A numerical simulation method for deposition stress of functionally graded thermal barrier coatings on curved substrates
A three-dimensional numerical model is established through ABAQUS finite element software to simulate the deposition process of functionally graded thermal barrier coatings on curved substrates layer by layer, solving the problem of inaccurate calculation results in the existing technology and achieving accurate calculation and analysis of deposition stress on curved substrates. Improved thermal cycle life performance.
Patent Information
- Application Number
- CN202210248236.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-14
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-03-14
AI Technical Summary
When the existing technology studies the thermal stress during the preparation process of functionally graded thermal barrier coatings on curved substrates, the calculation results are inaccurate and ignore the deposition stress caused by molten and semi-molten particles during the spraying process, resulting in cracks and peeling of the coating. , affecting bonding strength and thermal cycle life.
ABAQUS finite element software is used to establish a three-dimensional numerical model to simulate the deposition process of functional gradient thermal barrier coating on curved surface layer by layer. The deposition stress is calculated and imported into the next layer model, fine meshing and gradient mesh processing are performed to simulate the evolution of deposition stress. process.
The calculation accuracy and actual proximity are improved, and the deposition stress of functionally graded thermal barrier coatings on curved substrates can be accurately calculated, helping to study failure modes and optimizing design solutions, reducing costs, and enhancing performance support for thermal cycle life.
Smart Images

Figure CN114580245B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal stress of thermal barrier coatings, and in particular to a numerical simulation method for deposition stress of a functional gradient thermal barrier coating on a curved substrate. Background Art
[0002] Thermal barrier coatings (TBCs) are a key technology for gas turbines and aircraft engines. They have good thermal insulation properties and have gradually become a hot topic of research. Traditional thermal barrier coatings generally consist of three parts: a ceramic layer, an adhesive layer, and a high-temperature alloy substrate. In order to alleviate the stress concentration at the interface of thermal barrier coatings, foreign scholars have proposed the concept of functionally gradient thermal barrier coatings (FG-TBCs). Compared with traditional single-layer thermal barrier coatings, FG-TBCs deposits a functionally gradient coating composed of NiCrA1Y particles and ZrO2-8% Y2O3 between the pure metal layer (BC layer) and the pure ceramic layer (YSZ layer) and changes according to a certain gradient, realizing the transition from metal (BC) to ceramic (YSZ) in terms of composition and thermophysical properties.
[0003] Since thermal stress during the preparation of coatings is the main factor of coating failure, it seriously affects the service life of coatings. Accurately predicting the thermal stress during the preparation of functional gradient thermal barrier coatings has far-reaching significance for further studying its failure form, optimizing design schemes and industrial applications. As far as we know, the current research on thermal stress during the preparation of thermal barrier coatings focuses on the use of plane models. However, in fact, since the hot end components are curved, thermal barrier coatings are mostly deposited on curved substrates. It is more important to study the influence of thermal stress and curvature on the preparation of curved substrate FG-TBCs. Therefore, it is very necessary to study the finite element simulation (FiniteElement Method, FEM) method of thermal stress during the preparation of curved substrate FG-TBCs. However, the current finite element technology mostly uses the birth and death unit method to simulate the layer-by-layer deposition process of thermal barrier coatings. This method requires the definition of an ideal material between the birth unit and the death unit to transfer temperature, displacement and force. This ideal material is difficult to be close to the actual situation, which often causes inaccurate calculation results.
[0004] In addition, the current research on thermal stress in the preparation process of thermal barrier coatings on curved substrates focuses on the thermal mismatch stress caused by the mismatch of thermal expansion coefficients between layers during the cooling process after the coating is sprayed, and ignores the deposition stress caused by the quenching of molten and semi-molten particles during the spraying process. Previous studies have shown that compared with CTE thermal mismatch stress, this deposition stress has a more significant impact on the final thermal stress, which can lead to the initiation and expansion of coating cracks and coating peeling, and have a profound impact on the coating's bonding strength, thermal cycle life and other properties. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the present invention provides a numerical simulation method for the deposition stress of functional gradient thermal barrier coatings on curved substrates, and obtains the evolution process of deposition stress during the preparation process, which is of great significance for further studying the failure forms of functional gradient thermal barrier coatings, optimizing design schemes and preparation processes.
[0006] To achieve the above object, the present invention provides the following technical solution: a numerical simulation method for deposition stress of functional gradient thermal barrier coating on curved substrate, the specific steps are as follows:
[0007] S1 uses ABAQUS finite element software to establish a three-dimensional model of the substrate depositing the i+1th layer of coating, where the substrate is a curved substrate on which the i-th layer of coating is deposited, i=0,1,2…, i+1≤n, and n is the total number of coatings;
[0008] S2 obtains the material properties and structural properties of the substrate and the coating, and assigns the material properties and structural properties of the substrate and the coating to the substrate and the coating of the three-dimensional model established in step S1 to obtain a three-dimensional numerical model;
[0009] S3 analyzes the preparation process of functional gradient thermal barrier coatings, establishes analysis steps, creates interactions between coatings and between coatings and substrates, applies temperature loads to the three-dimensional numerical model, and sets boundary conditions;
[0010] S4 meshes the substrate and coating respectively;
[0011] S5 submits a three-dimensional numerical model for calculation to obtain the deposition stress of each coating layer during deposition and the deposition stress of the coating and substrate when the overall coating is prepared.
[0012] Furthermore, in step S5, the specific calculation process is:
[0013] S5.1 Calculation of the deposition stress P generated by the three-dimensional numerical model of the i-th coating deposited on the substrate during quenching i , i = 1, 2…, i ≤ n, n is the total number of coatings, and the calculated deposition stress P iImport into the three-dimensional numerical model of i+1 layers of coating deposited on the substrate;
[0014] S5.2 Calculation of the deposition stress P generated by the three-dimensional numerical model of the i+1 layer coating deposited on the substrate during quenching i+1 , and the calculated deposition stress P i+1 Import into the three-dimensional numerical model of i+2 layers of coating deposited on the substrate;
[0015] S5.3 and so on until the deposition stress P of the three-dimensional numerical model of the nth coating layer deposited on the substrate is calculated. n .
[0016] Furthermore, in step S1, the curved surface base is a cylindrical or elliptical cylinder model with arbitrary curvature.
[0017] Furthermore, in step S2, the coating is a functional gradient thermal barrier coating, and the coating is divided into n layers, each layer has a thickness of h, and each layer of the coating is composed of a certain proportion of material A particles and material B particles in a gradient manner.
[0018] Furthermore, in step S2, the material properties and structural properties of the substrate and the coating include Young's modulus, Poisson's ratio and thermal expansion coefficient at different temperatures.
[0019] Further, in step S3,
[0020] 301, create the analysis step as steady state, general; create field output, the output variables are stress and strain, displacement, action and reaction force, contact stress; create process output, the output variable is energy;
[0021] 302, create interaction, set the contact mode and contact properties between the coating and the substrate and between the coatings as Tie binding constraints;
[0022] 303, applying a temperature load to the three-dimensional numerical model, reducing the coating temperature from the melting point to the spraying temperature, so that the substrate is always at the spraying temperature state;
[0023] 304, setting boundary conditions, applying simply supported boundary conditions on the bottom edge of the base.
[0024] Furthermore, in step 304, the three-dimensional numerical model is processed by axisymmetry, and symmetric boundary conditions are applied to the cross sections at the symmetry points.
[0025] Furthermore, in step S4, when meshing the substrate and the coating, the unit type adopts 3DStressC3D8R unit, the unit shape adopts hexahedral unit, and the meshing technology adopts structured meshing technology.
[0026] Furthermore, in step S4, the substrate is divided into grids using grid units with gradient changes in size, and the coating is divided into grids using fine grid units.
[0027] Furthermore, in step S4, when meshing is performed, each layer of coating is distributed with 10 mesh units in the thickness direction.
[0028] Compared with the prior art, the present invention has at least the following beneficial effects:
[0029] The present invention provides a numerical simulation method for deposition stress of a functional gradient thermal barrier coating on a curved substrate. First, the present invention establishes a numerical model capable of calculating deposition stress caused by quenching during layer-by-layer deposition of FG-TBCs on a curved substrate. In practical applications, hot end components are mostly composed of different complex curved surfaces, and thermal barrier coatings are mostly deposited on various complex curved substrates. The numerical model of the curved substrate disclosed in the present invention can calculate deposition stress during the preparation process of a functional gradient thermal barrier coating system on a curved substrate. Compared with a model capable of only calculating the preparation of thermal barrier coatings on a plane, the numerical model is closer to the actual preparation process and meets actual production needs. The numerical model is of great significance for further studying the failure form, optimizing the design scheme and the preparation process of FG-TBCs on a curved substrate and obtaining the evolution law of thermal stress during the preparation process of FG-TBCs with different curvatures by studying the thermal stress during the preparation process of FG-TBCs on a curved substrate.
[0030] Secondly, the thermal stress in the preparation process of thermal barrier coatings includes the deposition stress during layer-by-layer deposition and the thermal mismatch stress when the deposition is completed and cooled to room temperature. Compared with the thermal mismatch stress, the deposition stress caused by quenching has a more significant effect on the final thermal stress, which will lead to the initiation, expansion and peeling of coating cracks, and have a profound impact on the coating's bonding strength, thermal cycle life and other properties. Compared with other known models, the numerical simulation method of deposition stress of functional gradient thermal barrier coatings on curved substrates disclosed in the present invention can calculate this deposition stress. By establishing different three-dimensional numerical models, the deposition stress caused by quenching in the preparation process of functional gradient thermal barrier coatings on curved substrates can be calculated, and the cost is low, which provides technical support for further research on the control of defects such as cracks in the preparation process of curved functional gradient thermal barrier coating systems and the thermal cycle life during use.
[0031] This new numerical simulation method invented is different from the traditional life and death unit technology. This method establishes the numerical model of each layer deposited in the layer-by-layer preparation process of the thermal barrier coating on the curved substrate, and uses the deposition stress result when preparing the previous layer to import the result into the numerical model when preparing the next layer. It more realistically simulates the layer-by-layer preparation process of the thermal barrier coating on the curved substrate, and the calculation results are more accurate.
[0032] When dividing the grid units, the present invention adopts the processing methods of the grid units with gradient variation in base size and the fine grid units of the coating respectively. The coating is thinner than the base. In order to eliminate this influence, the base grid unit size is processed by a gradient reduction from the inner surface to the outer surface; the coating adopts a fine grid, and each layer of coating has 10 grid units distributed in the thickness direction, which improves the calculation accuracy and efficiency of the model.
[0033] The present invention establishes a numerical model for the deposition of each layer of the thermal barrier coating on a curved substrate during the layer-by-layer preparation process, uses the deposition stress result when preparing the previous layer, and imports the result into the numerical model when preparing the next layer. Not only can the deposition stress distribution of the coating and the substrate be obtained when the overall coating is prepared, but also the deposition stress distribution when the coating is deposited on one of the layers can be obtained. In other words, the stress evolution of the coating during the layer-by-layer deposition process can be obtained. By analyzing the evolution of the deposition stress, the stress variation law of the coating during the layer-by-layer deposition process can be obtained, which is convenient for studying its failure form, optimizing the design of the thermal barrier coating, and guiding the actual preparation process. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The three-dimensional model of the curved substrate FG-TBCs (substrate plus all coatings) established using ABAQUS;
[0035] Figure 2 Schematic diagram of the change in the volume fraction of the ZrO2-8%Y2O3 / NiCrA1Y coating in the FG-TBCs on the curved substrate;
[0036] Figure 3 Schematic diagram of meshing for the numerical model of FG-TBCs on curved substrates;
[0037] Figure 4 The numerical simulation results of the deposition stress caused by quenching when the FG-TBCs deposition on the curved substrate is completed, where a is the radial deposition stress, b is the circumferential deposition stress, and c is the axial deposition stress;
[0038] Figure 5 The sedimentation stress evolution results during the preparation of FG-TBCs on curved substrates, where a is the radial sedimentation stress, b is the circumferential sedimentation stress, and c is the axial sedimentation stress; DETAILED DESCRIPTION
[0039] The embodiments of the present invention are described below in conjunction with the accompanying drawings, and the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0040] The present invention provides a numerical simulation method for deposition stress of functional gradient thermal barrier coatings on curved substrates. Based on ABAQUS finite element simulation software, the deposition stress caused by quenching in the process of preparing FG-TBCs on curved substrates by atmospheric plasma technology (APS) is numerically simulated, a numerical model of deposition stress caused by quenching in a layer-by-layer deposition process is developed, and the evolution process of deposition stress in the preparation of FG-TBCs on curved substrates is obtained.
[0041] A numerical simulation method for deposition stress of functional gradient thermal barrier coating on curved substrates comprises the following steps: 1) using ABAQUS finite element software to establish a three-dimensional model of depositing the i+1th layer of coating on multiple substrates, wherein the substrate is a curved substrate on which the i-th layer of coating is deposited, i=0,1,2..., i+1≤n, n is the total number of coatings, and the curved substrate is a cylindrical or elliptical cylinder model with arbitrary curvature.
[0042] 2) Obtaining the material properties and structural properties of the substrate and the coating, assigning the material properties and structural properties of the substrate and the coating to the substrate and the coating in the three-dimensional model established in step 1, and obtaining a three-dimensional numerical model.
[0043] 3) Analyze the preparation process, establish analysis steps, create interactions between coatings and between coatings and substrates, apply loads, and set boundary conditions.
[0044] 4) Meshing the substrate and coating respectively;
[0045] 5) Submit the three-dimensional numerical model for calculation.
[0046] In step 2, the specific method of establishing a material library is:
[0047] The coating is divided into n layers, each layer is h thick, and each layer is composed of a certain proportion of material A particles and material B particles. During the preparation process, the material A and material B powders of each layer are mixed in a certain proportion, heated to a molten state by a plasma spray gun, and then sprayed on the substrate surface at high speed. The molten A and B mixed particles quickly adhere, cool, and solidify on the substrate surface to form a coating. According to the determined volume fraction, the material properties of each layer of A and B materials are calculated, and each coating is assigned separately in the numerical model. The implementation method can be seen in the embodiment.
[0048] When the temperature changes, the thermophysical properties of each material will change. If fixed numerical values are used for calculation, the accuracy of the calculation results will be affected. Therefore, the present invention takes into account the changes in the thermophysical properties of the substrate and coating materials with temperature, including the Young's modulus, Poisson's ratio and thermal expansion coefficient of the substrate and coating materials.
[0049] Specifically, the present invention inputs the Young's modulus, Poisson's ratio and thermal expansion coefficient of the substrate and coating materials at several known temperatures into the ABAQUS software. The software will interpolate and calculate the Young's modulus, Poisson's ratio and thermal expansion coefficient of the coating and substrate at different temperatures when depositing each coating based on the input data.
[0050] The specific steps of step 3 are:
[0051] 301, create analysis steps, field output and process output;
[0052] 302, creating interactions, describing the contact mode and contact properties between the coating and the substrate and between the coatings, setting the contact mode and contact properties between the coating and the substrate and between the coatings as Tie binding constraints to describe the layer-by-layer preparation state of the coating;
[0053] 303, applying temperature load to the three-dimensional numerical model to simulate the temperature change during the layer-by-layer preparation of the coating, reducing the coating temperature from the melting point to the spraying temperature, so that the substrate is always at the spraying temperature state;
[0054] 304, set the boundary conditions, and apply the simply supported boundary conditions at the edge of the bottom surface of the base to avoid the infinite displacement of the rigid body. In order to reduce the data processing time, the overall three-dimensional numerical model is processed by axisymmetry (half cylinder), and the symmetric boundary conditions are applied to the cross section at the symmetry.
[0055] In step 4, if Figure 3 As shown in the figure, the base and coating are meshed respectively, and the unit type is 3DStressC3D8R unit, the unit shape is hexahedral unit, and the meshing technology is structured meshing technology. In order to improve the calculation accuracy and efficiency of the model, the processing methods of base size gradient change grid unit and coating fine grid unit are used respectively. The coating is thinner than the base. In order to eliminate this effect, the base grid unit size is processed by gradient reduction from the inner surface to the outer surface; the coating uses a fine grid, and each layer of coating is distributed with 10 grid units in the thickness direction, and the grid independence of the model is verified.
[0056] In step 5, the specific calculation process is:
[0057] 1) Calculate the deposition stress P generated by the three-dimensional numerical model of the i-th coating deposited on the substrate during quenching i (i=1,2…,i≤n,n is the total number of coatings), and the calculated deposition stress P i Import into the three-dimensional numerical model of i+1 layers of coating deposited on the substrate;
[0058] During the layer-by-layer deposition process, when the i-th layer is deposited, the deposition stress of the i-1 layers previously deposited and the deposition stress of the substrate will change. i represents the deposition stress of each layer of coating and substrate after the deposition of the i-th layer.
[0059] 2) Calculate the deposition stress P generated by the three-dimensional numerical model of the i+1 layer coating deposited on the substrate during quenching i+1 , and the calculated deposition stress P i+1 Import into the three-dimensional numerical model of i+2 layers of coating deposited on the substrate;
[0060] 5) And so on, until the deposition stress P of the three-dimensional numerical model of the nth layer of coating deposited on the substrate is calculated. n ; 6) Through the above method, the deposition stress P generated by quenching during the deposition process of FG-TBCs can be calculated i ~P n , thus obtaining the evolution process of deposition stress of FG-TBCs during deposition.
[0061] The present invention also provides a numerical simulation system for deposition stress of functional gradient thermal barrier coating on curved substrate, which specifically comprises:
[0062] A model building module is used to build a three-dimensional model of a substrate depositing an i+1th layer of coating, wherein the substrate is a curved surface substrate on which an i-th layer of coating is deposited, i=0,1,2…, i+1≤n, and n is the total number of coatings;
[0063] The property acquisition module is used to acquire the material properties and structural properties of the substrate and the coating, and assign the material properties and structural properties of the substrate and the coating to the substrate and the coating of the three-dimensional model established by the model establishment module to obtain a three-dimensional numerical model;
[0064] The analysis module is used to analyze the preparation process of functional gradient thermal barrier coatings, establish analysis steps, create the interactions between coatings and between coatings and substrates, apply temperature loads to the three-dimensional numerical model, and set boundary conditions;
[0065] A processing module for meshing the substrate and the coating respectively;
[0066] The calculation module is used to calculate the three-dimensional numerical model to obtain the deposition stress of each coating layer when it is deposited and the deposition stress of the coating and the substrate when the overall coating is prepared.
[0067] The present invention also provides a computer device, including a memory and a processor, wherein the memory stores a computer program, and when the processor executes the computer program, the steps of the numerical simulation method of the deposition stress of the functional gradient thermal barrier coating on the curved substrate are implemented.
[0068] The present invention also provides a computer-readable storage medium having a computer program stored thereon, which, when executed by a processor, implements the steps of the above-mentioned method for numerically simulating deposition stress of functional gradient thermal barrier coating on curved substrates.
[0069] Example 1
[0070] We calculated the deposition stress of FGC composed of ZrO2-8%Y2O3 and NiCrA1Y particles deposited on a curved nickel-based superalloy substrate. The total thickness of FG-TBCs (ZrO2-8%Y2O3 / NiCrA1Y) was 400μm, and the thickness of each coating was 50μm. The coating was deposited on the cylindrical surface of a cylindrical nickel-based alloy with an inner diameter of 6mm, an outer diameter of 8mm, and a length of 20mm. The volume fraction of ZrO2-8%Y2O3 and NiCrA1Y particles in each layer varied linearly in the FGC.
[0071] The specific steps include:
[0072] 1) Use ABAQUS finite element software to establish a three-dimensional model of the substrate plus the i+1th layer of coating (i=0,1,2…,i+1≤8), and obtain 8 three-dimensional models, among which the three-dimensional model of the substrate plus the 8th layer of coating is as follows Figure 1 As shown;
[0073] 2) Obtain the material properties and structural properties of the nickel-based alloy and the coating ZrO2-8%Y2O3 / NiCrA1Y, and assign the properties of the nickel-based alloy and the coating ZrO2-8%Y2O3 / NiCrA1Y to the substrate and coating in the three-dimensional model established in step 1.
[0074] The present invention takes into account the change of the thermophysical properties of the coating and substrate materials with temperature. Including the Young's modulus, Poisson's ratio and thermal expansion coefficient of each material. The Young's modulus, Poisson's ratio and thermal expansion coefficient of each material at a known temperature shown in Table 1 are input into the ABAQUS software, and the software will interpolate and calculate the Young's modulus, Poisson's ratio and thermal expansion coefficient of the coating and substrate at different temperatures when depositing each coating according to the input data.
[0075] Thermophysical properties of nickel-based alloy and coating ZrO2-8%Y2O3 / NiCrA1Y materials as a function of temperature are shown in Table 1;
[0076] Table 1 Physical parameters of materials required for calculation
[0077]
[0078]
[0079] In this embodiment, the A and B components in the coating change in a linear gradient (A represents ZrO2-8% Y2O3, and B represents NiCrAlY). The volume fractions of the two materials A and B in the i-th layer are respectively but
[0080]
[0081]
[0082] n represents the total number of coatings, which is n=8 in this embodiment. The volume fractions of the two materials A and B in each coating layer are calculated as shown in the figure below. Figure 2 .
[0083] The Young's modulus E, thermal expansion coefficient α, and Poisson's ratio v of the substrate, A, and B are expressed as (E sub , α sub , ν sub )、(E A , α A , ν A ) and (E B , α B , ν B ). Then the total Young's modulus E of the i-th layer of coating formed by a uniform mixture of A and B is (A+B)i 、Coefficient of thermal expansion α (A+B)i With Poisson's ratio v (A+B)i It can be expressed as
[0084]
[0085]
[0086]
[0087] The material properties of each layer of ZrO2-8%Y2O3 / NiCrA1Y material combination and the substrate material properties will be calculated and assigned to each coating and substrate in the numerical model.
[0088] 3) Analyze the APS preparation process of the ZrO2-8% Y2O3 / NiCrA1Y functional gradient thermal barrier coating system on the curved substrate, establish the analysis steps, create the interaction between the coating and the substrate, apply loads, and set boundary conditions, including:
[0089] 301, create the analysis step as steady state, general; create field output, the output variables are stress and strain, displacement, action and reaction force, contact stress; create process output, the output variable is energy;
[0090] 302, create interaction, set the contact mode of the outer cylindrical surface of the base cylinder, the inner cylindrical surface of the coating cylinder, and the cylindrical surfaces between the coatings to "Tie" connection;
[0091] 303, applying temperature load to the model, the melting points of NiCrAlY and YSZ particles are 1680℃ and 2680℃ respectively, the spraying temperature is 475℃, the coating is reduced from the initial state (melting point temperature) to the final state (spraying temperature), so that the substrate is always at the spraying temperature state;
[0092] 304, set boundary conditions, apply simply supported boundary conditions on the bottom edge of the cylindrical model to avoid infinite displacement of the rigid body. Apply symmetric boundary conditions on the cross section where the semi-cylindrical cross section is symmetrical.
[0093] 4) The substrate and coating are meshed separately. The unit type is 3DStressC3D8R unit, the unit shape is hexahedral unit, and the meshing technology is structured meshing technology. The mesh size of the substrate in the thickness direction is 0.01mm-0.1mm (gradient decreases from inner diameter to outer diameter). The coating is thinner than the substrate. In order to eliminate this effect, the coating uses a fine grid. Each layer of coating is distributed with 10 grid units in the thickness direction to improve the calculation accuracy. The mesh size of the coating in the thickness direction is 0.005mm. The mesh is divided as shown in 3.
[0094] 5) Submit the model for calculation, first calculate the deposition stress P1 generated by quenching of the three-dimensional numerical model of the first layer of coating deposited on the substrate, when the calculation is successfully completed, import the deposition stress P1 into the three-dimensional numerical model of the second layer of coating deposited on the substrate and perform the next second calculation to obtain the deposition stress P2 of the second layer of coating deposited on the substrate; import the deposition stress P2 into the three-dimensional numerical model of the third layer of coating deposited on the substrate and perform the next second calculation to obtain the deposition stress P3 of the third layer of coating deposited on the substrate, and so on, until the deposition stress P8 of the eighth layer of coating deposited on the substrate is calculated;
[0095] When the deposition is completed, the deposition stress results of the curved substrate ZrO2-8%Y2O3 / NiCrA1Y functional gradient thermal barrier coating system caused by quenching are shown in Figure 4 As shown, a is the radial deposition stress, b is the circumferential deposition stress, and c is the axial deposition stress. During the layer-by-layer deposition process, the deposition stress evolution of the curved substrate ZrO2-8%Y2O3 / NiCrA1Y functional gradient thermal barrier coating system caused by quenching is shown in Figure 5As shown, a is the evolution result of radial deposition stress, b is the evolution result of circumferential deposition stress, and c is the evolution result of axial deposition stress. As can be seen from the figure, the evolution result of radial stress is as follows: compressive stress is shown in both the coating and the substrate, the radial stress on the inner surface of the substrate is always 0, and the maximum value of radial stress generated on the substrate during the deposition of each layer of coating appears on the outer surface of the substrate; the evolution result of circumferential stress is as follows: the circumferential stress in the coating is always tensile stress, and the circumferential stress in the substrate is always compressive stress. As the deposition proceeds, the magnitude of the circumferential stress in each layer of coating decreases, and the magnitude of the circumferential compressive stress in the substrate increases; the evolution result of axial stress is as follows: the axial stress in the coating is always tensile stress, and the axial stress in the substrate is always compressive stress. When each layer of coating is deposited, the axial stress caused at each depth of the substrate is the same. As the deposition proceeds, the deposition stress in each layer of coating gradually decreases, and the compressive stress in the substrate gradually increases.
[0096] By the above method, the deposition stress result caused by quenching during the deposition of each layer of the ZrO2-8% Y2O3 / NiCrA1Y functional gradient thermal barrier coating system on the curved substrate and the evolution law of the deposition stress during the overall deposition process can be obtained. Therefore, the present invention has the following advantages: by analyzing the evolution law of the deposition stress during the deposition of the ZrO2-8% Y2O3 / NiCrA1Y functional gradient thermal barrier coating on the curved substrate and studying the influence of different curvatures on the deposition stress, it is of great significance for further studying its failure form, optimizing the design scheme and the preparation process. Secondly, this deposition stress caused by quenching will have a more significant effect on the final thermal stress, which will lead to the initiation, expansion and peeling of the coating cracks, and have a profound impact on the properties of the coating such as the bonding strength and thermal cycle life. The study of the deposition stress during the deposition of the ZrO2-8% Y2O3 / NiCrA1Y functional gradient thermal barrier coating on the curved substrate has guiding significance for the design and service process.
[0097] The present invention develops a numerical model that can calculate the deposition stress caused by quenching during the layer-by-layer deposition of FG-TBCs on a curved substrate, which has the following advantages: first, hot end components are mostly composed of different complex curved surfaces, and thermal barrier coatings are mostly deposited on various complex curved substrates. The curved substrate numerical model disclosed in the present invention is closer to the actual preparation process and meets actual production needs. By studying the thermal stress in the preparation of FG-TBCs on curved substrates, the thermal stress evolution law in the preparation of FG-TBCs with different curvatures is obtained, which is of great significance for further studying its failure form, optimizing the design scheme and the preparation process.
Claims
1. A numerical simulation method for deposition stress of functionally graded thermal barrier coating on curved substrate, characterized in that: The specific steps are as follows: S1 uses ABAQUS finite element software to establish the base deposition i+1 3D model of a coating layer, where the substrate is deposited i Layer coating of curved substrate, i=0,1,2…,i+1≤n , n is the total number of coatings; S2 obtains the material properties and structural properties of the substrate and the coating, and assigns the material properties and structural properties of the substrate and the coating to the substrate and the coating of the three-dimensional model established in step S1 to obtain a three-dimensional numerical model; S3 analyzes the preparation process of functional gradient thermal barrier coatings, establishes analysis steps, creates interactions between coatings and between coatings and substrates, applies temperature loads to the three-dimensional numerical model, and sets boundary conditions; S4 meshes the substrate and coating respectively; S5 submits a three-dimensional numerical model for calculation to obtain the deposition stress of each coating layer when it is deposited and the deposition stress of the coating and the substrate when the overall coating is prepared; In step S3, S3.1, create the analysis step as steady state, normal; create field output, the output variables are stress strain, displacement, action and reaction force, contact stress; create process output, the output variable is energy; S3.2, create interactions, set the contact mode and contact properties between the coating and the substrate and between the coatings as Tie binding constraints; S3.3, applying a temperature load to the three-dimensional numerical model, lowering the coating temperature from the melting point to the spraying temperature, so that the substrate is always at the spraying temperature state; S3.4, setting boundary conditions, applying simply supported boundary conditions at the bottom edge of the base; In step S5, the specific calculation process is: S5.1 Calculate the deposition on the substrate i Three-dimensional numerical model of the layer coating and the deposition stress P generated during quenching i , i=1, 2…, i≤n , n is the total number of coatings, and the calculated deposition stress P i Deposition on the substrate i+ In the three-dimensional numerical model of 1-layer coating; S5.2 Calculation of deposition on substrate i+ Deposition stress P generated during quenching in a three-dimensional numerical model of a coating i+1 , and the calculated deposition stress P i+1 Deposition on the substrate i+ Three-dimensional numerical model of 2-layer coating.
2. The method for numerical simulation of deposition stress of functionally graded thermal barrier coating on curved substrate according to claim 1, characterized in that: In step S1, the curved surface base is a cylindrical or elliptical cylinder model with arbitrary curvature.
3. The method for numerical simulation of deposition stress of functionally graded thermal barrier coating on curved substrate according to claim 1, characterized in that: In step S2, the coating is a functional gradient thermal barrier coating, and the coating is divided into n layers, each layer has a thickness of h, and each layer of the coating is composed of a certain proportion of material A particles and material B particles in a gradient manner.
4. The method for numerical simulation of deposition stress of functionally graded thermal barrier coating on curved substrate according to claim 1, characterized in that: In step S2, the material properties and structural properties of the substrate and the coating include Young's modulus, Poisson's ratio and thermal expansion coefficient at different temperatures.
5. The method for numerical simulation of deposition stress of functionally gradient thermal barrier coating on curved substrate according to claim 1, characterized in that: In step 3.4, the three-dimensional numerical model is processed by axisymmetry, and symmetric boundary conditions are applied to the cross sections at the symmetry points.
6. The method for numerical simulation of deposition stress of functionally graded thermal barrier coating on curved substrate according to claim 1, characterized in that: In step S4, when meshing the substrate and the coating, the unit type adopts 3DStressC3D8R unit, the unit shape adopts hexahedral unit, and the meshing technology adopts structured meshing technology.
7. The method for numerical simulation of deposition stress of functionally gradient thermal barrier coating on curved substrate according to claim 6, characterized in that: In step S4, the substrate is divided into grids using grid units with gradient sizes, and the coating is divided into grids using fine grid units.
8. The method for numerical simulation of deposition stress of functionally graded thermal barrier coating on curved substrate according to claim 7, characterized in that: In step S4, when meshing is performed, each layer of coating is distributed with 10 mesh units in the thickness direction.
Citation Information
Patent Citations
Finite element modeling method used for damage process of thermal barrier coating of turbine blade
CN101567025A
A finite element method for simulating internal and interface cracks in hard coatings
CN109190225A