Preparation process and application of glass sensor with double-sided simultaneous exposure, development and etching

Through simultaneous double-sided exposure, development, etching process and printing silver paste technology, problems such as scratches and disconnections in the glass sensor process are solved, the process yield and electrical yield are improved, the process flow is simplified, and the production cost is reduced. cost.

CN114594662BActive Publication Date: 2024-10-29牧东光电科技有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210286281.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-23
Publication Date
2024-10-29
Estimated Expiration
2042-03-23

AI Technical Summary

Technical Problem

There are appearance and functional problems such as scratches, foreign objects, broken wires, and unclean etching in the existing glass sensor manufacturing process, resulting in low process yield and increased production costs and loss of manpower and material resources.

Method used

It adopts a glass sensor preparation process of simultaneous double-sided exposure, development, and etching. By setting up UV-Cut coating and printing silver paste processes, mutual influence during double-sided exposure is avoided. The yellow light process for edge routing is cancelled, and all the components are formed directly by laser. No lines are needed to simplify the process.

Benefits of technology

The appearance yield rate has been improved to 95%, functional problems such as wire breakage and dirty etching have been solved, and the electrical yield rate has been increased to 98%, which reduces production costs, simplifies the preparation process, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114594662B_ABST
    Figure CN114594662B_ABST
Patent Text Reader

Abstract

The present invention relates to a preparation process of a glass sensor with double-sided simultaneous exposure, development and etching: cleaning glass → setting UV-Cut coating → preparing ITO glass → double-sided photoresist coating → double-sided exposure and development of ITO glass → double-sided etching of ITO glass → printing and laser edge routing → printing peelable adhesive. A novel glass sensor is also provided, which is made by the above-mentioned preparation process. The present invention realizes simultaneous exposure, development and etching on both sides of the glass by setting UV-Cut coating, which can avoid mutual influence of ITO exposure during double-sided exposure, and can effectively prevent scratches, foreign matter and other poor appearance caused by two etching processes on one side, and the appearance yield is increased from 80% to 95%; the yellow light process of edge routing is cancelled, and the printing silver paste process is adopted, without etching, and functional problems such as broken wires and incomplete etching are solved, and the electrical yield is increased from 90% to 98%; the preparation process is simplified, the production efficiency is improved, and the production cost is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of touch screens, and in particular to a preparation process and application of a glass sensor with double-sided simultaneous exposure, development and etching. Background Art

[0002] At present, in order to ensure better safety and higher strength, a large part of touch screens in the automotive and industrial control fields still use glass sensors as functional layer structures. In the existing glass sensor manufacturing process, Mo-Al-Mo is used as the conductive material for edge routing, and the minimum line width and line spacing is only 20um / 20um. Since the concentration of Mo-Al-Mo etching solution is difficult to control within a relatively stable range, when the etching solution concentration is too high, the edge routing will have side etching, that is, over-etching, which will cause the edge routing to break in severe cases; when the etching solution concentration is too low, the edge routing will be not etched cleanly, which will cause the edge routing to be connected in severe cases, and there will be problems such as side etching, broken wires, unclean etching, and connection, and the electrical yield is low. In addition, the two sides of the ITO glass need to be exposed, developed, and etched separately during the preparation process, which is easy to cause scratches, foreign matter and other poor appearance consequences, and the yield is low, generally between 70% and 80%. All of these cause loss of manpower and material resources and increase production costs. Summary of the invention

[0003] The present invention provides a novel glass sensor preparation method, the purpose of which is to solve the appearance and functional problems such as scratches, foreign matter, broken wires, and unclean etching in the existing glass sensor manufacturing process, improve the process yield, reduce the loss of manpower and material resources, reduce production costs, and simultaneously reduce the process flow to improve production efficiency.

[0004] In order to solve the above technical problems, the glass sensor preparation process of the present invention with double-sided simultaneous exposure, development and etching comprises the following steps:

[0005] Step S1: Cleaning the glass

[0006] Use a weak alkaline or neutral detergent to clean the upper and lower surfaces of the glass;

[0007] Step S2: Setting UV-Cut coating

[0008] Use a spray coating, spray coating or evaporation process to form UV-Cut coatings on the upper and lower surfaces of the glass, respectively. The upper surface of the glass is the upper UV-Cut coating, and the lower surface of the glass is the lower UV-Cut coating.

[0009] Step S3: Preparation of ITO glass

[0010] Through the magnetron sputtering process, ITO is coated on the surface of the upper UV-Cut coating and the lower UV-Cut coating, and the thickness of the ITO coating is controlled by adjusting the magnetron sputtering conditions to obtain the ITO glass with the required square resistance;

[0011] Step S4: Double-sided photoresist coating

[0012] Coating photoresist on the A and B surfaces of the ITO glass at the same time, and then baking, the baking temperature is 60°C to 120°C, and the baking time is 10min to 30min;

[0013] Step S5: Double-sided exposure and development of ITO glass

[0014] The ITO glass coated with photoresist on both sides is exposed on both sides in the designed A-side and B-side glass mask precision exposure machine, and then developed in a developer to develop the ITO pattern on the A-side and B-side. The developer is prepared with 90% solid electronic grade KOH, and then after washing with water and air drying, the liquid on the surface of the ITO glass is dried;

[0015] Step S6: Double-sided etching of ITO glass

[0016] Place the A and B surfaces of the ITO glass in an etching solution for double-sided etching, remove the ITO that is not needed for the surface pattern, and leave the ITO that is needed for the surface pattern; after washing with water and air drying, remove the photoresist on both sides in a stripping solution, the stripping solution is prepared with 99% electronic grade NaOH, and after washing with water and air drying, obtain the ITO glass with the upper and lower inner patterns;

[0017] The upper inner pattern and the lower inner pattern are a layer of patterned ITO coated on the upper and lower sides of the glass. A layer of ITO is first coated on the glass surface by magnetron sputtering, and then the required ITO pattern is obtained by exposure, development, and etching. The pattern of the ITO pattern can be a diamond, a rectangle, a square, or other regular shapes.

[0018] Step S7: Printing and lasering upper edge routing and lower edge routing

[0019] Silver paste is printed on the edge of the ITO Pattern on the A side by screen printing technology, and then baked to form a thick block silver paste, and then a high-precision laser machine is used to lased out a line with a line width and line spacing to obtain the upper edge routing; silver paste is printed on the edge of the ITO Pattern on the B side by screen printing technology, and then baked to form a thick block silver paste, and then a high-precision laser machine is used to lased out a line with a line width and line spacing to obtain the lower edge routing;

[0020] The baking temperature is 120℃~140℃, and the baking time is 10min~30min;

[0021] Conventional glass sensors use Mo-Al-Mo as the conductive material for edge routing, and the minimum line width and line spacing is only 20um / 20um. Since the concentration of Mo-Al-Mo etching solution is difficult to control within a relatively stable range, when the etching solution concentration is too high, the edge routing will be side-etched or over-etched, which may cause edge routing disconnection in severe cases. When the etching solution concentration is too low, the edge routing will not be etched cleanly, which may cause edge routing connection in severe cases.

[0022] The present invention adopts the printing silver paste process. The upper edge routing and the lower edge routing are silver paste block routing printed on the edge of the in-plane pattern using CCD precision screen printing technology. After the silver paste is baked and solidified, the silver paste circuit is lasered out under a CCD precision laser machine and certain parameters. The silver paste circuit is connected to the in-plane pattern channel. No etching is required, only baking and lasering can be used to obtain the required edge routing, which can solve the above problems of side etching, broken wires, unclean etching, and connection.

[0023] Step S8: Printing peelable adhesive

[0024] Printing a peelable adhesive on the A side by screen printing technology and baking it to form an upper peelable adhesive with thickness, and then printing a peelable adhesive on the B side by screen printing technology and baking it to form a lower peelable adhesive with thickness;

[0025] The baking temperature is between 120°C and 150°C, and the baking time is between 10min and 30min.

[0026] Furthermore, in step S1, the glass is strengthened sodium-lime glass or aluminosilicate glass, with a strengthening stress of more than 400 MPa, a strengthening depth of 8 to 15 μm, and a glass thickness of 0.2 mm to 1.1 mm. Generally, the strengthening stress of Asahi Glass sodium-lime glass is between 400 MPa and 650 MPa, and the strengthening stress of aluminosilicate glass of Longwei, Corning, etc. is more than 700 MPa.

[0027] Furthermore, in step S2, the upper UV-Cut coating and the lower UV-Cut coating have a UV light cutoff function, and the transmittance of the upper UV-Cut coating and the lower UV-Cut coating is 0 in the 190nm to 380nm band. Compared with conventional photoresists, the main feature of this UV-Cut coating is that the transmittance is basically 0% in the UV band. In the 380nm to 780nm band, the transmittance of the UV-Cut coating is very high, maintained between 80% and 92%; in the 190nm to 380nm band, the transmittance of the UV-Cut coating drops sharply to 0%, and UV light will not pass through the UV-Cut coating. The UV-Cut coating can avoid the mutual influence of double-sided ITO exposure during double-sided exposure, and the main components of the upper UV-Cut coating and the lower UV-Cut coating are phenolic UV blockers.

[0028] Furthermore, in step S3, the coating thickness of ITO is 20nm to 60nm, and the square resistance is 30Ω / □ to 100Ω / □. The thicker the ITO thickness is, the lower the ITO square resistance is. When the ITO thickness is 20nm, the ITO square resistance is 100Ω / □; when the ITO thickness is 30nm, the ITO square resistance is 60Ω / □; when the ITO thickness is 60nm, the ITO square resistance is 30Ω / □.

[0029] Furthermore, in step S4, the coating thickness of the photoresist is 1 μm to 5 μm. The photoresist is a positive photoresist or a negative photoresist.

[0030] Furthermore, the etching solution in step S6 is 36% electronic grade HCl and 5% to 68% electronic grade HNO 3 Prepared aqua regia or FeCl 3 .

[0031] Furthermore, in step S7, the thickness of the silver paste is 5 μm to 9 μm, and the line width and line spacing are 10 μm / 10 μm to 40 μm / 40 μm.

[0032] Furthermore, in step S8, the thickness of the upper peelable adhesive and the lower peelable adhesive is 50 μm. The upper peelable adhesive and the lower peelable adhesive are a single-component solvent-based viscous liquid with good adhesive properties and mechanical properties, and can play the role of water resistance, oil resistance, acid resistance, alkali resistance, corrosion resistance, etc., and form a peelable film after curing. The color can be black or blue.

[0033] The present invention also provides a novel glass sensor, which is prepared by the above preparation process and includes glass, wherein an upper UV-Cut coating, an upper inner pattern and an upper peelable adhesive are sequentially provided on the upper surface of the glass, and silver paste is printed on the edge of the upper inner pattern by screen printing technology. After the silver paste is baked and solidified, a silver paste circuit is lasered out by a high-precision laser machine to obtain an upper edge routing, and the upper edge routing is connected to the upper inner pattern channel; a lower UV-Cut coating, a lower inner pattern and a lower peelable adhesive are sequentially provided on the lower surface of the glass, and silver paste is printed on the edge of the lower inner pattern by screen printing technology. After the silver paste is baked and solidified, a silver paste circuit is lasered out by a high-precision laser machine to obtain a lower edge routing, and the lower edge routing is connected to the lower inner pattern channel; the upper inner pattern and the upper edge routing constitute a capacitive sensing layer, and the lower inner pattern and the lower edge routing constitute a capacitive driving layer, and the capacitive sensing layer and the capacitive driving layer complete signal reception and transmission.

[0034] Furthermore, the main components of the upper UV-Cut coating and the lower UV-Cut coating are phenolic UV blockers.

[0035] Furthermore, the main component of the strippable adhesive is polyvinyl chloride or a vinyl resin derivative, and the main component of the photoresist is a photosensitive resin such as propylene glycol methyl ether acetate, including components such as solvents, resins, photoinitiators and additives.

[0036] Beneficial effects of the present invention: The preparation process of the novel glass sensor of the present invention realizes simultaneous exposure, development and etching on both sides of the glass by setting a UV-Cut coating. The UV-Cut coating can avoid the mutual influence of double-sided ITO exposure during double-sided exposure, and can effectively prevent scratches, foreign matter and other poor appearance caused by the single-sided two-time etching process, and the appearance yield is increased from 80% to 95%; the edge routing yellow light process is cancelled, and the printing silver paste process is adopted, and etching is not required, which solves the functional problems such as broken wires and incomplete etching, and the electrical yield is increased from 90% to 98%; the preparation process is simplified, the production efficiency is improved, and the production cost is effectively reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The specific implementation of the present invention will be further explained below in conjunction with the accompanying drawings.

[0038] Figure 1 It is a schematic diagram of the structure of the novel glass sensor of the present invention;

[0039] Figure 2 It is the relationship curve between ITO thickness and ITO square resistance;

[0040] Figure 3 It is the transmittance curve of UV-Cut coating;

[0041] Figure 4 This is the schematic diagram of double-sided exposure of ITO glass without UV-Cut coating;

[0042] Figure 5 This is the schematic diagram of double-sided exposure of ITO glass with UV-Cut coating. DETAILED DESCRIPTION

[0043] Combination Figure 1 The glass sensor preparation process of the double-sided simultaneous exposure, development and etching of the present embodiment includes the following steps:

[0044] Step S1: Cleaning the glass 5

[0045] Use a weakly alkaline or neutral detergent to clean the upper and lower surfaces of the glass 5;

[0046] Step S2: Setting UV-Cut coating

[0047] A UV-Cut coating is formed on the upper surface and the lower surface of the glass 5 by using a flow coating, spray coating or evaporation process, wherein the upper surface of the glass 5 is an upper UV-Cut coating 4, and the lower surface of the glass 5 is a lower UV-Cut coating 6;

[0048] Step S3: Preparation of ITO glass

[0049] By means of magnetron sputtering, ITO is coated on the surface of the upper UV-Cut coating 4 and the lower UV-Cut coating 6, and the thickness of the ITO coating is controlled by adjusting the conditions of magnetron sputtering to obtain the ITO glass with the required square resistance;

[0050] Step S4: Double-sided photoresist coating

[0051] Coating photoresist on the A and B surfaces of the ITO glass at the same time, and then baking, the baking temperature is 60°C to 120°C, and the baking time is 10min to 30min;

[0052] Step S5: Double-sided exposure and development of ITO glass

[0053] The ITO glass coated with photoresist on both sides is exposed on both sides in the designed A-side and B-side glass mask precision exposure machine, and then developed in a developer to develop the ITO pattern on the A-side and B-side. The developer is prepared with 90% solid electronic grade KOH, and then after washing with water and air drying, the liquid on the surface of the ITO glass is dried;

[0054] Step S6: Double-sided etching of ITO glass

[0055] Place the A and B surfaces of the ITO glass in an etching solution for double-sided etching, remove the ITO that is not needed for the pattern in the surface, and leave the ITO that is needed for the pattern in the surface; after washing with water and air drying, remove the photoresist on both sides in a stripping solution, the stripping solution is prepared with 99% electronic grade NaOH, and after washing with water and air drying, obtain the ITO glass with pattern 2 on the upper side and pattern 7 on the lower side;

[0056] The upper inner pattern 2 and the lower inner pattern 7 are a layer of patterned ITO coated on the upper and lower sides of the glass 5. A layer of ITO is first coated on the glass surface by magnetron sputtering, and then the required ITO pattern is obtained by exposure, development, and etching. The pattern of the ITO pattern can be a diamond, a rectangle, a square, or other regular shapes.

[0057] Step S7: Printing and lasering upper edge trace 3 and lower edge trace 8

[0058] Silver paste is printed on the edge of the ITO Pattern on the A side by screen printing technology, and then baked to form a thick block silver paste, and then a line with a line width and line spacing is lasered out by a high-precision laser machine to obtain an upper edge routing 3; silver paste is printed on the edge of the ITO Pattern on the B side by screen printing technology, and then baked to form a thick block silver paste, and then a line with a line width and line spacing is lasered out by a high-precision laser machine to obtain a lower edge routing 8;

[0059] The baking temperature is 120℃~140℃, and the baking time is 10min~30min;

[0060] Step S8: Printing peelable adhesive

[0061] Printing a peelable adhesive on the A side by screen printing technology and baking it to form an upper peelable adhesive 1 with thickness, and then printing a peelable adhesive on the B side by screen printing technology and baking it to form a lower peelable adhesive 9 with thickness;

[0062] The baking temperature is between 120°C and 150°C, and the baking time is between 10min and 30min.

[0063] In this embodiment, preferably, in step S1, glass 5 is strengthened sodium-lime glass or aluminosilicate glass, with a strengthening stress of more than 400 MPa, a strengthening depth of 8 to 15 μm, and a glass thickness of 0.2 mm to 1.1 mm. Generally, the strengthening stress of sodium-lime glass of Asahi Glass is between 400 MPa and 650 MPa, and the strengthening stress of aluminosilicate glass of Longwei, Corning, etc. is more than 700 MPa.

[0064] In this embodiment, preferably, the upper UV-Cut coating 4 and the lower UV-Cut coating 6 in step S2 have a UV light cutoff function, and the transmittance of the upper UV-Cut coating 4 and the lower UV-Cut coating 6 is 0 in the 190nm to 380nm band. Compared with conventional photoresists, the main feature of this UV-Cut coating is that the transmittance is basically 0% in the UV band. The transmittance curve of the UV-Cut coating is as shown in FIG. Figure 3 As shown in the figure, in the 380nm to 780nm band, the transmittance of the UV-Cut coating is very high, maintained between 80% and 92%; in the 190nm to 380nm band, the transmittance of the UV-Cut coating drops sharply to 0%, and UV light will not pass through the UV-Cut coating.

[0065] In this embodiment, preferably, the ITO coating thickness in step S3 is 20nm to 60nm, and the square resistance is 30Ω / □ to 100Ω / □. The thicker the ITO thickness, the lower the ITO square resistance. The relationship curve between ITO thickness and ITO square resistance is as shown in FIG. Figure 2 As shown, when the ITO thickness is 20nm, the ITO square resistance is 100Ω / □; when the ITO thickness is 30nm, the ITO square resistance is 60Ω / □; when the ITO thickness is 60nm, the ITO square resistance is 30Ω / □.

[0066] In this embodiment, the coating thickness of the photoresist in step S4 is preferably 1 μm to 5 μm. The photoresist is a positive photoresist or a negative photoresist.

[0067] In this embodiment, the etching solution in step S6 is preferably 36% electronic grade HCl and 5% to 68% electronic grade HNO 3 Prepared aqua regia or FeCl 3 .

[0068] Preferably, in this embodiment, the thickness of the silver paste in step S7 is 5 μm to 9 μm, and the line width and line spacing are 10 μm / 10 μm to 40 μm / 40 μm.

[0069] In this embodiment, the thickness of the upper peelable adhesive 1 and the lower peelable adhesive 9 in step S8 is preferably 50 μm. The upper peelable adhesive 1 and the lower peelable adhesive 9 are a single-component solvent-based viscous liquid with good adhesive properties and mechanical properties, and can play the role of water resistance, oil resistance, acid resistance, alkali resistance, corrosion resistance, etc., and form a peelable film after curing. The color can be black or blue.

[0070] Combination Figure 1The present invention also provides a novel glass sensor, which is prepared by the above preparation process, including glass 5, wherein the upper surface of the glass 5 is provided with an upper UV-Cut coating 4, an upper inner pattern 2 and an upper peelable adhesive 1 in sequence, and the edge of the upper inner pattern 2 is printed with silver paste by screen printing technology. After the silver paste is baked and solidified, the silver paste circuit is lasered out by a high-precision laser machine to obtain an upper edge routing 3, and the upper edge routing 3 is connected to the upper inner pattern 2 channel; the lower surface of the glass 5 is provided with a lower UV-Cut coating 6, a lower inner pattern 7 and a lower peelable adhesive 9 in sequence, and the edge of the lower inner pattern 7 is printed with silver paste by screen printing technology. After the silver paste is baked and solidified, the silver paste circuit is lasered out by a high-precision laser machine to obtain a lower edge routing 8, and the lower edge routing 8 is connected to the lower inner pattern 7 channel; the upper inner pattern 2 and the upper edge routing 3 constitute a capacitive sensing layer, and the lower inner pattern 5 and the lower edge routing 6 constitute a capacitive driving layer, and the capacitive sensing layer and the capacitive driving layer complete signal reception and transmission.

[0071] In this embodiment, preferably, the main components of the upper UV-Cut coating 4 and the lower UV-Cut coating 6 are phenolic UV blocking agents.

[0072] In this embodiment, the main component of the strippable adhesive is polyvinyl chloride or a vinyl resin derivative, and the main component of the photoresist is a photosensitive resin such as propylene glycol methyl ether acetate, including components such as solvents, resins, photoinitiators and additives.

[0073] Ultraviolet light UV is used for photoresist exposure. If there is no UV-Cut coating, when both sides of the ITO glass are exposed at the same time, the UV light on the A side of the glass will pass through the photoresist and ITO on the A side, and then further pass through the glass to reach the ITO and photoresist on the B side, affecting the exposure effect of the photoresist on the B side of the glass. After the UV light on the B side of the glass passes through the photoresist and ITO on the B side, it will further pass through the glass to reach the ITO and photoresist on the A side, affecting the exposure effect of the photoresist on the A side of the glass. When the A and B sides of the glass are exposed on both sides, they affect each other, which will cause abnormal patterns on the A and B sides of the ITO in the plane. The principle diagram of double-sided exposure of ITO glass without UV-Cut coating is as follows: Figure 4 shown.

[0074] After using UV-Cut coating, when both sides of ITO glass are exposed at the same time, UV-Cut coating can avoid mutual influence of double-sided ITO exposure during double-sided exposure. The main components of upper UV-Cut coating 4 and lower UV-Cut coating 6 are phenolic UV blockers. The UV light on glass surface A will reach the upper UV-Cut coating 4 on surface A after passing through the photoresist on surface A and ITO on surface A. Since the UV light is cut off, the UV light will not further pass through the upper UV-Cut coating 4 on surface A to reach the photoresist on surface B, and will not affect the exposure of the photoresist on surface B of the glass; the UV light on glass surface B will reach the lower UV-Cut coating 6 on surface B after passing through the photoresist on surface B and ITO on surface B. Since the UV light is cut off, the UV light will not further pass through the lower UV-Cut coating 6 on surface B to reach the photoresist on surface A, and will not affect the exposure of the photoresist on surface A of the glass. When double-sided exposure of glass surface A and surface B does not affect each other, it will not cause abnormal pattern in the surface. The principle diagram of double-sided exposure of ITO glass with UV-Cut coating is as shown in Figure 5 shown.

[0075] Conventional glass sensors use Mo-Al-Mo as the conductive material for edge routing, and the minimum line width and line spacing is only 20μm / 20μm. Since the concentration of Mo-Al-Mo etching solution is difficult to control within a relatively stable range, when the etching solution concentration is too high, the edge routing will be side-etched or over-etched, which may cause edge routing disconnection in severe cases. When the etching solution concentration is too low, the edge routing will not be etched cleanly, which may cause edge routing connection in severe cases.

[0076] The present invention adopts the printing silver paste process. The upper edge routing 3 and the lower edge routing 8 are silver paste block routing printed on the edge of the in-plane pattern using CCD precision screen printing technology. After the silver paste is baked and solidified, the silver paste circuit is lasered out under a CCD precision laser machine and certain parameters. The silver paste circuit is connected to the in-plane pattern channel. No etching is required, only baking and lasering can be used to obtain the required edge routing, which can solve the above side etching, broken wires, unclean etching, connection problems.

[0077] The preparation process of the novel glass sensor of this embodiment realizes simultaneous exposure, development, and etching on both sides of the glass by setting a UV-Cut coating. The UV-Cut coating can avoid the mutual influence of double-sided ITO exposure during double-sided exposure, and can effectively prevent scratches, foreign matter and other poor appearance caused by the single-sided two-etching process, and the appearance yield is increased from 80% to 95%; the edge routing yellow light process is cancelled, and the printing silver paste process is adopted, and etching is not required, which solves functional problems such as broken wires and incomplete etching, and the electrical yield is increased from 90% to 98%; the preparation process is simplified, the production efficiency is improved, and the production cost is effectively reduced.

[0078] Many specific details are described in the above description to facilitate a full understanding of the present invention. However, the above description is only a preferred embodiment of the present invention. The present invention can be implemented in many other ways different from those described herein, so the present invention is not limited to the specific implementation disclosed above. At the same time, any person familiar with the art can make many possible changes and modifications to the technical solution of the present invention using the methods and technical contents disclosed above without departing from the scope of the technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of protection of the technical solution of the present invention.

Claims

1. A glass sensor manufacturing process with double-sided simultaneous exposure, development and etching, characterized in that: The steps include: Step S1: Cleaning the glass (5) Clean the upper and lower surfaces of the glass (5) using a weakly alkaline or neutral detergent; Step S2: Setting UV-Cut coating Using a flow coating, spray coating or evaporation process to form UV-Cut coatings on the upper surface and lower surface of the glass (5), respectively, the upper surface of the glass (5) is the upper UV-Cut coating (4), and the lower surface of the glass (5) is the lower UV-Cut coating (6); Step S3: Preparation of ITO glass By means of a magnetron sputtering process, an ITO film is coated on the surface of the upper UV-Cut coating (4) and the lower UV-Cut coating (6), and the thickness of the ITO film is controlled by adjusting the magnetron sputtering conditions to obtain an ITO glass with a desired square resistance; Step S4: Double-sided photoresist coating Coating photoresist on the A and B surfaces of the ITO glass at the same time, and then baking, the baking temperature is 60°C to 120°C, and the baking time is 10 min to 30 min; Step S5: Double-sided exposure and development of ITO glass The designed A-side and B-side glass masks are placed in a precision exposure machine, and the ITO glass coated with photoresist on both sides is exposed on both sides. After exposure, it is developed in a developer to develop the ITO pattern on the A-side and B-side. After washing with water and air drying, the liquid on the surface of the ITO glass is dried. Step S6: Double-sided etching of ITO glass Place the A and B surfaces of the ITO glass in an etching solution for double-sided etching, remove the ITO not needed for the surface pattern, and leave the ITO needed for the surface pattern; after washing with water and air drying, remove the photoresist on both sides in a stripping solution, and after washing with water and air drying, obtain the ITO glass with the upper inner pattern (2) and the lower inner pattern (7); Step S7: Printing and lasering the upper edge traces (3) and the lower edge traces (8) Silver paste is printed on the edge of the ITO Pattern on the A side by screen printing technology, and then baked to form a thick block of silver paste, and then a high-precision laser machine is used to lasing a line with a line width and line spacing to obtain an upper edge routing (3); silver paste is printed on the edge of the ITO Pattern on the B side by screen printing technology, and then baked to form a thick block of silver paste, and then a high-precision laser machine is used to lasing a line with a line width and line spacing to obtain a lower edge routing (8); The baking temperature is 120 ℃ ~ 140 ℃, and the baking time is 10 min ~ 30 min; Step S8: Printing peelable adhesive Printing a peelable adhesive on the A side by screen printing technology and baking it to form an upper peelable adhesive (1) with thickness, and then printing a peelable adhesive on the B side by screen printing technology and baking it to form a lower peelable adhesive (9) with thickness; The baking temperature is between 120 ℃ and 150 ℃, and the baking time is between 10 min and 30 min.

2. The process for preparing a glass sensor with double-sided simultaneous exposure, development and etching according to claim 1, characterized in that: In step S1, the glass (5) is strengthened sodium-lime glass or aluminosilicate glass, the strengthening stress is above 400 MPa, the strengthening depth is 8 to 15 μm, and the glass thickness is 0.2 mm to 1.1 mm.

3. The process for preparing a glass sensor with double-sided simultaneous exposure, development and etching according to claim 1, characterized in that: In step S2, the upper UV-Cut coating (4) and the lower UV-Cut coating (6) have a UV light cutoff function, and in the 190 nm to 380 nm band, the transmittance of the upper UV-Cut coating (4) and the lower UV-Cut coating (6) is 0.

4. The process for preparing a glass sensor with double-sided simultaneous exposure, development and etching according to claim 1, characterized in that: In step S3, the ITO coating thickness is 20 nm to 60 nm, and the square resistance is 30Ω / □ to 100Ω / □.

5. The process for preparing a glass sensor with double-sided simultaneous exposure, development and etching according to claim 1, characterized in that: The coating thickness of the photoresist in step S4 is 1 μm to 5 μm.

6. The process for preparing a glass sensor with double-sided simultaneous exposure, development and etching according to claim 1, characterized in that: The etching solution in step S6 is aqua regia or FeCl3 prepared by 36% electronic grade HCl and 5% to 68% electronic grade HNO3.

7. The process for preparing a glass sensor with double-sided simultaneous exposure, development and etching according to claim 1, characterized in that: In step S7, the thickness of the silver paste is 5 μm to 9 μm, and the line width and line spacing are 10 μm / 10 μm to 40 μm / 40 μm.

8. The process for preparing a glass sensor with double-sided simultaneous exposure, development and etching according to claim 1, characterized in that: In step S8, the thickness of the upper peelable adhesive (1) and the lower peelable adhesive (9) is 50 μm.

9. A novel glass sensor prepared by the process of claim 1, characterized in that: The invention comprises glass (5), wherein the upper surface of the glass (5) is provided with an upper UV-Cut coating (4), an upper inner pattern (2) and an upper peelable adhesive (1) in sequence, the edge of the upper inner pattern (2) is printed with silver paste by screen printing technology, after the silver paste is baked and solidified, a silver paste line is lasered out by a high-precision laser machine to obtain an upper edge wiring (3), and the upper edge wiring (3) is connected to the channel of the upper inner pattern (2); the lower surface of the glass (5) is provided with a lower UV-Cut coating (6), a lower inner pattern (2) and an upper peelable adhesive (1) in sequence. n (7) and a lower peelable adhesive (9), the edge of the lower inner pattern (7) is printed with silver paste by screen printing technology, and after the silver paste is baked and solidified, a silver paste circuit is lasered out by a high-precision laser machine to obtain a lower edge routing (8), and the lower edge routing (8) is connected to the channel of the lower inner pattern (7); the upper inner pattern (2) and the upper edge routing (3) form a capacitive sensing layer, and the lower inner pattern (7) and the lower edge routing (8) form a capacitive driving layer, and the capacitive sensing layer and the capacitive driving layer complete signal reception and transmission.

Citation Information

Patent Citations

  • Method for manufacturing sensor structure based on charge transfer

    CN102214042A

  • Method for manufacturing electrodes on two surfaces of capacitance touch screen

    CN102323869A