Wide-temperature flame-retardant electrolyte as well as preparation method and application thereof
By synthesizing TFNP as a diluent under concentrated sulfuric acid catalyzed, the problems of flammability and interface instability of lithium-ion battery electrolyte are solved, efficient and safe electrochemical performance in a wide temperature range is achieved, and the viscosity and cost of the electrolyte are reduced. Improves the Coulomb efficiency and life of lithium-ion batteries.
Patent Information
- Application Number
- CN202310643820.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-12-03
AI Technical Summary
The electrolyte of traditional lithium-ion battery is flammable and explosive, the interface between the electrolyte and the positive and negative electrode materials is unstable, and the high concentration electrolyte has problems of high viscosity and high cost, making it difficult to effectively use within a wide temperature range.
Using hydrothermal synthesis method to prepare 1,1,2,2-tetrafluoro-3-nitropropane (TFNP) under concentrated sulfuric acid catalytic conditions to form a local high concentration electrolyte. Combining specific steps and material ratios, wide temperatures are prepared Flame-retardant liquid electrolyte.
It improves the electrochemical stability and safety performance of the electrolyte, reduces viscosity and cost, enhances the Coulomb efficiency and life of lithium-ion batteries, and ensures the normal operation of the battery in a wide temperature range.
Abstract
Description
(I) Technical field
[0001] The invention belongs to the technical field of lithium ion battery liquid electrolytes, and in particular relates to a wide-temperature flame-retardant liquid electrolyte and a preparation method thereof. (II) Background technology
[0002] As an efficient, environmentally friendly and renewable energy storage technology, lithium-ion batteries have been widely used in digital electronics, portable mobile devices, electric vehicles and energy storage. Lithium-ion batteries are mainly composed of positive and negative electrodes, separators and electrolytes, among which the electrolyte is called the "blood" of lithium-ion batteries. The electrolyte has high lithium ion conductivity and good wettability. The electrolyte of traditional lithium batteries is mainly composed of carbonate organic solvents, which have various problems such as flammability and explosion, unstable interface between electrolyte and positive and negative electrode materials. The use of a new solvent system (local high concentration electrolyte, LHCEs) can effectively solve the above problems. It can not only avoid the safety hazards brought by traditional liquid electrolytes, but also support the normal operation of lithium batteries in a wide temperature range (-40℃-60℃). Therefore, lithium-ion batteries using local high concentration electrolytes have become the development direction of the new generation of lithium-ion batteries.
[0003] In low-concentration electrolytes, lithium salts are dissociated and form solvent-separated ion pairs (SSIPs) with the solvent. + It does not interact with anions, but is wrapped by solvent molecules, resulting in Li + The desolvation process is very difficult. By increasing the electrolyte concentration, the free solvent molecules are depleted and Li + The anions form solvated complexes, namely contact ion pairs (CIPs) and aggregates (AGGs), which are interconnected to form a three-dimensional network structure, resulting in the high-concentration electrolyte having the disadvantages of high viscosity and poor wettability. At this time, adding a diluent to it can form a local high-concentration electrolyte. The function of the diluent is to dilute or disperse these large clusters, so that Li + -Solvent-anion groups are easy to move. By using a diluent, the concentration of the electrolyte can be reduced to form a local high-concentration electrolyte. While ensuring the same solvent-lithium salt coordination structure as the high-concentration electrolyte, the negative effects of the high cost, high viscosity, and low wettability of the high-concentration electrolyte can be alleviated.
[0004] Therefore, the release agent needs to have low viscosity, high redox stability and non-flammability to maintain the advantages of high electrochemical stability of high-concentration electrolytes and overcome the disadvantages of high viscosity and high cost of high-concentration electrolytes. At present, hydrofluoroethers meet the above characteristics and are a suitable diluent. After research, local high-concentration electrolytes using hydrofluoroethers as additives have excellent performance and overcome a series of shortcomings of low-concentration electrolytes. However, the preparation of hydrofluoroethers is very difficult, making them too expensive, even higher than the sum of lithium salts and solvents, which runs counter to the reason for choosing diluents in the first place. (III) Summary of the invention
[0005] In view of the problems existing in the above background technology, the present invention aims to overcome the shortcomings of the above prior art and provide a method for synthesizing a novel fluorine-containing diluent, which is prepared by a hydrothermal synthesis method, and tetrafluoropropanol is converted into a novel diluent 1,1,2,2-tetrafluoro-3-nitropropane (TFNP) having a local polar structure (-NO2) under the catalytic condition of concentrated sulfuric acid. The polar lithiophilic segment (i.e. -NO2) can protect Li + , while the fluorinated lithium-phobic segment (i.e., -CF2CF2H) not only has high pressure resistance but also acts as an inert diluent to maintain the local anion-rich solvation structure.
[0006] To achieve the above object, the present invention provides a method for preparing a solid electrolyte of a reinforced concrete-like structure, characterized in that it comprises the following steps:
[0007] (1) Preparation of diluent TFNP (1,1,2,2-tetrafluoro-3-nitropropane): In an ice-water bath, prepare a mixed solution of concentrated sulfuric acid and concentrated nitric acid, add tetrafluoropropanol, keep the temperature below 15°C, and react for 2 hours under magnetic stirring. Then, add ice water, and after the temperature of the reaction system stabilizes, add sodium hydroxide solution to adjust the pH to neutral. Add the mixture system to a separatory funnel, separate the liquids, and the upper organic phase is the reaction product. Finally, transfer the product to a beaker, dry it in a vacuum oven, and then transfer it to a glove box to obtain TFNP.
[0008] (2) Dehydration of solvents and additives: Place 4A molecular sieve in a muffle furnace and heat it according to a certain temperature increase program for activation, then transfer it to a glove box while it is still hot and seal it for storage. After the temperature of the molecular sieve stabilizes, add the molecular sieve to the solvent / additive at a mass ratio of molecular sieve: solvent / additive = 1:4, and let it stand for 24 hours.
[0009] (3) Preparation of electrolyte: In a glove box with water and oxygen content less than 1 ppm, the solvent after dehydration is added to an aluminum bottle, followed by lithium salt and TFNP, and finally a small amount of additives. After magnetic stirring for a period of time, the solution is allowed to stand for a long time to obtain a local high-concentration electrolyte.
[0010] Preferably, the volume ratio of concentrated sulfuric acid to concentrated nitric acid in step (1) is 4:1 to 1:1.
[0011] Preferably, the mass ratio of tetrafluoropropanol in step (1) to the mixed acid solution is 5-20wt%.
[0012] Preferably, the reaction temperature in step (1) is 0-10°C.
[0013] Preferably, the proportion of ice water added in step (1) is 50-100% of the reaction mixture.
[0014] Preferably, the key parameters of the vacuum drying in the vacuum oven described in step (1) are: drying temperature of 60 to 90° C. and drying time of 16 to 24 hours.
[0015] Preferably, the heating program rate in step (2) is 5°C / min from room temperature to 350°C, kept at this temperature for 16 to 24 hours, and then naturally cooled to 200°C for hot transfer.
[0016] Preferably, the solvent in step (3) is one of ethylene glycol dimethyl ether, triethyl phosphate, dimethyl sulfoxide, ethylene carbonate or a combination thereof.
[0017] Preferably, the lithium salt described in step (3) is one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium hexafluorophosphate, lithium perchlorate, lithium oxalate difluoroborate, lithium tetrafluoroborate, or a combination thereof.
[0018] Preferably, the additive in step (3) is one or a combination of propylene carbonate, fluoroethylene carbonate, vinyl sulfate, and ethanedinitrile.
[0019] Preferably, the mass fraction of the lithium salt in step (3) is 15-25wt%, the mass fraction of the solvent is 15-25wt%, the mass fraction of the diluent is 50-75wt%, and the mass fraction of the additive is 1-3wt%.
[0020] Preferably, the stirring time in step (3) is 12 to 24 hours, the magnetic stirring speed is 600 to 800 rpm, and the standing time is 12 to 24 hours.
[0021] Due to the adoption of the above technical solution, the wide temperature flame retardant electrolyte of the present invention has the following characteristics:
[0022] (1) The introduction of a high-concentration electrolyte system solves problems such as the instability of the interface between the electrolyte and the positive and negative electrodes, greatly improves the Coulomb efficiency and inhibits the growth of lithium dendrites.
[0023] (2) The self-synthesized diluent TFNP reduces the high cost and high viscosity problems caused by high-concentration electrolytes and maintains the high electrochemical stability of the electrolyte.
[0024] (3) The high mass ratio of TFNPs greatly improves the electrochemical stability window of the electrolyte and ensures the non-flammability of the electrolyte, thereby improving the safety performance of the battery.
[0025] (4) The local polar structure of TFNP with a high mass ratio can protect lithium ions and anions, making the desolvation of lithium ions easier during charging and discharging, greatly improving the battery life.
[0026] The above four characteristics make the prepared wide-temperature flame-retardant electrolyte have more excellent electrochemical properties, playing a key role in the continuous development of liquid lithium-ion batteries. (IV) Description of the drawings
[0027] none
[0028] (V) Specific implementation methods
[0029] The present invention will be further described below in conjunction with specific embodiments.
[0030] Example 1
[0031] (1) Preparation of diluent TFNP (1,1,2,2-tetrafluoro-3-nitropropane): In an ice-water bath, prepare a mixed solution of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1, add 15wt% tetrafluoropropanol, keep the temperature below 5°C, and react for 2 hours under magnetic stirring. Then, add 100% ice water. After the temperature of the reaction system stabilizes, add sodium hydroxide solution to adjust the pH to neutral. Add the mixture system to a separatory funnel, separate the liquids, and the upper organic phase is the reaction product. Finally, transfer the product to a beaker, dry it in a vacuum oven at 80°C for 24 hours, and then transfer it to a glove box to obtain TFNP.
[0032] (2) Dehydration of solvent and additive: Place 4A molecular sieve in a muffle furnace and heat it from room temperature to 350°C at a heating rate of 5°C / min, keep it at this temperature for 16 hours, then cool it naturally to 200°C and transfer it to a glove box while it is hot and seal it for storage. After the temperature of the molecular sieve stabilizes, add the molecular sieve to the solvent / additive at a mass ratio of molecular sieve: solvent / additive = 1:4, and let it stand for 24 hours.
[0033] (3) Preparation of electrolyte: In a glove box with water and oxygen content less than 1 ppm, add the solvent ethylene glycol dimethyl ether after dehydration into an aluminum bottle, then add lithium hexafluorophosphate (LiPF6) and TFNP, and finally add fluoroethylene carbonate. After magnetic stirring for 12 hours, let it stand for 12 hours to prepare a local high-concentration electrolyte.
[0034] Example 2
[0035] (1) Same as Example 1
[0036] (2) Same as Example 1
[0037] (3) Preparation of electrolyte: In a glove box with water and oxygen content less than 1 ppm, the solvent triethyl phosphate after dehydration was added to an aluminum bottle, followed by lithium hexafluorophosphate (LiPF6) and TFNP, and finally fluoroethylene carbonate. After magnetic stirring for 12 hours, the mixture was allowed to stand for 12 hours to obtain a local high-concentration electrolyte.
[0038] Example 3
[0039] (1) Same as Example 1
[0040] (2) Same as Example 1
[0041] (3) Preparation of electrolyte: In a glove box with water and oxygen content less than 1 ppm, the solvent triethyl phosphate after dehydration was added to an aluminum bottle, followed by lithium hexafluorophosphate (LiPF6) and TFNP, and finally ethylenediamine. After magnetic stirring for 12 hours, the mixture was allowed to stand for 12 hours to obtain a local high-concentration electrolyte.
[0042] Example 4
[0043] (1) Preparation of diluent TFNP (1,1,2,2-tetrafluoro-3-nitropropane): In an ice-water bath, prepare a mixed solution of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 2:1, add 20wt% tetrafluoropropanol, keep the temperature below 5°C, and react for 2 hours under magnetic stirring. Then, add 100% ice water. After the temperature of the reaction system stabilizes, add sodium hydroxide solution to adjust the pH to neutral. Add the mixture system to a separatory funnel, separate the liquids, and the upper organic phase is the reaction product. Finally, transfer the product to a beaker, dry it in a vacuum oven at 60°C for 24 hours, and then transfer it to a glove box to obtain TFNP.
[0044] (2) Same as Example 1
[0045] (3) Same as Example 1
[0046] Example 5
[0047] (1) Same as Example 1
[0048] (2) Same as Example 1
[0049] (3) Preparation of electrolyte: In a glove box with water and oxygen content less than 1 ppm, the solvent ethylene glycol dimethyl ether after dehydration was added to an aluminum bottle, followed by lithium bis(fluorosulfonyl)imide (LiFSI) and TFNP, and finally ethanedinitrile. After magnetic stirring for 12 hours, the mixture was allowed to stand for 12 hours to obtain a local high-concentration electrolyte.
[0050] Example 6
[0051] (1) Preparation of diluent TFNP (1,1,2,2-tetrafluoro-3-nitropropane): In an ice-water bath, prepare a mixed solution of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 4:1, add 10wt% tetrafluoropropanol, keep the temperature below 10°C, and react for 2 hours under magnetic stirring. Then, add 50% ice water. After the temperature of the reaction system stabilizes, add sodium hydroxide solution to adjust the pH to neutral. Add the mixture system to a separatory funnel, separate the liquids, and the upper organic phase is the reaction product. Finally, transfer the product to a beaker, dry it in a vacuum oven at 65°C for 24 hours, and then transfer it to a glove box to obtain TFNP.
[0052] (2) Same as Example 1
[0053] (3) Same as Example 1
[0054] Example 7
[0055] (1) Same as Example 1
[0056] (2) Same as Example 1
[0057] (3) Preparation of electrolyte: In a glove box with water and oxygen content less than 1 ppm, the solvent dimethyl sulfoxide after dehydration was added to an aluminum bottle, followed by the addition of lithium bis(fluorosulfonyl)imide (LiFSI) and TFNP, and finally fluoroethylene carbonate. After magnetic stirring for 12 hours, the mixture was allowed to stand for 12 hours to obtain a local high-concentration electrolyte.
[0058] Example 8
[0059] (1) Same as Example 1
[0060] (2) Same as Example 1
[0061] (3) Preparation of electrolyte: In a glove box with water and oxygen content less than 1 ppm, add the solvent ethylene carbonate after dehydration into an aluminum bottle, then add lithium bis(fluorosulfonyl)imide (LiFSI) and TFNP, and finally add fluoroethylene carbonate. After magnetic stirring for 12 hours, let it stand for 12 hours to prepare a local high-concentration electrolyte.
[0062] Example 9
[0063] (1) Same as Example 1
[0064] (2) Same as Example 1
[0065] (3) Preparation of electrolyte: In a glove box with water and oxygen content less than 1 ppm, add the solvent ethylene carbonate after dehydration into an aluminum bottle, then add lithium bis(fluorosulfonyl)imide (LiFSI) and TFNP, and finally add fluoroethylene carbonate and ethylene glycol dimethyl ether. After magnetic stirring for 12 hours, let it stand for 12 hours to obtain a local high-concentration electrolyte. Use of a wide-temperature flame-retardant electrolyte of the present invention: Used in liquid lithium-ion batteries.
Claims
1. A method for preparing a wide temperature flame retardant electrolyte, the specific preparation method comprising the following steps: (1) Preparation of diluent TFNP (1,1,2,2-tetrafluoro-3-nitropropane): In an ice-water bath, prepare a mixed solution of concentrated sulfuric acid and concentrated nitric acid, add tetrafluoropropanol, keep the temperature below 5°C, and react for 2 hours under magnetic stirring. Then, add ice water, and after the temperature of the reaction system stabilizes, add sodium hydroxide solution to adjust the pH to neutral. Add the mixture system to a separatory funnel, separate the liquids, and the upper organic phase is the reaction product. Finally, transfer the product to a beaker, dry it in a vacuum oven, and then transfer it to a glove box to obtain TFNP. (2) Dehydration of solvents and additives: Place 4A molecular sieve in a muffle furnace and heat it according to a certain temperature increase program for activation, then transfer it to a glove box while it is still hot and seal it for storage. After the temperature of the molecular sieve stabilizes, add the molecular sieve to the solvent / additive at a mass ratio of molecular sieve: solvent / additive = 1:4, and let it stand for 24 hours. (3) Preparation of electrolyte: In a glove box with water and oxygen content less than 1 ppm, the solvent triethyl phosphate (TEP) after dehydration was added to an aluminum bottle, followed by lithium hexafluorophosphate (LiPF6) and TFNP, and finally fluoroethylene carbonate (FEC). After magnetic stirring for 12 hours, the mixture was allowed to stand for 12 hours to obtain a local high-concentration electrolyte.
2. The method according to claim 1, characterized in that: In the step (1), the volume ratio of concentrated sulfuric acid to concentrated nitric acid is 2:1, and the added mass proportion of tetrafluoropropanol is 15wt%.
3. The method according to claim 1, characterized in that: The mass ratio of ice water added in step (1) is 100%, and the mass fraction of sodium hydroxide solution is 20%.
4. The method according to claim 1, characterized in that: The key parameters of the vacuum oven are: oven temperature is 80°C and drying time is 24 hours.
5. The method according to claim 1, characterized in that: In the step (2), the temperature of the muffle furnace is raised from room temperature to 350°C at a heating rate of 5°C / min, kept at this temperature for 16 hours, and then naturally cooled to 200°C for removal.
6. The method according to claim 1, characterized in that: In the step (3), the mass ratio of LiPF6, TEP and TFNP is 1:1:
3.
7. The method according to claim 1, characterized in that: The mass percentage of FEC added in step (3) is 5wt%.