Nanocomposite electrode material for improving glucose sensing performance and preparation method thereof

By co-depositing bimetallic elements on the surface of titanium-based amorphous alloy nanotubes, forming a double-layer nanostructure, the glucose sensing performance is improved, and the problems of insufficient detection sensitivity and detection limit of existing titanium-based nanotubes are solved, achieving high Sensitivity and low detection limit glucose sensing effect.

CN114646672BActive Publication Date: 2024-11-01NANJING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011507374.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-18
Publication Date
2024-11-01
Estimated Expiration
2040-12-18

AI Technical Summary

Technical Problem

The sensitivity and detection limits of existing titanium-based nanotubes are insufficient in glucose detection, and their sensing performance needs to be improved.

Method used

Bimetallic elements (such as Mn, Fe, Co, Ni, Cu) are used to co-deposit on the surface of titanium-based amorphous alloy nanotubes to form a bilayer nanostructure, and the specific surface area and electrons of the nanocomposite electrode material are enhanced by electrochemical pulse deposition method. Transmission rate.

Benefits of technology

The sensitivity and detection limit of glucose sensing are significantly improved. The nanocomposite electrode material formed has a larger specific surface area and stronger catalytic activity. The sensitivity is as high as 3340μA·mM-1·cm-2 when detecting glucose, and the detection limit is low. It is up to 0.041 μM, and has a simple process and low cost, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0002845323580000011
    Figure HDA0002845323580000011
  • Figure HDA0002845323580000012
    Figure HDA0002845323580000012
  • Figure HDA0002845323580000013
    Figure HDA0002845323580000013
Patent Text Reader

Abstract

The present invention discloses a nanocomposite electrode material for improving glucose sensing performance. The nanocomposite electrode material has a composite structure formed by a double-layer nanostructure, wherein the double-layer nanostructure includes a bottom structure and a surface structure, wherein the bottom structure is a titanium-based amorphous alloy nanotube with an open upper end face, and the surface structure is a nanostructure formed by two transition metal elements, and the surface structure is attached to the upper end face of the titanium-based amorphous alloy nanotube; wherein the transition metal elements are any two of Mn, Fe, Co, Ni and Cu. The present invention also discloses a method for preparing a nanocomposite electrode material for improving glucose sensing performance. The nanocomposite electrode material of the present invention co-deposits the two metal elements on the surface of the titanium-based amorphous alloy nanotube to form a nanocomposite structure, so that the electrode material has a larger specific surface area, more active sites and a faster electron transmission rate, and has a higher sensitivity and a lower detection limit when detecting glucose.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nano-metal functional materials, and in particular to a nano-composite electrode material for improving glucose sensing performance and a preparation method thereof. Background Art

[0002] TiO 2 Nanotubes are a new type of inorganic functional material. Due to their unique porous structure and semiconductor properties, they are used in photocatalysis, dye-sensitized batteries, and sensors. Traditional titanium-based nanotubes are basically prepared using crystalline alloys and precursors. This is because for most alloy systems, their amorphous formation ability is limited or even cannot form an amorphous state; secondly, amorphous alloys have strong corrosion resistance, which is limited in the process of preparing nanostructured materials. However, the amorphous structure has a long-range disorder and short-range order. When forming a nanotube structure, the orderly arranged nanotubes may further increase the specific surface area, increase the reaction active sites, and promote catalytic oxidation during the reaction process, which can greatly improve the performance of nanomaterials.

[0003] The Chinese patent application number 201810698988.1 discloses a titanium-based amorphous nanotube and its preparation method. The nanotube is obtained by arc melting to obtain a Ti-based alloy ingot, and amorphous strips are obtained by single-roll stripping. The amorphous nanotube is obtained by constant potential polarization in ethylene glycol electrolyte, and glucose is detected by electrochemical method. It is concluded that the nanotube has high sensitivity and low detection limit. However, when the nanotube detects glucose, its sensitivity and detection limit need to be further improved. Summary of the invention

[0004] The purpose of the present invention is to address the deficiencies of the prior art and provide a nanocomposite electrode material for improving the glucose sensing performance. The nanocomposite electrode material co-deposits bimetallic elements on the surface of titanium-based amorphous alloy nanotubes to form a nanocomposite structure, so that the electrode material has a larger specific surface area, more active sites and a faster electron transfer rate, and has higher sensitivity and lower detection limit when detecting glucose.

[0005] Another object of the present invention is to provide a method for preparing a nanocomposite electrode material for improving glucose sensing performance.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] A nanocomposite electrode material for improving glucose sensing performance, the nanocomposite electrode material having a composite structure formed by a double-layer nanostructure, the double-layer nanostructure comprising a bottom structure and a surface structure, the bottom structure being a titanium-based amorphous alloy nanotube with an open upper end face, the surface structure being a nanostructure formed by two transition metal elements, and the surface structure being attached to the upper end face of the titanium-based amorphous alloy nanotube;

[0008] Wherein, the transition metal elements are any two of Mn, Fe, Co, Ni and Cu.

[0009] Furthermore, the nanostructure of the surface layer is any one of a nano-mesh structure, a nano-cotton-like structure, a nano-fragment structure, a nano-cheese structure, a nano-ball structure, a nano-particle structure, a nano-worm-like structure, and a nano-flower bud structure.

[0010] Furthermore, the titanium-based amorphous alloy nanotubes include a plurality of TiCuO amorphous alloy nanotubes, and the plurality of TiCuO amorphous alloy nanotubes are neatly arranged into a nanotube array structure.

[0011] Furthermore, the specific surface area of ​​the electrode material is 11-25 times that of the TiCuO amorphous alloy nanotubes.

[0012] A method for preparing a nanocomposite electrode material for improving glucose sensing performance comprises the following steps:

[0013] S1: Preparation of titanium-based amorphous alloy nanotubes

[0014] Using titanium-copper amorphous alloy strips as substrate, TiCuO amorphous nanotubes were prepared by anodization.

[0015] S2: Preparation of Nanocomposite Electrode Materials

[0016] The TiCuO amorphous nanotubes obtained in step S1 are used as working electrodes, the Pt sheet is used as counter electrodes, and the saturated calomel electrode is used as reference electrodes. The working electrodes, counter electrodes, and reference electrodes are placed in a deposition solution and connected to an electrochemical workstation to deposit metals onto the TiCuO amorphous nanotubes by an electrochemical pulse deposition method;

[0017] The TiCuO amorphous nanotubes with deposited metal are taken out, washed in deionized water, and dried naturally at room temperature to obtain the desired nanocomposite electrode material.

[0018] Furthermore, the deposition solution in step S2 is a 0.01M-0.3M chloride salt solution of two transition metal elements, and the molar ratio of the two metals is 1:(1-3).

[0019] Furthermore, in step S2, the parameters of the electrochemical pulse deposition method are: positive pulse current density: +40 to +80 mA / cm 2 , duration 2-5ms; pulse positive current density: -30~-80mA / cm 2 , duration 8-12ms; cycle: 500~1000; pulse interval: 50-100ms.

[0020] Furthermore, the temperature of the deposition solution is 35-40° C., and a magnetic stirrer is used for stirring at a stirring speed of 140-160 rpm.

[0021] Furthermore, in step S2, the TiCuO amorphous nanotubes with deposited metal are washed in deionized water for 30-60 seconds.

[0022] Furthermore, the preparation method in step S1 is as follows: Ti 60 Cu 40 The metal single substance is smelted to obtain the master alloy, and then the master alloy is rapidly cooled and spun through a high-speed rotating copper roller to obtain Ti 60 Cu 40 Amorphous alloy strip, Ti 60 Cu 40 The amorphous alloy strips were subjected to constant potential polarization treatment in ethylene glycol electrolyte and then washed with deionized water and anhydrous ethanol to obtain TiCuO amorphous nanotubes.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The nanocomposite electrode material of the present invention has a double-layer nanostructure, wherein the bottom layer is a TiCuO amorphous nanotube with an open upper end face, and the surface layer is a nanostructure formed by co-deposition of two transition metal elements. The surface nanostructure is formed by co-depositing the two transition metal elements on the upper end face of the TiCuO amorphous nanotube by an electrochemical pulse deposition method, and by specific conditions, the two transition metal elements form a nanostructure together during the deposition process. The transition metal elements have multiple electron orbits and are easy to lose or gain electrons, thereby having strong redox properties. At the same time, the two metal components also have a synergistic effect, a geometric effect or a coupling effect, thereby having a better catalytic activity than a single metal component, and the co-formed nanostructure has a stronger adhesion to the nanotube, thereby enhancing the structural stability of the electrode material during operation, thereby ensuring its sensing performance.

[0025] 2. The electrode material of the present invention has a high specific surface area, and the nanostructure formed by co-deposition penetrates into the nanotubes without causing blockage, thereby further improving the specific surface area of ​​the electrode material. Its specific surface area is 11-25 times that of the TiCuO amorphous alloy nanotubes. It has more active sites, providing more attachment points for glucose, thereby providing more places for redox reactions and accelerating the reaction rate. On the other hand, the electrode material combines the excellent longitudinal electron transfer rate of the nanotubes themselves and the excellent catalytic performance and conductivity of the transition metal elements. When detecting glucose, the sensitivity is as high as 3340μA·mM-1·cm-2, and the detection limit is as low as 0.041μM.

[0026] 3. The electrode material of the present invention has a self-supporting structure, avoids the pretreatment of the catalytic electrode material, is evenly dispersed, does not agglomerate during the working process, has high efficiency, is simple to operate, and is easy to repeat; at the same time, the preparation process of the electrode material of the present invention is simple, low cost, short time consumption, easy to industrialize and widely used, has better practicality, and does not require strong acid solution in the whole process, is environmentally friendly, and is beneficial to environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 and Figure 2 It is a SEM picture of the TiCuO amorphous nanotube of the present invention.

[0028] Figure 3 This is a SEM image of the (Ni-Co) / TiCuO nanocomposite electrode material obtained in Example 1.

[0029] Figure 4 This is the TEM scan image corresponding to the (Ni-Co) / TiCuO nanocomposite electrode material obtained in Example 1.

[0030] Figure 5a , 5b, 5c are respectively Figure 4 Perform EDS surface scans of Ti, Ni, and Co.

[0031] Figure 6-Figure 14 They are SEM images of the nanocomposite electrode materials obtained in Examples 2-10 respectively.

[0032] Fig.15 It is a fitted straight line graph of the electrochemical active areas of four samples, namely, the electrode material of Example 1, the TiCuO amorphous nanotubes, the electrode material of Comparative Example 1, and the electrode material of Comparative Example 2.

[0033] Fig.16 It is a fitted straight line graph of the electrochemical active areas of four samples, namely, the electrode material of Example 1, the TiCuO amorphous nanotubes, the electrode material of Comparative Example 1, and the electrode material of Comparative Example 2. DETAILED DESCRIPTION

[0034] In order to better understand the technical content of the present invention, specific embodiments are given and described as follows in conjunction with the accompanying drawings.

[0035] Unless otherwise specified, the raw materials in the following examples were purchased from commercial sources.

[0036] Example 1

[0037] S1: Preparation of titanium-based amorphous alloy nanotubes

[0038] The purity of 99.99% Ti and Cu is Ti 60 Cu 40 The required mass was weighed and put into an arc melting furnace. The alloy was repeatedly melted 5 times in a high-purity argon atmosphere, and magnetic stirring was turned on to ensure that the alloy elements were evenly mixed. The alloy ingot was taken out, the surface oxide layer was polished to remove it, and 5g was put into a quartz tube. In a high-purity argon atmosphere, a strip with a width of about 1mm and a thickness of about 20μm was prepared by spinning the strip. A small part was cut and welded with nickel wire, and the welding place was painted with ordinary nail polish, and the exposed surface area of ​​the strip was ensured to be 0.3cm 2 The prepared sample was used as the anode and the platinum sheet was used as the counter electrode in about 50 ml of ethylene glycol electrolyte with 0.2 wt% NH 4 F+2.0vol%H 2 O was polarized at a constant voltage of 15 V for 4 h using an electrochemical workstation, and then taken out and ultrasonically cleaned in deionized water for 5 s, and then cleaned with anhydrous ethanol to obtain TiCuO amorphous nanotubes.

[0039] S2: Preparation of (Ni-Co) / TiCuO nanocomposite electrode materials

[0040] The TiCuO amorphous nanotubes obtained in step S1 were used as working electrodes, the Pt sheet was used as counter electrodes, and the saturated calomel electrode was used as reference electrodes. The working electrodes, counter electrodes, and reference electrodes were placed in a 0.02 M NiCl 2 +0.02M CoCl 2 The solution was stirred at 150 rpm with a magnetic stirrer and connected to an electrochemical workstation. Ni-Co was deposited onto the TiCuO amorphous nanotubes by electrochemical pulse deposition. The pulse deposition conditions were: negative current -50 mA / cm 2 (8ms), positive current 40mA / cm 2 (2ms), pulse interval 100ms, number of cycles 1000.

[0041] The TiCuO amorphous nanotubes on which Ni-Co was deposited were taken out, washed in deionized water for 60 seconds, and dried naturally at room temperature to obtain the desired (Ni-Co) / TiCuO nanocomposite electrode material.

[0042] Example 2

[0043] S1: Preparation of titanium-based amorphous alloy nanotubes

[0044] The purity of 99.99% Ti and Cu is Ti 60 Cu 40 The required mass was weighed and put into an arc melting furnace. The alloy was repeatedly melted 5 times in a high-purity argon atmosphere, and magnetic stirring was turned on to ensure that the alloy elements were evenly mixed. The alloy ingot was taken out, the surface oxide layer was polished to remove it, and 5g was put into a quartz tube. In a high-purity argon atmosphere, a strip with a width of about 1mm and a thickness of about 20μm was prepared by spinning the strip. A small part was cut and welded with nickel wire, and the welding place was painted with ordinary nail polish, and the exposed surface area of ​​the strip was ensured to be 0.3cm 2 The prepared sample was used as the anode and the platinum sheet was used as the counter electrode in about 50 ml of ethylene glycol electrolyte with 0.2 wt% NH 4 F+2.0vol%H 2 O was polarized at a constant voltage of 15 V for 4 h using an electrochemical workstation, and then taken out and ultrasonically cleaned in deionized water for 5 s, and then cleaned with anhydrous ethanol to obtain TiCuO amorphous nanotubes.

[0045] S2: Preparation of (Ni-Fe) / TiCuO nanocomposite electrode materials

[0046] The TiCuO amorphous nanotubes obtained in step S1 were used as working electrodes, the Pt sheet was used as counter electrodes, and the saturated calomel electrode was used as reference electrodes. The working electrodes, counter electrodes, and reference electrodes were placed in a 0.01 M NiCl 2 +0.02M FeCl 2 The solution was stirred at 140 rpm with a magnetic stirrer at a temperature of 35 °C and connected to an electrochemical workstation to deposit Ni-Co onto the TiCuO amorphous nanotubes by electrochemical pulse deposition. The pulse deposition conditions were: negative current -40 mA / cm 2 (8ms), positive current 60mA / cm 2 (2ms), pulse interval 50ms, cycle number 1000.

[0047] The TiCuO amorphous nanotubes on which Ni-Fe was deposited were taken out, washed in deionized water for 40 seconds, and dried naturally at room temperature to obtain the desired (Ni-Fe) / TiCuO nanocomposite electrode material.

[0048] Example 3

[0049] S1: Preparation of titanium-based amorphous alloy nanotubes

[0050] The purity of 99.99% Ti and Cu is Ti 60 Cu 40 The required mass was weighed and put into an arc melting furnace. The alloy was repeatedly melted 5 times in a high-purity argon atmosphere, and magnetic stirring was turned on to ensure that the alloy elements were evenly mixed. The alloy ingot was taken out, the surface oxide layer was polished to remove it, and 5g was put into a quartz tube. In a high-purity argon atmosphere, a strip with a width of about 1mm and a thickness of about 20μm was prepared by spinning the strip. A small part was cut and welded with nickel wire, and the welding place was painted with ordinary nail polish, and the exposed surface area of ​​the strip was ensured to be 0.3cm 2 The prepared sample was used as the anode and the platinum sheet was used as the counter electrode in about 50 ml of ethylene glycol electrolyte with 0.2 wt% NH 4 F+2.0vol%H 2 O was polarized at a constant voltage of 15 V for 4 h using an electrochemical workstation, and then taken out and ultrasonically cleaned in deionized water for 5 s, and then cleaned with anhydrous ethanol to obtain TiCuO amorphous nanotubes.

[0051] S2: Preparation of (Ni-Mn) / TiCuO nanocomposite electrode materials

[0052] The TiCuO amorphous nanotubes obtained in step S1 were used as working electrodes, the Pt sheet was used as counter electrodes, and the saturated calomel electrode was used as reference electrodes. The working electrodes, counter electrodes, and reference electrodes were placed in 0.1 M NiCl 2 +0.3M MnCl 2 The solution was stirred at 160 rpm with a magnetic stirrer and connected to an electrochemical workstation. Ni-Mn was deposited onto the TiCuO amorphous nanotubes by electrochemical pulse deposition. The pulse deposition conditions were: negative current -80 mA / cm 2 (8ms), positive current 60mA / cm 2 (2ms), pulse interval 70ms, cycle number 500.

[0053] The TiCuO amorphous nanotubes on which Ni-Mn was deposited were taken out, washed in deionized water for 40 seconds, and dried naturally at room temperature to obtain the desired (Ni-Mn) / TiCuO nanocomposite electrode material.

[0054] Example 4

[0055] S1: Preparation of titanium-based amorphous alloy nanotubes

[0056] The purity of 99.99% Ti and Cu is Ti 60 Cu 40The required mass was weighed and put into an arc melting furnace. The alloy was repeatedly melted 5 times in a high-purity argon atmosphere, and magnetic stirring was turned on to ensure that the alloy elements were evenly mixed. The alloy ingot was taken out, the surface oxide layer was polished to remove it, and 5g was put into a quartz tube. In a high-purity argon atmosphere, a strip with a width of about 1mm and a thickness of about 20μm was prepared by spinning the strip. A small part was cut and welded with nickel wire, and the welding place was painted with ordinary nail polish, and the exposed surface area of ​​the strip was ensured to be 0.3cm 2 The prepared sample was used as the anode and the platinum sheet was used as the counter electrode in about 50 ml of ethylene glycol electrolyte with 0.2 wt% NH 4 F+2.0vol%H 2 O was polarized at a constant voltage of 15 V for 4 h using an electrochemical workstation, and then taken out and ultrasonically cleaned in deionized water for 5 s, and then cleaned with anhydrous ethanol to obtain TiCuO amorphous nanotubes.

[0057] S2: Preparation of (Co-Cu) / TiCuO nanocomposite electrode materials

[0058] The TiCuO amorphous nanotubes obtained in step S1 were used as working electrodes, the Pt sheet was used as counter electrodes, and the saturated calomel electrode was used as reference electrodes. The working electrodes, counter electrodes, and reference electrodes were placed in 0.07 M CuCl 2 +0.07M CoCl 2 The solution was stirred at 160 rpm with a magnetic stirrer and connected to an electrochemical workstation. Co-Cu was deposited onto the TiCuO amorphous nanotubes by electrochemical pulse deposition. The pulse deposition conditions were: negative current -50 mA / cm 2 (8ms), positive current 80mA / cm 2 (2ms), pulse interval 60ms, cycle number 1000.

[0059] The TiCuO amorphous nanotubes on which Co-Cu was deposited were taken out, washed in deionized water for 30 seconds, and dried naturally at room temperature to obtain the desired (Co-Cu) / TiCuO nanocomposite electrode material.

[0060] Example 5

[0061] S1: Preparation of titanium-based amorphous alloy nanotubes

[0062] The purity of 99.99% Ti and Cu is Ti 60 Cu 40The required mass was weighed and put into an arc melting furnace. The alloy was repeatedly melted 5 times in a high-purity argon atmosphere, and magnetic stirring was turned on to ensure that the alloy elements were evenly mixed. The alloy ingot was taken out, the surface oxide layer was polished to remove it, and 5g was put into a quartz tube. In a high-purity argon atmosphere, a strip with a width of about 1mm and a thickness of about 20μm was prepared by spinning the strip. A small part was cut and welded with nickel wire, and the welding place was painted with ordinary nail polish, and the exposed surface area of ​​the strip was ensured to be 0.3cm 2 The prepared sample was used as the anode and the platinum sheet was used as the counter electrode in about 50 ml of ethylene glycol electrolyte with 0.2 wt% NH 4 F+2.0vol%H 2 O was polarized at a constant voltage of 15 V for 4 h using an electrochemical workstation, and then taken out and ultrasonically cleaned in deionized water for 5 s, and then cleaned with anhydrous ethanol to obtain TiCuO amorphous nanotubes.

[0063] S2: Preparation of (Fe-Mn) / TiCuO nanocomposite electrode materials

[0064] The TiCuO amorphous nanotubes obtained in step S1 were used as working electrodes, the Pt sheet was used as counter electrodes, and the saturated calomel electrode was used as reference electrodes. The working electrodes, counter electrodes, and reference electrodes were placed in 0.03 M FeCl 2 +0.06M MnCl 2 The solution was stirred at 160 rpm with a magnetic stirrer and connected to an electrochemical workstation. Fe-Mn was deposited onto the TiCuO amorphous nanotubes by electrochemical pulse deposition. The pulse deposition conditions were: negative current -70 mA / cm 2 (8ms), positive current 60mA / cm 2 (2ms), pulse interval 80ms, cycle number 800 turns.

[0065] The TiCuO amorphous nanotubes on which Fe-Mn was deposited were taken out, washed in deionized water for 30 seconds, and dried naturally at room temperature to obtain the desired (Fe-Mn) / TiCuO nanocomposite electrode material.

[0066] Example 6

[0067] S1: Preparation of titanium-based amorphous alloy nanotubes

[0068] The purity of 99.99% Ti and Cu is Ti 60 Cu 40The required mass was weighed and put into an arc melting furnace. The alloy was repeatedly melted 5 times in a high-purity argon atmosphere, and magnetic stirring was turned on to ensure that the alloy elements were evenly mixed. The alloy ingot was taken out, the surface oxide layer was polished to remove it, and 5g was put into a quartz tube. In a high-purity argon atmosphere, a strip with a width of about 1mm and a thickness of about 20μm was prepared by spinning the strip. A small part was cut and welded with nickel wire, and the welding place was painted with ordinary nail polish, and the exposed surface area of ​​the strip was ensured to be 0.3cm 2 The prepared sample was used as the anode and the platinum sheet was used as the counter electrode in about 50 ml of ethylene glycol electrolyte with 0.2 wt% NH 4 F+2.0vol%H 2 O was polarized at a constant voltage of 15 V for 4 h using an electrochemical workstation, and then taken out and ultrasonically cleaned in deionized water for 5 s, and then cleaned with anhydrous ethanol to obtain TiCuO amorphous nanotubes.

[0069] S2: Preparation of (Fe-Co) / TiCuO nanocomposite electrode materials

[0070] The TiCuO amorphous nanotubes obtained in step S1 were used as working electrodes, the Pt sheet was used as counter electrodes, and the saturated calomel electrode was used as reference electrodes. The working electrodes, counter electrodes, and reference electrodes were placed in 0.08 M FeCl 2 +0.08M CoCl 2 The solution was stirred at 160 rpm with a magnetic stirrer and connected to an electrochemical workstation. Fe-Co was deposited onto the TiCuO amorphous nanotubes by electrochemical pulse deposition. The pulse deposition conditions were: negative current -40 mA / cm 2 (8ms), positive current 50mA / cm 2 (2ms), pulse interval 90ms, cycle number 800.

[0071] The TiCuO amorphous nanotubes on which Fe-Co was deposited were taken out, washed in deionized water for 60 seconds, and dried naturally at room temperature to obtain the desired (Fe-Co) / TiCuO nanocomposite electrode material.

[0072] Example 7

[0073] S1: Preparation of titanium-based amorphous alloy nanotubes

[0074] The purity of 99.99% Ti and Cu is Ti 60 Cu 40The required mass was weighed and put into an arc melting furnace. The alloy was repeatedly melted 5 times in a high-purity argon atmosphere, and magnetic stirring was turned on to ensure that the alloy elements were evenly mixed. The alloy ingot was taken out, the surface oxide layer was polished to remove it, and 5g was put into a quartz tube. In a high-purity argon atmosphere, a strip with a width of about 1mm and a thickness of about 20μm was prepared by spinning the strip. A small part was cut and welded with nickel wire, and the welding place was painted with ordinary nail polish, and the exposed surface area of ​​the strip was ensured to be 0.3cm 2 The prepared sample was used as the anode and the platinum sheet was used as the counter electrode in about 50 ml of ethylene glycol electrolyte with 0.2 wt% NH 4 F+2.0vol%H 2 O was polarized at a constant voltage of 15 V for 4 h using an electrochemical workstation, and then taken out and ultrasonically cleaned in deionized water for 5 s, and then cleaned with anhydrous ethanol to obtain TiCuO amorphous nanotubes.

[0075] S2: Preparation of (Mn-Co) / TiCuO nanocomposite electrode materials

[0076] The TiCuO amorphous nanotubes obtained in step S1 were used as working electrodes, the Pt sheet was used as counter electrodes, and the saturated calomel electrode was used as reference electrodes. The working electrodes, counter electrodes, and reference electrodes were placed in 0.05 M MnCl 2 +0.15M CoCl 2 The solution was stirred at 160 rpm with a magnetic stirrer at a temperature of 35 °C and connected to an electrochemical workstation to deposit Mn-Co onto the TiCuO amorphous nanotubes by electrochemical pulse deposition. The pulse deposition conditions were: negative current -80 mA / cm 2 (8ms), positive current 60mA / cm 2 (2ms), pulse interval 90ms, cycle number 500.

[0077] The TiCuO amorphous nanotubes on which Mn-Co was deposited were taken out, washed in deionized water for 60 seconds, and dried naturally at room temperature to obtain the desired (Mn-Co) / TiCuO nanocomposite electrode material.

[0078] Example 8

[0079] S1: Preparation of titanium-based amorphous alloy nanotubes

[0080] The purity of 99.99% Ti and Cu is Ti 60 Cu 40The required mass was weighed and put into an arc melting furnace. The alloy was repeatedly melted 5 times in a high-purity argon atmosphere, and magnetic stirring was turned on to ensure that the alloy elements were evenly mixed. The alloy ingot was taken out, the surface oxide layer was polished to remove it, and 5g was put into a quartz tube. In a high-purity argon atmosphere, a strip with a width of about 1mm and a thickness of about 20μm was prepared by spinning the strip. A small part was cut and welded with nickel wire, and the welding place was painted with ordinary nail polish, and the exposed surface area of ​​the strip was ensured to be 0.3cm 2 The prepared sample was used as the anode and the platinum sheet was used as the counter electrode in about 50 ml of ethylene glycol electrolyte with 0.2 wt% NH 4 F+2.0vol%H 2 O was polarized at a constant voltage of 15 V for 4 h using an electrochemical workstation, and then taken out and ultrasonically cleaned in deionized water for 5 s, and then cleaned with anhydrous ethanol to obtain TiCuO amorphous nanotubes.

[0081] S2: Preparation of (Ni-Cu) / TiCuO nanocomposite electrode materials

[0082] The TiCuO amorphous nanotubes obtained in step S1 were used as working electrodes, the Pt sheet was used as counter electrodes, and the saturated calomel electrode was used as reference electrodes. The working electrodes, counter electrodes, and reference electrodes were placed in a 0.07 M NiCl 2 +0.07M CuCl 2 The solution was stirred at 160 rpm with a magnetic stirrer and connected to an electrochemical workstation. Ni-Cu was deposited onto the TiCuO amorphous nanotubes by electrochemical pulse deposition. The pulse deposition conditions were: negative current -65 mA / cm 2 (8ms), positive current 30mA / cm 2 (2ms), pulse interval 60ms, cycle number 1000.

[0083] The TiCuO amorphous nanotubes on which Ni-Cu was deposited were taken out, washed in deionized water for 60 seconds, and dried naturally at room temperature to obtain the desired (Ni-Cu) / TiCuO nanocomposite electrode material.

[0084] Example 9

[0085] S1: Preparation of titanium-based amorphous alloy nanotubes

[0086] The purity of 99.99% Ti and Cu is Ti 60 Cu 40The required mass was weighed and put into an arc melting furnace. The alloy was repeatedly melted 5 times in a high-purity argon atmosphere, and magnetic stirring was turned on to ensure that the alloy elements were evenly mixed. The alloy ingot was taken out, the surface oxide layer was polished to remove it, and 5g was put into a quartz tube. In a high-purity argon atmosphere, a strip with a width of about 1mm and a thickness of about 20μm was prepared by spinning the strip. A small part was cut and welded with nickel wire, and the welding place was painted with ordinary nail polish, and the exposed surface area of ​​the strip was ensured to be 0.3cm 2 The prepared sample was used as the anode and the platinum sheet was used as the counter electrode in about 50 ml of ethylene glycol electrolyte with 0.2 wt% NH 4 F+2.0vol%H 2 O was polarized at a constant voltage of 15 V for 4 h using an electrochemical workstation, and then taken out and ultrasonically cleaned in deionized water for 5 s, and then cleaned with anhydrous ethanol to obtain TiCuO amorphous nanotubes.

[0087] S2: Preparation of (Fe-Cu) / TiCuO nanocomposite electrode materials

[0088] The TiCuO amorphous nanotubes obtained in step S1 were used as working electrodes, the Pt sheet was used as counter electrodes, and the saturated calomel electrode was used as reference electrodes. The working electrodes, counter electrodes, and reference electrodes were placed in 0.03 M FeCl 2 +0.03M CuCl 2 The solution was stirred at 160 rpm with a magnetic stirrer and connected to an electrochemical workstation. Fe-Cu was deposited onto the TiCuO amorphous nanotubes by electrochemical pulse deposition. The pulse deposition conditions were: negative current -65 mA / cm 2 (8ms), positive current 30mA / cm 2 (2ms), pulse interval 60ms, cycle number 1000.

[0089] The TiCuO amorphous nanotubes on which Fe-Cu was deposited were taken out, washed in deionized water for 60 seconds, and dried naturally at room temperature to obtain the desired (Fe-Cu) / TiCuO nanocomposite electrode material.

[0090] Example 10

[0091] S1: Preparation of titanium-based amorphous alloy nanotubes

[0092] The purity of 99.99% Ti and Cu is Ti 60 Cu 40The required mass was weighed and put into an arc melting furnace. The alloy was repeatedly melted 5 times in a high-purity argon atmosphere, and magnetic stirring was turned on to ensure that the alloy elements were evenly mixed. The alloy ingot was taken out, the surface oxide layer was polished to remove it, and 5g was put into a quartz tube. In a high-purity argon atmosphere, a strip with a width of about 1mm and a thickness of about 20μm was prepared by spinning the strip. A small part was cut and welded with nickel wire, and the welding place was painted with ordinary nail polish, and the exposed surface area of ​​the strip was ensured to be 0.3cm 2 The prepared sample was used as the anode and the platinum sheet was used as the counter electrode in about 50 ml of ethylene glycol electrolyte with 0.2 wt% NH 4 F+2.0vol%H 2 O was polarized at a constant voltage of 15 V for 4 h using an electrochemical workstation, and then taken out and ultrasonically cleaned in deionized water for 5 s, and then cleaned with anhydrous ethanol to obtain TiCuO amorphous nanotubes.

[0093] S2: Preparation of (Mn-Cu) / TiCuO nanocomposite electrode materials

[0094] The TiCuO amorphous nanotubes obtained in step S1 were used as working electrodes, the Pt sheet was used as counter electrodes, and the saturated calomel electrode was used as reference electrodes. The working electrodes, counter electrodes, and reference electrodes were placed in 0.02 M MnCl 2 +0.02M CuCl 2 The solution was stirred at 160 rpm with a magnetic stirrer at a temperature of 35 °C and connected to an electrochemical workstation to deposit Mn-Cu onto the TiCuO amorphous nanotubes by electrochemical pulse deposition. The pulse deposition conditions were: negative current -65 mA / cm 2 (8ms), positive current 55mA / cm 2 (2ms), pulse interval 100ms, cycle number 600.

[0095] The TiCuO amorphous nanotubes on which Mn-Cu was deposited were taken out, washed in deionized water for 60 seconds, and dried naturally at room temperature to obtain the desired (Mn-Cu) / TiCuO nanocomposite electrode material.

[0096] Comparative Example 1

[0097] S1: Preparation of titanium-based amorphous alloy nanotubes

[0098] The purity of 99.99% Ti and Cu is Ti 60 Cu 40The required mass is weighed and put into an arc melting furnace. The alloy is repeatedly melted 5 times in an atmosphere of high-purity argon, and magnetic stirring is turned on to ensure that the alloy elements are evenly mixed; the alloy ingot is taken out, the surface oxide layer is polished to remove it, and 5g is put into a quartz tube, and a strip with a width of about 1mm and a thickness of about 20μm is prepared by spinning in an atmosphere of high-purity argon; a small part is cut and welded with a nickel wire, and the welding part is painted with ordinary nail polish, and the exposed surface area of ​​the strip is ensured to be 0.3cm2; the prepared sample is used as the anode and the platinum sheet as the counter electrode. It is placed in about 50ml of ethylene glycol electrolyte 0.2wt% NH4F + 2.0vol% H2O, and a constant voltage of 15V is applied using an electrochemical workstation for polarization for 4h, and the TiCuO amorphous nanotubes are obtained after being taken out and ultrasonically cleaned in deionized water for 5s, and then cleaned with anhydrous ethanol.

[0099] S2: Preparation of Ni / TiCuO nanocomposite electrode materials

[0100] The TiCuO amorphous nanotubes obtained in step S1 were used as working electrodes, the Pt sheet was used as counter electrodes, and the saturated calomel electrode was used as reference electrodes. The working electrodes, counter electrodes, and reference electrodes were placed in a 0.02 M NiCl 2 The solution was stirred at 150 rpm with a magnetic stirrer and connected to an electrochemical workstation. Ni was deposited onto the TiCuO amorphous nanotubes by electrochemical pulse deposition. The pulse deposition conditions were: negative current -50 mA / cm 2 (8ms), positive current 40mA / cm 2 (2ms), pulse interval 100ms, number of cycles 1000.

[0101] The TiCuO amorphous nanotubes on which Ni was deposited were taken out, washed in deionized water for 60 seconds, and dried naturally at room temperature to obtain the desired Ni / TiCuO nanocomposite electrode material.

[0102] Comparative Example 2

[0103] S1: Preparation of titanium-based amorphous alloy nanotubes

[0104] The purity of 99.99% Ti and Cu is Ti 60 Cu 40The required mass is weighed and put into an arc melting furnace. The alloy is repeatedly melted 5 times in an atmosphere of high-purity argon, and magnetic stirring is turned on to ensure that the alloy elements are evenly mixed; the alloy ingot is taken out, the surface oxide layer is polished to remove it, and 5g is put into a quartz tube, and a strip with a width of about 1mm and a thickness of about 20μm is prepared by spinning in an atmosphere of high-purity argon; a small part is cut and welded with a nickel wire, and the welding part is painted with ordinary nail polish, and the exposed surface area of ​​the strip is ensured to be 0.3cm2; the prepared sample is used as the anode and the platinum sheet as the counter electrode. It is placed in about 50ml of ethylene glycol electrolyte 0.2wt% NH4F + 2.0vol% H2O, and a constant voltage of 15V is applied using an electrochemical workstation for polarization for 4h, and the TiCuO amorphous nanotubes are obtained after being taken out and ultrasonically cleaned in deionized water for 5s, and then cleaned with anhydrous ethanol.

[0105] S2: Preparation of Co / TiCuO nanocomposite electrode materials

[0106] The TiCuO amorphous nanotubes obtained in step S1 were used as working electrodes, the Pt sheet was used as counter electrodes, and the saturated calomel electrode was used as reference electrodes. The working electrodes, counter electrodes, and reference electrodes were placed in a 0.02 M CoCl 2 The solution was stirred at 150 rpm with a magnetic stirrer and connected to an electrochemical workstation. Co was deposited onto the TiCuO amorphous nanotubes by electrochemical pulse deposition. The pulse deposition conditions were: negative current -50 mA / cm 2 (8ms), positive current 40mA / cm 2 (2ms), pulse interval 100ms, number of cycles 1000.

[0107] The TiCuO amorphous nanotubes on which Co was deposited were taken out, washed in deionized water for 60 seconds, and dried naturally at room temperature to obtain the desired Co / TiCuO nanocomposite electrode material.

[0108]

Characterization

[0109] 1. SEM, TEM and EDS

[0110] Figure 1 and Figure 2 : is a SEM picture of TiCuO amorphous nanotubes. It can be seen from the picture that the TiCuO amorphous nanotubes are open at the upper end surface and are composed of multiple TiCuO amorphous alloy nanotubes neatly arranged into a nanotube array structure.

[0111] Figure 3 This is a SEM image of the (Ni-Co) / TiCuO nanocomposite electrode material obtained in Example 1. It can be seen from the image that the Ni-Co bimetallic element forms a nano-network structure on the surface of the TiCuO amorphous nanotubes; Figure 4This is the TEM scan image corresponding to the (Ni-Co) / TiCuO nanocomposite electrode material. Figure 4 It can be seen that the 2 areas between the two horizontal lines are closely arranged nanotube structures in the longitudinal direction, the 3 areas below the lower horizontal line are TiCu amorphous alloy substrates, and the 1 area above the upper horizontal line is a nano-network structure formed by Ni-Co bimetallic co-deposition, which is consistent with the SEM image; Figure 5a , 5b It can be clearly observed from Figure 5c that the elements co-deposited on the titanium-based nanotubes are Ni and Co, and some of them enter the interior of the nanotubes; and the EDS results show that the Ni content is 9.10 at.%, and the Co content is 33.83 at.%

[0112] Figure 6-Figure 1410. The SEM images of the nanocomposite electrode materials obtained in Examples 2-10 are shown in Figures. As can be seen from the figure, in the nanocomposite electrode material obtained in Example 2, the Ni-Fe bimetallic elements form a nano-cotton-like structure on the surface of the amorphous nanotubes, wherein the content of the Ni element is 29.21 at.%, and the content of the Fe element is 12.03 at.%; in the nanocomposite electrode material obtained in Example 3, the Ni-Mn bimetallic elements form a nano-fragment structure on the surface of the amorphous nanotubes, wherein the content of the Ni element is 19.32 at.%, and the content of the Mn element is 21.83 at.%; In the nanocomposite electrode material obtained in Example 5, the Co-Cu bimetallic elements form a nano-cheese structure on the surface of the amorphous nanotubes, wherein the content of the Co element is 20.11 at.%, and the content of the Cu element is 21.33 at.%. In the nanocomposite electrode material obtained in Example 6, the Fe-Co bimetallic elements form a nano-particle structure on the surface of the amorphous nanotubes, wherein the content of the Fe element is 10.34 at.%, and the content of the Mn element is 32.66 at.%. The content of Fe element is 12.44at.%, ​​and the content of Co element is 29.79at.%; in the nanocomposite electrode material obtained in Example 7, the Mn-Co bimetallic element forms a nanoworm-like structure on the surface of the amorphous nanotube, wherein the content of Fe element is 7.39at.%, ​​and the content of Co element is 35.22at.%; in the nanocomposite electrode material obtained in Example 8, the Ni-Cu bimetallic element forms a nanobud structure on the surface of the amorphous nanotube, wherein the content of Ni element is 17.54at.%, ​​and the content of Cu element is 25.01at.%; in the nanocomposite electrode material obtained in Example 9, the Mn-Co bimetallic element forms a nanoworm-like structure on the surface of the amorphous nanotube, wherein the content of Fe element is 7.39at.%, ​​and the content of Co element is 35.22at.%; In the nanocomposite electrode material obtained in Example 10, the Fe-Cu bimetallic elements form a nano-bud structure on the surface of the amorphous nanotubes, wherein the content of Fe element is 25.36at.%, and the content of Cu element is 17.88at.%. In the nanocomposite electrode material obtained in Example 10, the Mn-Cu bimetallic elements form a nano-particle structure on the surface of the amorphous nanotubes, wherein the content of Mn element is 13.84at.%, and the content of Cu element is 27.91at.%. It can be seen from EDS that in the materials obtained in each embodiment, the nanostructure formed on the surface of the TiCuO amorphous nanotube is composed of the target deposited metal elements.

[0113] 2. Specific surface area

[0114] Fig.15The electrochemically active area of ​​the four samples of (Ni-Co) / TiCuO nanocomposite electrode material, TiCuO amorphous nanotubes, Ni / TiCuO nanocomposite electrode material obtained in Example 1, and Co / TiCuO nanocomposite electrode material obtained in Comparative Example 2 is fitted straight line. The electrochemically active area (i.e., specific surface area) can be determined according to the slope of the straight line. Half of the slope of the straight line is the capacitance value C. dl , the capacitance value C dl Dividing it by the standard capacitance (0.04 mF) gives the specific surface area of ​​the electrode material. The specific surface areas are: (Ni-Co) / TiCuO nanocomposite electrode material is 57.25 cm -2 , Ni / TiCuO nanocomposite electrode material is 16.25cm -2 , Co / TiCuO nanocomposite electrode material is 3.15cm -2 , TiCuO amorphous nanotubes are 2.28 cm -2 , that is, the specific surface area of ​​(Ni-Co) / TiCuO nanocomposite electrode material is 25 times that of TiCuO amorphous nanotubes.

[0115] The specific surface areas of the (Ni-Fe) / TiCuO nanocomposite electrode materials obtained in Example 2 were 33.25 cm -2 , which is 14 times that of TiCuO amorphous nanotubes; the specific surface areas of the (Ni-Mn) / TiCuO nanocomposite electrode materials obtained in Example 3 are 41.38 cm -2 , which is 18 times that of TiCuO amorphous nanotubes; the specific surface areas of the (Co-Cu) / TiCuO nanocomposite electrode materials obtained in Example 4 are 45.11 cm -2 , which is 19 times that of TiCuO amorphous nanotubes; the specific surface areas of the (Fe-Mn) / TiCuO nanocomposite electrode materials obtained in Example 5 are 26.42 cm -2 , which is 11 times that of TiCuO amorphous nanotubes; the specific surface areas of the (Fe-Co) / TiCuO nanocomposite electrode materials obtained in Example 6 are 35.89 cm -2 , which is 15 times that of TiCuO amorphous nanotubes; the specific surface areas of the (Mn-Co) / TiCuO nanocomposite electrode materials obtained in Example 7 are 45.64 cm -2 , which is 20 times that of TiCuO amorphous nanotubes; the specific surface areas of the (Ni-Cu) / TiCuO nanocomposite electrode materials obtained in Example 8 are 25.71 cm -2 , which is 11 times that of TiCuO amorphous nanotubes; the specific surface areas of the (Fe-Cu) / TiCuO nanocomposite electrode materials obtained in Example 9 are 30.27 cm -2, which is 13 times that of TiCuO amorphous nanotubes; the specific surface areas of the (Mn-Cu) / TiCuO nanocomposite electrode materials obtained in Example 10 are 36.47 cm -2 , which is 16 times that of TiCuO amorphous nanotubes.

[0116] From the above results, it can be seen that the specific surface area of ​​the TiCuO amorphous nanotubes deposited with bimetallic elements is larger than the surface area of ​​the original TiCuO amorphous nanotubes, which is 11-25 times the specific surface area of ​​the TiCuO amorphous alloy nanotubes.

[0117]

Performance test

[0118] The (Ni-Co) / TiCuO nanocomposite electrode material, TiCuO amorphous nanotubes, Ni / TiCuO nanocomposite electrode material obtained in Example 1, and Co / TiCuO nanocomposite electrode material obtained in Comparative Example 2 were used as electrodes, and the performance of each electrode material on the catalytic oxidation of glucose was tested by cyclic voltammetry and chronoamperometry. Glucose solutions of different concentrations were dropped into each electrode material for current response. The current response curve of each electrode material was fitted with the glucose concentration. The slope of the fitting curve represents the sensitivity of the electrode material to glucose sensing. The larger the slope, the higher the sensitivity. The results are shown in FIG. Fig.15 As shown, it can be seen that the sensitivity of the electrode materials to glucose sensing is from high to low: (Ni-Co) / TiCuO nanocomposite electrode material>Ni / TiCuO nanocomposite electrode material>Co / TiCuO nanocomposite electrode material>TiCuO amorphous nanotubes.

[0119] The detection limit refers to the corresponding amount of 3 times the value of the instrument background signal generated by the matrix blank, or the average value of the background signal generated by the matrix blank plus 3 times the mean standard deviation. According to the formula L = kSb / S, (where Sb is the standard deviation of multiple blank measurements; S is the sensitivity of the determination method, that is, the slope obtained above; k is a coefficient determined according to a certain confidence level, generally 3.29), it can be obtained that the detection limit of (Ni-Co) / TiCuO nanocomposite electrode material is 0.041μM, the detection limit of Ni / TiCuO nanocomposite electrode material is 0.052μM, the detection limit of Co / TiCuO nanocomposite electrode material is 0.183μM, and the detection limit of TiCuO amorphous nanotubes is 0.290μM. It can be seen that the detection limit of (Ni-Co) / TiCuO nanocomposite electrode material is the lowest.

[0120] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. A person with ordinary knowledge in the technical field to which the present invention belongs may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the definition of the claims.

Claims

1. A nanocomposite electrode material for improving glucose sensing performance, characterized in that: The nanocomposite electrode material has a composite structure formed by a double-layer nanostructure, wherein the double-layer nanostructure includes a bottom structure and a surface structure, wherein the bottom structure is a titanium-based amorphous alloy nanotube with an open upper end surface, and the surface structure is a nanostructure formed by two transition metal elements, and the surface structure is attached to the upper end surface of the titanium-based amorphous alloy nanotube; The nanostructure of the surface layer is any one of a nano-net structure, a nano-cotton structure, a nano-fragment structure, a nano-cheese structure, a nano-ball structure, a nano-particle structure, a nano-worm structure, and a nano-bud structure; The transition metal elements are any two of Mn, Fe, Co, Ni and Cu. The nanostructure formed by the two transition metal elements penetrates deeply into the nanotubes, thereby enhancing the adhesion to the nanotubes and increasing the specific surface area of ​​the electrode material, thereby enhancing the structural stability of the composite electrode material during operation, improving the sensitivity of the composite material in detecting glucose and reducing the detection limit.

2. The nanocomposite electrode material for improving glucose sensing performance according to claim 1, characterized in that: The titanium-based amorphous alloy nanotubes include a plurality of TiCuO amorphous alloy nanotubes, and the plurality of TiCuO amorphous alloy nanotubes are neatly arranged into a nanotube array structure.

3. The nanocomposite electrode material for improving glucose sensing performance according to any one of claims 1 to 2, characterized in that: The specific surface area of ​​the electrode material is 11-25 times that of the TiCuO amorphous alloy nanotube.

4. A method for preparing a nanocomposite electrode material for improving glucose sensing performance according to any one of claims 1 to 3, characterized in that: The specific steps include: S1: Preparation of titanium-based amorphous alloy nanotubes Using titanium-copper amorphous alloy strips as substrate, TiCuO amorphous nanotubes were prepared by anodization. S2: Preparation of Nanocomposite Electrode Materials The TiCuO amorphous nanotubes obtained in step S1 are used as working electrodes, the Pt sheet is used as counter electrodes, and the saturated calomel electrode is used as reference electrodes. The working electrodes, counter electrodes, and reference electrodes are placed in a deposition solution and connected to an electrochemical workstation to deposit metals onto the TiCuO amorphous nanotubes by an electrochemical pulse deposition method; The TiCuO amorphous nanotubes with deposited metal are taken out, washed in deionized water, and dried naturally at room temperature to obtain the desired nanocomposite electrode material.

5. The method for preparing a nanocomposite electrode material for improving glucose sensing performance according to claim 4, characterized in that: The deposition solution in step S2 is a 0.01M-0.3M chloride salt solution of two transition metal elements, and the molar ratio of the two metals is 1:(1-3).

6. The method for preparing a nanocomposite electrode material for improving glucose sensing performance according to claim 4, characterized in that: In step S2, the parameters of the electrochemical pulse deposition method are: pulse positive current density: +40 ~ +80 mA / cm 2 , duration 2-5 ms; pulse positive current density: -30 ~ -80mA / cm 2 , duration 8-12 ms; cycle: 500~1000; pulse interval: 50-100 ms.

7. The method for preparing a nanocomposite electrode material for improving glucose sensing performance according to claim 4 or 5, characterized in that: The temperature of the deposition solution was 35-40° C. and the solution was stirred with a magnetic stirrer at a stirring speed of 140-160 rpm.

8. The method for preparing a nanocomposite electrode material for improving glucose sensing performance according to claim 4, characterized in that: In step S2, the TiCuO amorphous nanotubes with deposited metal are washed in deionized water for 30-60 seconds.

9. The method for preparing a nanocomposite electrode material for improving glucose sensing performance according to claim 4, characterized in that: The preparation method in step S1 is as follows: Ti 60 Cu 40 The metal single substance is smelted to obtain the master alloy, and then the master alloy is rapidly cooled and spun through a high-speed rotating copper roller to obtain Ti 60 Cu 40 Amorphous alloy strip, Ti 60 Cu 40 The amorphous alloy strips were subjected to constant potential polarization treatment in ethylene glycol electrolyte and then washed with deionized water and anhydrous ethanol to obtain TiCuO amorphous nanotubes.