Microporous layer, gas diffusion layer and preparation method thereof, fuel cell
By setting protruding modules on the microporous layer to form grooves, the problems of water flooding and low transmission efficiency of the fuel cell gas diffusion layer are solved, efficient gas transmission is achieved, the preparation process is simplified and the cost is reduced, making it suitable for commercialization application.
Patent Information
- Application Number
- CN202210259219.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-14
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-03-14
AI Technical Summary
The gas diffusion layer of existing fuel cells is prone to water flooding, has low mass transfer efficiency, complex preparation methods, high costs, and is difficult to commercialize.
By arranging multiple convex modules on the flat part of the microporous layer, grooves are formed to collect water generated by the catalytic layer and provide transmission channels for oxygen, thereby improving mass transfer efficiency. The microporous layer is composed of carbon black, isopropyl alcohol and polytetrafluoroethylene emulsion. It is prepared by spraying and sintering technology to prepare a highly efficient gas diffusion layer.
It significantly improves the mass transfer efficiency of the gas diffusion layer, increases the ultimate current density of the fuel cell, simplifies the preparation method, and reduces the cost, making it suitable for commercialization.
Smart Images

Figure CN114628698B_ABST
Abstract
Description
Technical Field
[0001] The present invention specifically relates to a microporous layer, a gas diffusion layer and a preparation method thereof, and a fuel cell. Background Art
[0002] With the rapid development of social economy, the energy demand is increasing and the environmental pollution problem is becoming increasingly serious. The development of efficient, reliable and environmentally friendly green energy has received attention from all countries. In order to achieve good energy conversion, electrochemical catalysis, as an efficient and convenient way to achieve energy conversion and storage, is of great significance for the application of new energy storage. Among them, the gas diffusion layer plays an important role in the energy conversion process.
[0003] The gas diffusion layer is composed of a microporous layer and a substrate layer, wherein the porosity of the microporous layer is 60-90%, and it is composed of carbon materials and binders, which can provide mechanical support for the catalyst layer, reduce the contact resistance between the catalyst layer and the gas diffusion layer, reduce the probability of flooding of the catalyst layer and the gas diffusion layer, and reduce mass transfer restrictions. The preparation of the microporous layer mainly includes three steps: slurry preparation, deposition and sintering. Specifically, the carbon material is mechanically mixed with the binder dispersed in water, and the resulting slurry is deposited on the surface of the substrate layer. After the deposition is completed, heat treatment is performed, and the completely dried gas diffusion layer is sintered at a higher temperature so that the carbon material is well bonded to the surface of the substrate layer.
[0004] A lot of work has been done on gas diffusion layers. Chinese patent document CN112761025A discloses a gas diffusion layer, which is a three-dimensional cross-linked fiber membrane formed by multiple carbon fibers, and the micropores are connected to the macropores, but the method has complicated operation steps and is difficult to commercialize. Antoni Forner-Cuenca et al. (Adv. Mater. 2015, 27, 6317–6322) constructed a hydrophilic and hydrophobic structure of the substrate layer by radiation grafting, but the radiation grafting method is complicated and only targets the substrate layer, making it difficult to apply and promote. Therefore, how to develop a gas diffusion layer with simple process, low price and high transmission efficiency has become an important challenge in the research and development of fuel cells. Summary of the invention
[0005] The technical problem actually solved by the present invention is to overcome the problems of the gas diffusion layer of the fuel cell in the prior art being easy to be flooded, having low mass transfer efficiency, complex preparation method, high cost, and difficulty in commercialization, and to provide a microporous layer, a gas diffusion layer and a preparation method thereof, and a fuel cell. The gas diffusion layer of the present invention is not prone to flooding, greatly improves the mass transfer efficiency of the gas diffusion layer, and improves the limiting current density of the fuel cell. In addition, the preparation method of the microporous layer and the gas diffusion layer of the present invention is simple, low-cost, and suitable for commercialization.
[0006] The present invention solves the above technical problems through the following technical solutions:
[0007] The present invention provides a microporous layer, which comprises a flat part and a plurality of raised modules arranged on the flat part; the raised modules are arranged at intervals, the interval between the raised modules is 0.05 to 0.6 mm, the height of the raised modules is 2 to 10 μm, wherein the interval refers to the width of a groove formed between two adjacent raised modules.
[0008] The present invention arranges a plurality of protruding modules on the flat part of the microporous layer, so that grooves are formed between the protruding modules. Water generated by the catalytic layer is preferentially collected in the grooves. The protruding modules provide transmission channels for oxygen, thereby achieving the purpose of improving mass transmission efficiency.
[0009] In the present invention, the thickness of the flat portion is preferably 5 to 15 μm.
[0010] In the present invention, the height of the protruding module is preferably 3 to 15 μm, more preferably 5 to 10 μm.
[0011] In the present invention, the height of the protruding module refers to the height of the protruding module relative to the protruding module of the flat portion.
[0012] In the present invention, the shape of the protrusion module can be conventional in the art, preferably a column.
[0013] In the present invention, the cross-sectional shape of the raised module may be conventional in the art, preferably one or more of square, rectangular and circular, more preferably square, wherein the cross-sectional shape is parallel to the cross-sectional shape of the flat portion.
[0014] The cross-sectional area is preferably 0.09 to 0.49 mm 2 , more preferably 0.16 to 0.36 mm 2 , for example 0.25mm 2 .
[0015] In some preferred embodiments of the present invention, the cross-section of the protruding module is in the shape of a square, and the side length of the square is preferably 0.3-0.8 mm, more preferably 0.4-0.6 mm, such as 0.5 mm.
[0016] In some preferred embodiments of the present invention, the shapes of the plurality of protrusion modules are the same, the shapes of the cross sections of the plurality of protrusion modules are the same, and the areas of the cross sections of the plurality of protrusion modules are the same.
[0017] In the present invention, the pitch of the protruding modules is preferably 0.1-0.6 mm, more preferably 0.2 mm-0.4 mm, and even more preferably 0.2 mm.
[0018] In the present invention, preferably, the plurality of protrusion modules are arranged in an array.
[0019] In some preferred embodiments of the present invention, the cross section of the protruding module is a square with a side length of 0.4-0.5 mm, and the pitch of the protruding modules is 0.2 mm, 0.4 mm or 0.6 mm.
[0020] In the present invention, the area ratio of the protruding module to the microporous layer is preferably 15% to 60%, more preferably 16 to 55%, for example 21%, 25%, 31%, 44% or 51%. The area of the protruding module generally refers to the cross-sectional area of the protruding module parallel to the flat portion.
[0021] In the present invention, the protruding module and the flat portion can be prepared by conventional methods in the art, and can generally be obtained by curing the microporous layer slurry.
[0022] The microporous layer slurry may be conventional in the art, preferably comprising 1 part of carbon black, 180-220 parts of isopropanol and 2-3 parts of polytetrafluoroethylene emulsion, wherein the parts are by mass.
[0023] In the microporous layer slurry, the isopropyl alcohol is preferably 200 parts.
[0024] In the microporous layer slurry, the polytetrafluoroethylene emulsion is preferably 2.2 parts.
[0025] In the microporous layer slurry, the concentration of the polytetrafluoroethylene emulsion can be conventional in the art, preferably 8 to 12 wt.%, more preferably 10 wt.%.
[0026] The present invention also provides a method for preparing the microporous layer as described above, which comprises the following steps:
[0027] S1: applying a microporous layer slurry on the base layer to obtain the flat portion;
[0028] S2: applying a microporous layer slurry at a position corresponding to the protruding module on the flat portion, and forming the protruding module after curing.
[0029] In the present invention, the application method may be conventional in the art, preferably coating, more preferably spraying.
[0030] In S2, preferably, a hollow mask is laid on the flat portion, and the microporous layer slurry is applied on the hollow mask, and the protruding module is formed after curing.
[0031] Among them, those skilled in the art can generally understand that the hollowed-out part of the hollowed-out mask corresponds to the position of the protruding module, and the shape and area of the hollowed-out part are the same as the cross-section of the protruding module.
[0032] The thickness of the hollow mask may be conventional in the art, generally greater than the height of the protruding module, preferably greater than 30 μm.
[0033] The material of the hollow mask may be conventional in the art, preferably polytetrafluoroethylene or polyvinyl chloride.
[0034] In S2, the curing can be performed by conventional methods in the art, preferably sintering.
[0035] The sintering temperature may be conventional in the art, preferably 300-400°C, more preferably 350°C.
[0036] The sintering time may be conventional in the art, preferably 0.8 to 1.5 hours, more preferably 1 hour.
[0037] The equipment used for sintering can be conventional in the art, generally a muffle furnace.
[0038] In the present invention, the preparation method of the microporous layer slurry can be conventional in the art, and generally comprises the following steps: mixing the components of the microporous layer slurry.
[0039] The mixing method may be conventional in the art, preferably ultrasonic dispersion.
[0040] The ultrasonic dispersion time may be conventional in the art, preferably 2 to 4 hours, more preferably 3 hours.
[0041] In the present invention, the curing can be carried out by conventional methods in the art, preferably sintering.
[0042] The sintering temperature may be conventional in the art, preferably 300-400°C, more preferably 350°C.
[0043] The sintering time may be conventional in the art, preferably 0.8 to 1.2 hours, more preferably 1 hour.
[0044] The present invention also provides a gas diffusion layer, comprising a substrate layer and the microporous layer as described above supported on the substrate layer, wherein the flat portion of the microporous layer is adjacent to the substrate layer.
[0045] In the present invention, the base layer preferably includes a carbon-based material and a hydrophobic coating attached to the surface of the carbon-based material.
[0046] The carbon-based material may be conventional in the field of fuel cells, generally carbon cloth, carbon paper or carbon felt, preferably carbon paper.
[0047] Wherein, the hydrophobic coating is preferably a PTFE layer.
[0048] The loading amount of the hydrophobic coating may be conventional in the art, preferably 25-35 wt.%, more preferably 30 wt.%. The loading amount refers to the mass ratio of the hydrophobic coating to the carbon-based material.
[0049] In the present invention, when the base layer includes the hydrophobic coating, the preparation method of the base layer can be conventional in the art. Preferably, the carbon-based material is treated with a hydrophobic material and then cured.
[0050] The hydrophobic material may be conventional in the field of fuel cells, such as PTFE emulsion.
[0051] The concentration of the PTFE emulsion may be conventional in the art, preferably 8 to 12 wt.%, more preferably 10 wt.%.
[0052] The hydrophobic treatment may be performed by conventional methods in the art, generally by immersing the carbon-based material in an emulsion containing the hydrophobic material and drying it.
[0053] In the hydrophobic treatment, the drying temperature may be conventional in the art, preferably 50-80°C, more preferably 60°C.
[0054] In the hydrophobic treatment, the drying time may be conventional in the art, preferably 0.5 to 2 hours, such as 1 hour.
[0055] Preferably, the carbon-based material is also cleaned before being subjected to the hydrophobic treatment.
[0056] The cleaning treatment can be carried out by conventional methods in the art, preferably by ultrasonication and drying in a solvent.
[0057] In the cleaning process, the solvent may be any conventional solvent in the art, preferably acetone.
[0058] In the cleaning process, the ultrasonic time can be conventional in the art, preferably 20 to 40 minutes, such as 30 minutes.
[0059] In the cleaning process, the drying temperature may be conventional in the art, preferably 60°C.
[0060] The present invention also provides a method for preparing the gas diffusion layer as described above, which comprises the following steps: loading the microporous layer on the base layer.
[0061] Among them, the method of loading the microporous layer can be conventional in the art. Preferably, the microporous layer slurry is applied on the base layer, and the flat part is formed after curing; the microporous layer slurry is applied at the position corresponding to the protruding module on the flat part, and the protruding module is formed after curing.
[0062] The present invention also provides a fuel cell, which comprises the gas diffusion layer as described above.
[0063] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0064] The reagents and raw materials used in the present invention are commercially available.
[0065] The positive and progressive effects of the present invention are:
[0066] The gas diffusion layer of the present invention is not prone to water flooding, greatly improves the mass transfer efficiency of the gas diffusion layer, and improves the limiting current density of the fuel cell. The limiting current density can be increased to 1.1 mA / cm 2 Above, even up to 1.4mA / cm 2 ; and the preparation method of the microporous layer and the gas diffusion layer of the present invention is simple, low-cost and suitable for commercialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] Figure 1 This is a schematic diagram of a top view of a gas diffusion layer in Example 1; the squares therein are protruding modules, and the serpentine lines are positions corresponding to the flow channels;
[0068] Figure 2 for Figure 1 A partial enlarged view of
[0069] Figure 3 a~g are polarization curves of Examples 1 to 6 and Comparative Example 1, respectively.
[0070] Reference numerals
[0071] 1-protruding module; d-the distance between the protruding modules. DETAILED DESCRIPTION
[0072] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0073] Example 1
[0074] S1: Preparation of the basal layer
[0075] Carbon paper (thickness 190 μm) was placed in an acetone solution and ultrasonically treated for 30 minutes, placed in a 60°C oven for drying, and then placed in a 10wt% PTFE emulsion and repeatedly immersed and dried (dried in a 60°C oven for 1 hour) multiple times to make the loading amount of the PTFE coating be 30wt%, where the loading amount is the mass ratio of the PTFE coating to the carbon paper.
[0076] S2: Gas Diffusion Layer Preparation
[0077] 0.09g carbon black, 18g isopropanol, 0.2g 10wt% polytetrafluoroethylene emulsion, ultrasonic dispersion for 3h to form a microporous layer slurry with good dispersion. Spray the microporous layer slurry onto the substrate to a loading of 1.5mg / cm 2 , forming a flat part with a height of 15μm. Then, a hollow mask with a thickness of 80μm (hollow shape: square, hollow spacing: 0.6mm (same for horizontal and vertical directions, both 0.6mm), hollow size: 0.5*0.5mm) was placed on the flat part. The overall size of the hollow mask was consistent with the base layer. The microporous layer slurry was sprayed. The spraying amount of the microporous layer slurry on the hollow mask was 1mg / cm 2 That is, 1 mg of microporous layer slurry is sprayed on each square centimeter of the hollow mask. After spraying, the mask is removed to obtain multiple protruding modules with a height of about 10 μm. The protruding modules are placed in a muffle furnace and sintered at 350°C for 1 hour to obtain a gas diffusion layer. The area ratio of the protruding modules to the microporous layer is the area ratio of the hollow to the hollow mask, which is 21%. The top view of the gas diffusion layer is shown in the figure below. Figure 1 As shown, Figure 1 A partial enlarged picture of Figure 2 As shown. Figure 1 and Figure 2 It can be seen that the protrusion modules 1 are arranged on the gas diffusion layer at equal intervals, and the size of the protrusion modules is consistent with the hollowing size, which is 0.5*0.5 mm; the spacing d of the protrusion modules is the hollowing spacing, which is 0.6 mm. Figure 1 The serpentine line in the figure represents the location of the corresponding flow channel.
[0078] Example 2
[0079] S1: Preparation of the basal layer
[0080] Same as S1 in Example 1.
[0081] S2: Gas Diffusion Layer Preparation
[0082] Hollow shape: square, hollow spacing: 0.4mm, hollow size: 0.5*0.5mm, the area ratio of the protruding module to the microporous layer is the area ratio of the hollow to the hollow mask, which is 31%, and the rest is the same as in Example 1, to obtain a gas diffusion layer.
[0083] Example 3
[0084] S1: Preparation of the basal layer
[0085] Same as S1 in Example 1.
[0086] S2: Gas Diffusion Layer Preparation
[0087] Hollow shape: square, hollow spacing: 0.2mm, hollow size: 0.5*0.5mm, the ratio of the area of the protruding module to the area of the microporous layer is the ratio of the hollow to the area of the hollow mask, which is 51%, and the rest is the same as in Example 1, to obtain a gas diffusion layer.
[0088] Example 4
[0089] S1: Preparation of the basal layer
[0090] Same as S1 in Example 1.
[0091] S2: Gas Diffusion Layer Preparation
[0092] Hollow shape: square, hollow spacing: 0.2mm, hollow size: 0.5*0.5mm, the area ratio of the raised module to the microporous layer is the ratio of the hollow to the hollow mask area, which is 51%, and the spraying amount of the microporous layer slurry on the hollow mask is 0.5mg / cm 2 The height of the protruding module is about 5 μm, and the rest is the same as in Example 1 to obtain a gas diffusion layer.
[0093] Example 5
[0094] S1: Preparation of the basal layer
[0095] Same as S1 in Example 1.
[0096] S2: Gas Diffusion Layer Preparation
[0097] Hollow shape: square, hollow spacing: 0.4mm, hollow size: 0.5*0.5mm, the area ratio of the raised module to the microporous layer is the ratio of the hollow to the hollow mask area, which is 31%, and the spraying amount of the microporous layer slurry on the hollow mask is 0.5mg / cm 2 The height of the protruding module is about 5 μm, and the rest is the same as in Example 1 to obtain a gas diffusion layer.
[0098] Example 6
[0099] S1: Preparation of the basal layer
[0100] Same as S1 in Example 1.
[0101] S2: Gas Diffusion Layer Preparation
[0102] Hollow shape: square, hollow spacing: 0.2mm, hollow size: 0.4*0.4mm, the area ratio of the raised module to the microporous layer is the ratio of the hollow to the hollow mask area, which is 44%, and the spraying amount of the microporous layer slurry on the hollow mask is 0.5mg / cm 2 The height of the protruding module is about 5 μm, and the rest is the same as in Example 1 to obtain a gas diffusion layer.
[0103] Comparative Example 1
[0104] S1: Preparation of the basal layer
[0105] Same as S1 in Example 1.
[0106] S2: Gas Diffusion Layer Preparation
[0107] 0.09 g of carbon black, 18 g of isopropanol and 0.2 g of 10 wt.% polytetrafluoroethylene emulsion were ultrasonically dispersed for 3 h to form a microporous layer slurry with good dispersion. The microporous layer slurry was sprayed onto the substrate to a loading of 2 mg / cm 2 (That is, the amount of microporous layer slurry sprayed per square centimeter of the base layer is 2 mg), the thickness of the formed microporous layer is about 20 μm, and then it is sintered in a muffle furnace at 350° C. for 1 hour to obtain a gas diffusion layer.
[0108] Effect Example
[0109] Fuel cell limiting current density test
[0110] The gas diffusion layers prepared in Examples 1 to 6 and Comparative Example 1 were assembled into a fuel cell, wherein the substrate layer was adjacent to the bipolar plate, and a US Gore PRIMEA membrane electrode assembly (catalytic layer + proton exchange membrane, i.e., CCM) was used, wherein the cathode catalyst Pt / C loading was 0.4 mg / cm 2 , the anode Pt / C loading is 0.05 mg / cm 2 The obtained membrane electrode assembly is placed in the middle of the positive and negative bipolar plates, which provide reaction gas for the membrane electrode. The graphite current collector is placed outside the positive and negative plates to collect current. The sealing component is a rubber sealing ring, and the sealing component is used to form an air chamber between the membrane electrode and the plate and between the plate and the end plate; the outer surface of the end plate has an air inlet and an air outlet.
[0111] Battery performance test conditions: temperature 60°C, humidity 100%, back pressure 50KPa, cathode: 275mL / min of air, anode: 110mL / min of hydrogen.
[0112] The results are as follows Figure 3 As shown, Figure 3 a~g are the polarization curves of the fuel cells assembled in Examples 1~6 and Comparative Example 1, respectively. The respective limiting current densities can be obtained from the polarization curves, as shown in Table 1.
[0113] Table 1 Effect data table of each embodiment and comparative example
[0114]
[0115]
[0116] From Examples 1 to 3 in Table 1, it can be seen that, under the premise that the spraying amount of the microporous layer slurry on the hollow mask, i.e., the height of the protruding module, and the hollow size, i.e., the size of the protruding module, are consistent, the hollow spacing, i.e., the spacing of the protruding modules, affects the gas and water transmission efficiency of the gas diffusion layer. When the spacing is 0.2 mm, the limiting current density of the fuel cell is the largest. When the hollow spacing is 0.2 mm and the hollow size is 0.5*0.5 mm, the height of the protruding module is changed, i.e., the spraying amount of the microporous layer slurry on the hollow mask is reduced to 0.5 mg / cm 2 As shown in Example 4, the limiting current density of the fuel cell is further improved, and the limiting current density can be as high as 1.40 mA / cm 2 , indicating that the height of the protruding module also directly affects the transmission efficiency of gas and water. Compared with Example 4, Example 6 only differs in the size of the hollowing, which shows that the size of the protruding module also affects the transmission efficiency. The fuel cells composed of the gas diffusion layers obtained in Examples 1 to 6 have significantly improved limiting current densities compared to the fuel cells composed of conventional gas diffusion layers in Comparative Example 1.
Claims
1. A microporous layer, characterized in that: It includes a flat part and a plurality of raised modules arranged on the flat part; the raised modules are arranged vertically on the flat part; the cross section of the raised modules is in the shape of a square; the cross section is parallel to the flat part; the area of the cross section is 0.16-0.36mm 2 The protrusion modules are arranged at intervals, the pitch of the protrusion modules is 0.05~0.2mm, the height of the protrusion modules is 3~5μm, wherein the pitch is the width of the groove formed between two adjacent protrusion modules.
2. The microporous layer according to claim 1, characterized in that The thickness of the flat part is 5-15 μm; And / or, the protruding module is in the shape of a column.
3. The microporous layer according to claim 1, characterized in that The cross-sectional area is 0.25 mm 2 ; and / or, the pitch of the protruding modules is 0.2 mm; and / or, the protruding modules occupy 15% to 60% of the area of the microporous layer; And / or, the plurality of protrusion modules are arranged in an array.
4. The microporous layer according to claim 3, characterized in that The area ratio of the protrusion module to the microporous layer is 16-55%.
5. The microporous layer according to claim 3, characterized in that The protrusion modules occupy 21%, 25%, 31%, 44% or 51% of the area of the microporous layer.
6. The microporous layer according to claim 1, characterized in that The protruding modules and the flattened portion are obtained by curing the microporous layer slurry.
7. The microporous layer according to claim 6, characterized in that The microporous layer slurry comprises 1 part of carbon black, 180-220 parts of isopropanol and 2-3 parts of polytetrafluoroethylene emulsion, wherein the parts are by mass.
8. The microporous layer according to claim 7, characterized in that The isopropanol is 200 parts; And / or, the polytetrafluoroethylene emulsion is 2.2 parts; And / or, the concentration of the polytetrafluoroethylene emulsion is 8-12wt.%.
9. The microporous layer according to claim 8, characterized in that The concentration of the polytetrafluoroethylene emulsion is 10 wt.%.
10. A method for preparing a microporous layer according to any one of claims 1 to 9, characterized in that: It includes the following steps: S1: applying a microporous layer slurry on the base layer to obtain the flat portion; S2: applying microporous layer slurry at the position corresponding to the protruding module on the flat part, and forming the protruding module after curing.
11. The method for preparing a microporous layer according to claim 10, characterized in that: The method of applying is coating; And / or, in S2, laying a hollow mask on the flat part, spraying the microporous layer slurry on the hollow mask, and forming the protruding module after sintering; And / or, the solidification method is sintering.
12. The method for preparing a microporous layer according to claim 11, characterized in that: The application method is spraying; And / or, the thickness of the hollow mask is greater than 30 μm; And / or, the sintering temperature is 300-400°C; And / or, the sintering time is 0.8~1.5h.
13. The method for preparing a microporous layer according to claim 12, characterized in that: The sintering temperature is 350°C; And / or, the sintering time is 1 hour.
14. A gas diffusion layer, characterized in that: The invention comprises a base layer and a microporous layer as claimed in any one of claims 1 to 9 supported on the base layer, wherein the flat portion of the microporous layer is adjacent to the base layer.
15. The gas diffusion layer according to claim 14, characterized in that The base layer includes a carbon-based material and a hydrophobic coating attached to the surface of the carbon-based material.
16. The gas diffusion layer according to claim 15, characterized in that The carbon-based material is carbon paper; And / or, the hydrophobic coating is a PTFE layer; And / or, the loading amount of the hydrophobic coating is 25-35wt.%, and the loading amount refers to the mass ratio of the hydrophobic coating to the carbon-based material.
17. The gas diffusion layer according to claim 15, characterized in that The loading amount of the hydrophobic coating is 30 wt.%, and the loading amount refers to the mass ratio of the hydrophobic coating to the carbon-based material.
18. A method for preparing a gas diffusion layer according to any one of claims 14 to 17, characterized in that: The method comprises the following steps: loading the microporous layer on the base layer.
19. A fuel cell, characterized in that: It comprises the gas diffusion layer according to any one of claims 14 to 17.