Aqueous electrolyte for supercapacitors and preparation method and application thereof
By using a neutral aqueous electrolyte composed of sulfate and small molecular weight PEG, the problems of low energy density of supercapacitors, safety hazards and high cost of existing electrolytes are solved, achieving low cost, high electrochemical stability window and good cycle performance. of supercapacitors.
Patent Information
- Application Number
- CN202210225296.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-09
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-03-09
AI Technical Summary
The low energy density of supercapacitors is a key factor restricting their development. Existing electrolytes such as organic electrolytes and ionic liquids have safety hazards, high costs, environmental pollution and other problems, and high-concentration "water-in-salt" electrolytes are expensive Expensive and toxic, not suitable for large-scale applications.
Use a neutral aqueous electrolyte composed of sulfate and small molecular weight polyethylene glycol PEG. The electrolyte molar concentration is 0.1-2mol/L and the PEG mass percentage is 1-20%. Dissolve the electrolyte into deionized water and stir thoroughly. Prepare aqueous electrolyte for use in supercapacitors.
A low-cost, environmentally friendly, non-toxic and non-polluting high electrochemical stability window has been achieved. The supercapacitor has a voltage window of up to 2.0V at room temperature and has good rate performance and cycle performance.
Smart Images

Figure CN114582637B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of supercapacitors, and in particular relates to an aqueous electrolyte for supercapacitors and a preparation method and application thereof. Background Art
[0002] Supercapacitors are a new type of energy storage device between traditional capacitors and rechargeable batteries. They have the characteristics of fast charging and discharging of capacitors, and at the same time have higher energy density than traditional capacitors. Compared with batteries and traditional capacitors, supercapacitors have the advantages of high power density, long cycle life, wide operating temperature range, maintenance-free, and green environmental protection. At present, supercapacitors have been used in rail transportation, aerospace and other fields due to their high power density.
[0003] The low energy density of supercapacitors is a key factor restricting their development. Supercapacitors are mainly composed of electrode materials, current collectors, diaphragms and electrolytes. If you want to improve its energy density, you can improve it by widening the voltage window. In fact, the performance of the electrolyte greatly affects the performance of supercapacitors. The electrolytes that are widely studied at present are aqueous electrolyte systems, organic electrolyte systems and ionic liquids. Organic electrolytes have a higher working voltage, but their poor ion transmission capacity, high cost, toxicity, flammability and serious pollution also bring safety hazards, high cost and environmental pollution to actual production. Ionic liquids are also not conducive to their large-scale application due to their high price and low ionic conductivity. In contrast, aqueous electrolytes have lower costs, high ionic conductivity, higher safety and easy operation, which deserve more attention. Aqueous electrolytes are divided into acidic electrolyte systems, alkaline electrolyte systems and neutral electrolyte systems. Neutral electrolyte systems are safer and non-corrosive.
[0004] Although high-concentration "salt-in-water" electrolytes have a larger electrochemical stability window than traditional aqueous electrolytes, they are still not suitable for large-scale applications due to their high viscosity, high ion conductivity, high cost, and certain toxicity. The development of low-cost, environmentally friendly, non-toxic, and non-corrosive neutral aqueous electrolyte systems is crucial to the development of electrolytes. Summary of the invention
[0005] The purpose of the present invention is to provide an aqueous electrolyte for a supercapacitor and a preparation method and application thereof. The obtained aqueous electrolyte is low in price and more environmentally friendly.
[0006] The aqueous electrolyte provided by the present invention has an electrochemical stability window of up to about 4.6V, and is non-toxic, non-polluting and non-corrosive; compared with "salt-in-water" and organic electrolytic liquids, the price is extremely low; the aqueous supercapacitor assembled based on the neutral aqueous electrolyte of the present invention has a voltage window of up to 2.0V at room temperature and has good rate performance.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions.
[0008] A water-based electrolyte for supercapacitors, prepared from electrolyte, water and low molecular weight polyethylene glycol (PEG); wherein: the electrolyte is sulfate, the low molecular weight PEG has a number average molecular weight M n =200-600 or more are mixed in any proportion; the molar concentration of the electrolyte in the aqueous electrolyte is 0.1-2 mol / L; the mass percentage of the low molecular weight PEG in the aqueous electrolyte is 1-20%.
[0009] The sulfate is one or more of lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, zinc sulfate or aluminum sulfate mixed in any proportion.
[0010] The electrolyte is lithium sulfate with a molar concentration of 0.2-2 mol / L in an aqueous electrolyte, sodium sulfate with a molar concentration of 0.1-1 mol / L in an aqueous electrolyte, potassium sulfate with a molar concentration of 0.1-0.5 mol / L in an aqueous electrolyte, magnesium sulfate with a molar concentration of 0.2-1 mol / L in an aqueous electrolyte, zinc sulfate with a molar concentration of 0.2-1.5 mol / L in an aqueous electrolyte, or aluminum sulfate with a molar concentration of 0.1-1 mol / L in an aqueous electrolyte.
[0011] Preferably, the electrolyte is lithium sulfate with a molar concentration of 0.5-1.5 mol / L in the aqueous electrolyte, sodium sulfate with a molar concentration of 0.5-1 mol / L in the aqueous electrolyte, potassium sulfate with a molar concentration of 0.2-0.5 mol / L in the aqueous electrolyte, magnesium sulfate with a molar concentration of 0.5-1 mol / L in the aqueous electrolyte, zinc sulfate with a molar concentration of 0.5-1.5 mol / L in the aqueous electrolyte, or aluminum sulfate with a molar concentration of 0.5-1 mol / L in the aqueous electrolyte. The mass fraction of low molecular weight PEG in the electrolyte is 1-10%.
[0012] The present invention also provides a method for preparing the aqueous electrolyte of the supercapacitor, which comprises first mixing deionized water and low molecular weight PEG in proportion, then dissolving the electrolyte in the mixed solvent, and stirring the mixture to obtain the aqueous electrolyte of the supercapacitor.
[0013] The present invention also provides another method for preparing the aqueous electrolyte of the supercapacitor, which comprises first dissolving the electrolyte in water to form an aqueous electrolyte solution, and then mixing the aqueous electrolyte solution with a small molecular weight PEG and stirring them thoroughly to obtain the aqueous electrolyte of the supercapacitor.
[0014] The present invention further provides application of the aqueous electrolyte of the supercapacitor in the supercapacitor.
[0015] The supercapacitor includes electrode material, current collector, diaphragm and electrolyte; the supercapacitor includes electrode material, current collector, diaphragm and electrolyte; the center of the aqueous supercapacitor is the diaphragm, and the two sides are electrode material and current collector from the inside to the outside.
[0016] The electrode material is activated carbon; the current collector is any one of nickel foam, aluminum foil or stainless steel foil; the diaphragm is a cellulose diaphragm or a glass fiber diaphragm; and the electrolyte is an aqueous electrolyte of any supercapacitor described in claims 1-5.
[0017] The center of the water-based supercapacitor of the present invention is a diaphragm, and the two sides are electrode materials and current collectors from the inside to the outside; the electrolyte is the water-based electrolyte described in the above scheme. The water-based supercapacitor provided by the present invention can work safely and has a wide temperature application range. The method provided by the present invention is simple, the materials are cheap and easy to obtain, the assembly method is simple, the cost is low, and it is conducive to mass production and application.
[0018] The aqueous electrolyte provided by the present invention has a high electrochemical stability window, is safe, pollution-free, non-corrosive, has a simple preparation method, is low-cost, and is conducive to mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a linear sweep voltammetric comparison diagram of the aqueous electrolyte of Example 1 and the aqueous electrolyte of the comparative example without adding the small molecular weight PEG;
[0020] Figure 2 It is a comparison diagram of constant current charge and discharge curves of the aqueous electrolytes of Examples 2 and 3 at a current density of 1 A / g under a three-electrode test;
[0021] Figure 3 It is a comparison chart of the cycle performance curves of the button-type supercapacitor based on aqueous electrolyte in Examples 4, 5, 6 and their comparative examples under a voltage window of 2V. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0023] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs, and the disclosure and materials cited therein are hereby incorporated by reference.
[0024] Technical equivalents to the specific embodiments described that are apparent to those skilled in the art using no more than routine experimentation are intended to be encompassed by this application.
[0025] The experimental methods in the following examples are all conventional methods unless otherwise specified. The instruments and equipment used in the following examples are all conventional laboratory instruments and equipment unless otherwise specified; the experimental materials used in the following examples are all purchased from conventional biochemical reagent stores unless otherwise specified.
[0026] Example 1: Sodium sulfate with an aqueous electrolyte concentration of 1 mol / L is dissolved in 90 wt% deionized water to form an electrolyte aqueous solution, and then 10 wt% PEG-200 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 1M Na2SO4-10%PEG200.
[0027] Comparative Example: Sodium sulfate with a concentration of 1 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 1M Na2SO4.
[0028] Example 2: Lithium sulfate with an aqueous electrolyte concentration of 0.5 mol / L is dissolved in 95 wt% deionized water to form an electrolyte aqueous solution, and then 5 wt% PEG-200 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M Li2SO4-5%PEG200.
[0029] Comparative Example: Lithium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M Li2SO4.
[0030] Example 3: Lithium sulfate with an aqueous electrolyte concentration of 0.5 mol / L is dissolved in 97 wt% deionized water to form an electrolyte aqueous solution, and then 3 wt% PEG-200 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M Li2SO4-3%PEG200.
[0031] Comparative Example: Lithium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M Li2SO4.
[0032] Example 4: Potassium sulfate with an aqueous electrolyte concentration of 0.5 mol / L is dissolved in 95 wt% deionized water to form an electrolyte aqueous solution, and then 5 wt% PEG-200 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M K2SO4-5%PEG200.
[0033] Comparative Example: Potassium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M K2SO4.
[0034] Example 5: Potassium sulfate with a concentration of 0.5 mol / L of aqueous electrolyte is dissolved in 97 wt% deionized water to form an electrolyte aqueous solution, and then 3 wt% PEG-200 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M K2SO4-3%PEG200.
[0035] Comparative Example: Potassium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M K2SO4.
[0036] Example 6: Potassium sulfate with a concentration of 0.5 mol / L of aqueous electrolyte is dissolved in 99 wt% of deionized water to form an electrolyte aqueous solution, and then 1 wt% of PEG-200 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M K2SO4-1%PEG200.
[0037] Comparative Example: Potassium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M K2SO4.
[0038] Example 7: Sodium sulfate with a concentration of 0.5 mol / L of aqueous electrolyte is dissolved in 97 wt% deionized water to form an electrolyte aqueous solution, and then 3 wt% PEG-200 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M Na2SO4-3%PEG200.
[0039] Comparative Example: Sodium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M Na2SO4.
[0040] Example 8: Sodium sulfate with a concentration of 0.5 mol / L of aqueous electrolyte is dissolved in 99 wt% of deionized water to form an electrolyte aqueous solution, and then 1 wt% of PEG-200 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M Na2SO4-1%PEG200.
[0041] Comparative Example: Sodium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M Na2SO4.
[0042] Example 9: Magnesium sulfate with an aqueous electrolyte concentration of 0.5 mol / L is dissolved in 95 wt% deionized water to form an electrolyte aqueous solution, and then 5 wt% PEG-200 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M MgSO4-5%PEG200.
[0043] Comparative Example: Magnesium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M MgSO4.
[0044] Example 10: Zinc sulfate with an aqueous electrolyte concentration of 1 mol / L is dissolved in 95 wt% deionized water to form an electrolyte aqueous solution, and then 5 wt% PEG-200 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 1M ZnSO4-5%PEG200.
[0045] Comparative Example: Zinc sulfate with a concentration of 1 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M ZnSO4.
[0046] Example 11: Aluminum sulfate with an aqueous electrolyte concentration of 1 mol / L is dissolved in 95 wt% deionized water to form an electrolyte aqueous solution, and then 5 wt% PEG-200 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 1M Al2(SO4)3-5%PEG200.
[0047] Comparative Example: Aluminum sulfate with a concentration of 1 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 1MAl2(SO4)3.
[0048] Example 12: Potassium sulfate with a concentration of 0.5 mol / L of aqueous electrolyte is dissolved in 95 wt% of deionized water to form an electrolyte aqueous solution, and then 5 wt% of PEG-300 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M K2SO4-5%PEG300.
[0049] Comparative Example: Potassium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M K2SO4.
[0050] Example 13: Potassium sulfate with a concentration of 0.5 mol / L of aqueous electrolyte is dissolved in 95 wt% of deionized water to form an electrolyte aqueous solution, and then 5 wt% of PEG-400 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M K2SO4-5%PEG400.
[0051] Comparative Example: Potassium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M K2SO4.
[0052] Example 14: Potassium sulfate with a concentration of 0.5 mol / L of aqueous electrolyte is dissolved in 95 wt% of deionized water to form an electrolyte aqueous solution, and then 5 wt% of PEG-600 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M K2SO4-5%PEG600.
[0053] Comparative Example: Potassium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M K2SO4.
[0054] Example 15: Sodium sulfate with a concentration of 0.5 mol / L of aqueous electrolyte is dissolved in 95 wt% of deionized water to form an electrolyte aqueous solution, and then 5 wt% of PEG-300 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M Na2SO4-5%PEG300.
[0055] Comparative Example: Sodium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M Na2SO4.
[0056] Example 16: Lithium sulfate with a concentration of 0.5 mol / L of aqueous electrolyte is dissolved in 95 wt% of deionized water to form an electrolyte aqueous solution, and then 5 wt% of PEG-300 is mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M Li2SO4-5%PEG300.
[0057] Comparative Example: Lithium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M Li2SO4.
[0058] Example 17: Dissolve magnesium sulfate with an aqueous electrolyte concentration of 0.5 mol / L in 95 wt% deionized water to form an electrolyte aqueous solution, and then mix 3 wt% PEG-400 with the electrolyte aqueous solution and stir them thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M MgSO4-5%PEG400.
[0059] Comparative Example: Magnesium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M MgSO4.
[0060] Example 18: Dissolve zinc sulfate with an aqueous electrolyte concentration of 1 mol / L in 95 wt% deionized water to form an electrolyte aqueous solution, and then mix 5 wt% PEG-400 with the electrolyte aqueous solution and stir them thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 1M ZnSO4-5%PEG400.
[0061] Comparative Example: Zinc sulfate with a concentration of 1 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 1MZnSO4.
[0062] Example 19: Potassium sulfate with a concentration of 0.5 mol / L of aqueous electrolyte is dissolved in 94 wt% deionized water to form an electrolyte aqueous solution, and then 3 wt% PEG-200 and 3 wt% PEG-300 are mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5MK2SO4-3%PEG200-3%PEG300.
[0063] Comparative Example: Potassium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M K2SO4.
[0064] Example 20: Sodium sulfate with a concentration of 1 mol / L of aqueous electrolyte is dissolved in 90 wt% of deionized water to form an electrolyte aqueous solution, and then 5 wt% of PEG-200 and 5 wt% of PEG-300 are mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 1MNa2SO4-5%PEG200-5%PEG300.
[0065] Comparative Example: Sodium sulfate with a concentration of 1 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M Na2SO4.
[0066] Example 21: Lithium sulfate with an aqueous electrolyte concentration of 1 mol / L is dissolved in 90 wt% deionized water to form an electrolyte aqueous solution, and then 5 wt% PEG-200 and 5 wt% PEG-300 are mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 1MLi2SO4-5%PEG200-5%PEG300.
[0067] Comparative Example: Dissolve 1 mol / L lithium sulfate in deionized water to form an electrolyte solution, recorded as 1MLi2SO4
[0068] Example 22: Potassium sulfate with a concentration of 0.5 mol / L of aqueous electrolyte is dissolved in 94 wt% deionized water to form an electrolyte aqueous solution, and then 3 wt% PEG-200 and 3 wt% PEG400 are mixed with the electrolyte aqueous solution and stirred thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5MK2SO4-3%PEG200-3%PEG400.
[0069] Comparative Example: Potassium sulfate with a concentration of 0.5 mol / L was dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5 M K2SO4.
[0070] Example 23: Dissolve 0.5 mol / L of lithium sulfate and 0.5 mol / L of sodium sulfate in 90 wt% deionized water to form an aqueous electrolyte solution, and then mix 10 wt% PEG-200 with the aqueous electrolyte solution and stir them thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5MLi2SO4+0.5M Na2SO4-10%PEG200.
[0071] Comparative Example: 0.5 mol / L lithium sulfate and 0.5 mol / L sodium sulfate were dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5M Li2SO4+0.5M Na2SO4.
[0072] Example 24: Dissolve 0.5 mol / L of lithium sulfate and 0.5 mol / L of potassium sulfate in 95 wt% deionized water to form an aqueous electrolyte solution, and then mix 5 wt% PEG-200 with the aqueous electrolyte solution and stir them thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5MLi2SO4+0.5M K2SO4-5%PEG200.
[0073] Comparative Example: 0.5 mol / L lithium sulfate and 0.5 mol / L potassium sulfate were dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5M Li2SO4+0.5M K2SO4.
[0074] Example 25: Dissolve 0.5 mol / L of lithium sulfate and 0.5 mol / L of sodium sulfate in 90 wt% deionized water to form an aqueous electrolyte solution, then mix 5 wt% PEG-200 and 5 wt% PEG300 with the aqueous electrolyte solution and stir them thoroughly to obtain one of the aqueous electrolytes provided by the present invention, recorded as 0.5M Li2SO4+0.5M Na2SO4-5%PEG200-5%PEG300.
[0075] Comparative Example: 0.5 mol / L lithium sulfate and 0.5 mol / L sodium sulfate were dissolved in deionized water to form an electrolyte aqueous solution, recorded as 0.5M Li2SO4+0.5M Na2SO4.
[0076] The aqueous electrolyte prepared by the present invention has been tested to have a wider electrochemical stability window. Figure 1 As shown, a glassy carbon electrode is used as a working electrode, a platinum mesh is used as a counter electrode, and a saturated calomel electrode is used as a reference electrode. Compared with a 1M Na2SO4 electrolyte, after adding 10wt% PEG, the electrochemical window displayed by LSV is widened from the previous -2.1~2V to -2.1~2.2V. When the aqueous electrolyte described in Example 4 and the corresponding comparative electrolyte are subjected to LSV testing, the electrochemical window is widened from the previous -2.2~2.1V to -2.5~2.1V.
[0077] When the prepared aqueous electrolyte was used for the three-electrode test, YP-50F activated carbon, super P conductive carbon black and polytetrafluoroethylene binder were mixed into a slurry in a mass ratio of 8:1:1, anhydrous ethanol was added for dispersion, and the mixture was ground for 20 minutes and evenly coated on the nickel foam substrate with a coating area of 1 cm. 2 The coating mass is 4-6 mg, placed in a vacuum oven at 80 ° C for 12 hours, and finally pressed into a working electrode using a tablet press. The counter electrode is a 1×1 cm platinum mesh, and the reference electrode is a saturated calomel electrode. Under the three-electrode test, the current density is 1A g -1 The constant current charge and discharge comparison diagram is as follows Figure 2 As shown, the selected aqueous electrolytes all have good specific capacitance under the three-electrode test.
[0078] The aqueous supercapacitor described in the present invention is a button-type supercapacitor, the center of the button-type supercapacitor is a diaphragm, and the two sides are electrode materials and current collectors from the inside to the outside; the electrolyte is the aqueous electrolyte described in the above scheme. The electrode material is YP-50F activated carbon. YP-50F activated carbon, super P conductive carbon black and polytetrafluoroethylene binder are mixed into a slurry according to a mass ratio of 8:1:1, anhydrous ethanol is added for dispersion, and the mixture is ground for 20 minutes. The mixture is evenly coated on a circular nickel foam substrate with a diameter of 1.2 cm, and the coating mass is 4-6 mg. The mixture is placed in a vacuum oven at 80°C and dried for 12 hours. Finally, the mixture is pressed with a tablet press, and two pole pieces with the same mass of active materials are selected. The pieces are assembled in the order of positive electrode shell-positive electrode piece-diaphragm-negative electrode piece-stainless steel gasket-spring-negative electrode shell, and an aqueous electrolyte described in the present invention is added. The amount of the electrolyte is 50-150 μL. The assembled button-type supercapacitor is tested for its cycle performance using a Xinwei battery test cabinet, as shown in FIG. Figure 3 As shown, it is a comparison diagram of the cycle performance curves of button-type supercapacitors based on aqueous electrolytes in a 2V voltage window. As shown in the figure, the aqueous electrolyte after adding PEG has better cycle performance than 0.5M K2SO4 in a 2V voltage window, among which the 0.5M K2SO4-3%PEG aqueous electrolyte has the best cycle performance. The aqueous electrolyte provided by the present invention still has good cycle performance and rate performance while improving the electrochemical stability window.
[0079] Table 1 lists the experimental parameters and results of some examples. The electrolytes described in the examples in the table were all prepared at room temperature, and button-type supercapacitors were used to test the cycle performance.
[0080] Table 1
[0081]
[0082] Through the above embodiments, the aqueous electrolyte provided by the present invention has better safety and a wide electrochemical stability window, and the aqueous supercapacitor based on the electrolyte of the present invention has good cycle performance and capacitance behavior, and has a higher energy density than other aqueous electrolytes. The embodiments described are only preferred embodiments of the present invention.
[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. An aqueous electrolyte for a supercapacitor, Features: It is prepared from electrolyte, water and low molecular weight polyethylene glycol PEG; wherein: the electrolyte is sulfate, and the low molecular weight PEG is one or more of the number average molecular weight Mn=200-600 mixed in any proportion; The electrolyte is lithium sulfate with a molar concentration of 0.2-2 mol / L in an aqueous electrolyte, sodium sulfate with a molar concentration of 0.1-1 mol / L in an aqueous electrolyte, potassium sulfate with a molar concentration of 0.1-0.5 mol / L in an aqueous electrolyte, magnesium sulfate with a molar concentration of 0.2-1 mol / L in an aqueous electrolyte, zinc sulfate with a molar concentration of 0.2-1.5 mol / L in an aqueous electrolyte, or aluminum sulfate with a molar concentration of 0.1-1 mol / L in an aqueous electrolyte; The mass percentage of low molecular weight PEG in the aqueous electrolyte is 1-20%.
2. The aqueous electrolyte for supercapacitor according to claim 1, Features: The electrolyte is lithium sulfate with a molar concentration of 0.5-1.5 mol / L in an aqueous electrolyte, sodium sulfate with a molar concentration of 0.5-1 mol / L in an aqueous electrolyte, potassium sulfate with a molar concentration of 0.2-0.5 mol / L in an aqueous electrolyte, magnesium sulfate with a molar concentration of 0.5-1 mol / L in an aqueous electrolyte, zinc sulfate with a molar concentration of 0.5-1.5 mol / L in an aqueous electrolyte, or aluminum sulfate with a molar concentration of 0.5-1 mol / L in an aqueous electrolyte.
3. The aqueous electrolyte for supercapacitor according to claim 1, Features: The mass fraction of low molecular weight PEG in the electrolyte is 1-10%.
4. A method for preparing an aqueous electrolyte for a supercapacitor according to any one of claims 1 to 3, Features: First, deionized water and low molecular weight PEG are mixed in proportion, and then the electrolyte is dissolved in the mixed solvent and stirred thoroughly to obtain the aqueous electrolyte of the supercapacitor.
5. A method for preparing an aqueous electrolyte for a supercapacitor according to any one of claims 1 to 3, Features: First, the electrolyte is dissolved in water to form an aqueous electrolyte solution, and then the aqueous electrolyte solution is mixed with a small molecular weight PEG and stirred thoroughly to obtain an aqueous electrolyte for the supercapacitor.
6. Use of the aqueous electrolyte of any supercapacitor according to claim 1 to claim 3 in a supercapacitor.
7. The use according to claim 6, Features: The supercapacitor comprises electrode materials, current collectors, diaphragms and electrolytes. The center of the aqueous supercapacitor is the diaphragm, and the two sides are electrode materials and current collectors from the inside to the outside.
8. The use according to claim 7, Features: The electrode material is activated carbon; the current collector is any one of nickel foam, aluminum foil or stainless steel foil; the diaphragm is a cellulose diaphragm or a glass fiber diaphragm; The electrolyte is an aqueous electrolyte for the supercapacitor according to any one of claims 1 to 3.