a mass ratio of tannic acid to prepolymer E95C of 1:20, measure 20 mL of tetrahydrofuran and pour it into the reaction container, and continue stirring for 10 minutes until the tannic acid is completely dissolved, so as to obtain a tetrahydrofuran solution of tannic acid; the second step is to weigh prepolymer E95C and add it to the tetrahydrofuran solution of tannic acid according to a mass ratio of tannic acid to prepolymer E95C of 1:20, raise the reaction temperature to 40°C, and continue stirring for 10 minutes until the prepolymer E95C is completely dissolved in the tetrahydrofuran solution of tannic acid to obtain a reaction mixed solution; the third step is to rotary evaporate the reaction mixed solution at a pressure of -0.1 MPa and a temperature of 45°C for 20 minutes to remove tetrahydrofuran and generate a viscous liquid. The viscous liquid was then poured into a tetrafluoroethylene mold, reacted at 80°C for 4 hours to remove the unevaporated tetrahydrofuran, and then heated to 120°C for 12 hours to solidify it into a polyurethane elastomer, thereby obtaining a polyurethane elastomer with a mass ratio of tannic acid to prepolymer E95C of 1:20.
[0020] Example 4
[0021] The first step is to weigh tannic acid and add it to a reaction container according to a mass ratio of tannic acid to prepolymer E95C of 1:10, measure 20 mL of tetrahydrofuran and pour it into the reaction container, and continue stirring for 10 minutes until the tannic acid is completely dissolved, so as to obtain a tetrahydrofuran solution of tannic acid; the second step is to weigh prepolymer E95C and add it to the tetrahydrofuran solution of tannic acid according to a mass ratio of tannic acid to prepolymer E95C of 1:10, raise the reaction temperature to 40°C, and continue stirring for 10 minutes until the prepolymer E95C is completely dissolved in the tetrahydrofuran solution of tannic acid to obtain a reaction mixed solution; the third step is to rotary evaporate the reaction mixed solution at a pressure of -0.1 MPa and a temperature of 45°C for 20 minutes to remove tetrahydrofuran and generate a viscous liquid. The viscous liquid was then poured into a tetrafluoroethylene mold, reacted at 80°C for 4 hours to remove the unevaporated tetrahydrofuran, and then heated to 120°C for 12 hours to solidify it into a polyurethane elastomer, thereby obtaining a polyurethane elastomer with a mass ratio of tannic acid to prepolymer E95C of 1:10.
[0022] Example 5
[0023] The first step is to weigh tannic acid and add it to a reaction container according to a mass ratio of tannic acid to prepolymer E95C of 1:5, measure 20 mL of tetrahydrofuran and pour it into the reaction container, and continue stirring for 10 minutes until the tannic acid is completely dissolved, so as to obtain a tetrahydrofuran solution of tannic acid; the second step is to weigh prepolymer E95C and add it to the tetrahydrofuran solution of tannic acid according to a mass ratio of tannic acid to prepolymer E95C of 1:5, raise the reaction temperature to 40°C, and continue stirring for 10 minutes until the prepolymer E95C is completely dissolved in the tetrahydrofuran solution of tannic acid to obtain a reaction mixed solution; the third step is to rotary evaporate the reaction mixed solution at a pressure of -0.1 MPa and a temperature of 45°C for 20 minutes to remove tetrahydrofuran and generate a viscous liquid. The viscous liquid was then poured into a tetrafluoroethylene mold, reacted at 80°C for 4 hours to remove all the unevaporated tetrahydrofuran, and then heated to 120°C for 12 hours to solidify it into a polyurethane elastomer, thereby obtaining a polyurethane elastomer with a mass ratio of tannic acid to prepolymer E95C of 1:5.
[0024] Comparative Example:
[0025] Experimental Group 1: The tensile strength and elongation at break of the flame-retardant polyurethane elastomer prepared in Example 1 using 1,4-butanediol as a cross-linking agent were 14.17 MPa and 1334.95%, respectively, and the flame-retardant test LOI value was 20%.
[0026] Experimental Group 2: The tensile strength and elongation at break of the bio-based flame retardant polyurethane elastomer prepared in Example 2 with gallic acid as the crosslinking agent were 14.22 MPa and 1381.27%, respectively. The flame retardant test LOI value was 40%
[0027] Experimental Group 3: The tensile strength and elongation at break of the bio-based flame-retardant polyurethane elastomer prepared in Example 3 using tannic acid as a cross-linking agent were 13.20 MPa and 431.69%, respectively, and the flame retardant test LOI value was 41%.
[0028] Experimental Group 4: The tensile strength and elongation at break of the bio-based flame-retardant polyurethane elastomer prepared in Example 4 using tannic acid as a cross-linking agent were 24.83 MPa and 484.16%, respectively, and the flame retardant test LOI value was 40%.
[0029] Experimental Group 5: The tensile strength and elongation at break of the bio-based flame retardant polyurethane elastomer prepared in Example 5 using tannic acid as a cross-linking agent were 30.43 MPa and 618.87%, respectively, and the flame retardant test LOI value was 34%.
[0030] The following table compares the mechanical properties and flame retardant properties of each experimental group:
[0031]
[0032] Note: The tensile properties refer to GB / T 528-2009 Test Method for Determination of Tensile Stress-Strain Properties of Vulcanized Rubber or Thermoplastic Rubber, and the CMT4254 microcomputer-controlled electronic universal testing machine (Shenzhen Xinsansi) is used to determine the tensile properties of the material. The tensile test speed is 100mm / min, and the test temperature is room temperature. The LOI performance refers to GB / T 2406.2-2009 Test Method for Determination of Combustion Behavior by Oxygen Index Method for Plastics, and the HC-2C oxygen index tester (Nanjing Shangyuan) is used to determine the flame retardant properties of the material.
Claims
1. A method for preparing a bio-based flame-retardant polyurethane elastomer, characterized in that: In the first step, according to the mass ratio of tannic acid to prepolymer E95C of 1:20, tannic acid is weighed and added to the reaction container, 20 mL of tetrahydrofuran is measured and poured into the reaction container, and stirring is continued for 10 minutes until the tannic acid is completely dissolved to obtain a tetrahydrofuran solution of tannic acid; in the second step, according to the mass ratio of tannic acid to prepolymer E95C of 1:20, prepolymer E95C is weighed and added to the tetrahydrofuran solution of tannic acid, the reaction temperature is raised to 40°C, and stirring is continued for 10 minutes until the prepolymer E95 C is completely dissolved in the tetrahydrofuran solution of tannic acid to obtain a reaction mixed solution; in the third step, the reaction mixed solution is rotary evaporated at a pressure of -0.1 MPa and a temperature of 45°C for 20 minutes to remove tetrahydrofuran and generate a viscous liquid; the viscous liquid is then poured into a tetrafluoroethylene mold, reacted at 80°C for 4 hours to remove the unevaporated tetrahydrofuran, and then heated to 120°C for 12 hours to solidify it into a polyurethane elastomer, thereby obtaining a polyurethane elastomer with a mass ratio of tannic acid to prepolymer E95C of 1:
20.
2. The bio-based flame retardant polyurethane elastomer prepared by the preparation method according to claim 1.
Citation Information
Patent Citations
Biomass-resource-modified water-based polyurethane emulsion and preparation method thereof
CN105924616A
Polyurethane elastomer and product and preparation method thereof
CN106832191A