A flexible ultrasonic sensor based on nano zinc oxide composite material
By using nano zinc oxide composite material as the piezoelectric layer in a flexible ultrasonic sensor and combining with a flexible substrate, the fracture and warping problems of traditional ultrasonic sensors in a bending state is solved, and the flexibility and robustness of the equipment are improved, and the flexibility and robustness of the equipment are achieved. High-sensitivity ultrasound detection effect is suitable for wearable devices in modern medicine.
Patent Information
- Application Number
- CN202210277798.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The piezoelectric layer of traditional flexible ultrasonic sensors is prone to breaking and warping in a bending state, affecting its working performance and stability. The combination effect of the flexible substrate and the piezoelectric layer is not good, making it difficult to meet the needs of modern medicine for wearable devices.
Using nano zinc oxide composite material as piezoelectric layer, nano zinc oxide structures are prepared by hydrothermal growth method, and flexible colloids are filled therebetween, combined with flexible substrates to form a high-sensitivity ultrasonic sensor to ensure that there is no damage in large deformation and bending states. and improve electromechanical conversion efficiency.
The high flexibility, robustness and bending strength of ultrasonic sensors are achieved, the ability to detect any surface shape targets is enhanced, the preparation cost and process complexity are reduced, and it is suitable for large-scale production.
Smart Images

Figure CN114652347B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a flexible ultrasonic sensor based on a nano zinc oxide composite material, and belongs to the field of ultrasonic sensors and micro-nano processing. Background Art
[0002] With the advancement of modern medicine and ultrasonic imaging technology, the application scope of ultrasonic sensors is becoming increasingly broad. However, for some detection objects that require wearable devices (such as human skin, eyes, etc.), the rigid structure of traditional ultrasonic sensors no longer meets the requirements. Therefore, ultrasonic sensors with flexible structures have become a new direction that urgently needs breakthroughs and development in the field of modern medicine. Flexible ultrasonic sensors can bend and deform, so they can be attached to surfaces of any shape for detection, or they can be prepared into wearable devices for detection on the human body. At present, many researchers have proved that flexible ultrasonic sensors can realize real-time monitoring of human physiological signals, and have the characteristics of high efficiency, stability, and wide applicability in practical applications.
[0003] Commonly used flexible ultrasonic sensors mostly use flexible substrates to increase their tensile strength and bending strength, but the piezoelectric layer is mostly a rigid piezoelectric material, and different degrees of shape changes will still affect the working performance and stability of the piezoelectric layer. Therefore, the improvement of flexible ultrasonic sensors not only needs to start from the flexible substrate, but also needs to improve the traditional piezoelectric layer to make it more flexible and robust, while maintaining a high electromechanical conversion efficiency. Zinc oxide film has the advantages of mature preparation technology, low cost, low toxicity, good piezoelectricity, and easy graphics. Therefore, it is very suitable as the piezoelectric layer of ultrasonic sensors. However, zinc oxide film will still have problems such as breakage and warping due to stress in the bent state. Therefore, in order to achieve an effective combination of zinc oxide film and flexible substrate, it is still necessary to explore the reasonable structure and new preparation methods of zinc oxide film. Summary of the invention
[0004] In view of the above technical problems, the present invention discloses a flexible ultrasonic sensor based on a nano zinc oxide composite material. The flexible ultrasonic sensor is mainly composed of a flexible substrate, a nano zinc oxide composite material, an acoustic matching layer and an electrode. The nano zinc oxide composite material serves as a piezoelectric layer and is composed of a nano zinc oxide structure and a flexible colloid, wherein the nano zinc oxide structure is prepared by a hydrothermal growth method, and the flexible colloid is filled in the nano zinc oxide structure. Based on the structure of the flexible substrate and the nano zinc oxide composite material, the robustness, flexibility and bending strength of the ultrasonic sensor can be improved, and the sensor has high sensitivity, so that conformal ultrasonic detection can be performed on targets of arbitrary curved shapes.
[0005] The purpose of the present invention is achieved through the following technical solutions.
[0006] A flexible ultrasonic sensor based on a nano zinc oxide composite material comprises a flexible substrate, an electrode, a nano zinc oxide composite material and an acoustic matching layer; the nano zinc oxide composite material consists of a nano zinc oxide structure and a flexible colloid; the nano zinc oxide composite material is placed between two electrode layers and is placed on the flexible substrate as a whole; the acoustic matching layer is located above the top electrode.
[0007] The nano zinc oxide structure is prepared by a hydrothermal growth method, and its nanoscale linear structure ensures that the zinc oxide material will not undergo destructive deformations such as breakage and warping under large deformation bending conditions; the flexible colloid is filled in the nano zinc oxide structure, ensuring that the entire sensor has good robustness, which is conducive to achieving close contact between double-sided electrodes and can achieve the effect of improving the electromechanical conversion efficiency.
[0008] The nano zinc oxide structure comprises nano wires, nano rods, nano needles and nano cones, the thickness of which is 1 to 100 μm and the top diameter is less than 1 μm.
[0009] The hydrothermal method for growing the nano zinc oxide thick film comprises: placing the sample in a chemical reaction kettle for thick film growth or placing the sample in a microchannel for thick film growth.
[0010] The flexible colloid includes polyimide, polystyrene, SU-8 and PDMS.
[0011] The flexible colloid filling method includes spin coating, spray coating and sputtering.
[0012] The flexible substrate is a polymer material including polyimide, PDMS, polyethylene terephthalate and polystyrene, with a thickness of not less than 50 μm, a tensile strength of not less than 10 MPa, and a bending strength of not less than 10 MPa.
[0013] The electrode comprises a top electrode and a bottom electrode, wherein the bottom electrode is located between the flexible substrate and the piezoelectric layer, and the top electrode is located between the piezoelectric layer and the matching layer. The electrode materials comprise gold, chromium, titanium, aluminum, silver and copper, and the thickness is not less than 100 nm.
[0014] The acoustic matching layer is one or more layers of material. The material and thickness of the acoustic matching layer are designed according to the acoustic impedance of the piezoelectric material and the detected object, so that the acoustic impedance of the acoustic matching layer is between the impedance of the piezoelectric material and the detected target. According to traditional theory, the piezoelectric material and the detected target medium are regarded as semi-infinite, and the impedance of the piezoelectric material and the detected target are respectively Z p and Z m , the acoustic impedance of the i-th matching layer is Z i , then the acoustic impedance of the matching layer satisfies the following formula when the single layer is matched:
[0015]
[0016] The acoustic matching layer is prepared on the top electrode, or the acoustic matching layer is directly adhered to the top electrode, and the matching layer acts as an electrical insulating layer and a sealing layer at the same time.
[0017] A method for preparing a flexible ultrasonic sensor based on nano zinc oxide composite material is as follows:
[0018] Step 1: Select a flexible substrate and clean it; use acetone, alcohol, and deionized water to ultrasonically clean the substrate in sequence, and then use nitrogen to blow clean the surface;
[0019] Step 2: prepare a bottom electrode on a flexible substrate; use magnetron sputtering to uniformly deposit one or more layers of metal material on the substrate, and the vacuum degree of the substrate is less than 1×10 -3 Pa, ignition gas pressure 5-10Pa, sputtering power 50-250W, the thickness of the bottom electrode is controlled by controlling the sputtering time;
[0020] Step 3: Prepare a piezoelectric layer on the bottom electrode. First, a zinc oxide seed layer is prepared on the bottom electrode by magnetron sputtering. The thickness of the seed layer does not exceed 800 nm. The vacuum degree of the substrate is less than 1×10 -3 Pa, ignition pressure 5-10Pa, sputtering power 50-100W, flow ratio of argon to oxygen 5-8:1, and thickness of zinc oxide is controlled by controlling sputtering time; then a layer of nano zinc oxide thick film is prepared on the seed layer by hydrothermal growth method; the reaction solution includes alkali solution and zinc nitrate solution, the molar ratio of zinc ions to hydroxide ions in the reaction solution is 1:4-8, the growth temperature is 60-100 degrees Celsius, and thickness of synthesized zinc oxide is controlled by controlling reaction time; synthesized zinc oxide crystals grow along C axis, with certain gaps between crystals;
[0021] Step 4: Fill the gaps between zinc oxide crystals with flexible colloid to ensure that a smooth and dense filling surface is obtained in the end;
[0022] Step 5: prepare a top electrode on the piezoelectric layer; use magnetron sputtering to uniformly deposit one or more layers of metal material on the substrate; the vacuum degree of the substrate is less than 1×10 -3 Pa, ignition gas pressure 5-10Pa, sputtering power 50-250W, the thickness of the top electrode is controlled by controlling the sputtering time;
[0023] Step 6: preparing an acoustic matching layer on the top electrode;
[0024] Step 7: Lead out the upper and lower electrodes, and perform electrical insulation and sealing packaging on the prepared sensor as a whole to obtain a flexible ultrasonic sensor.
[0025] Beneficial effects:
[0026] 1. The flexibility and bending strength of ultrasonic sensors can be improved by combining flexible substrates with nano zinc oxide composite materials.
[0027] 2. The composite material composed of nano zinc oxide structure and flexible colloid can not only increase the flexibility and robustness of the piezoelectric layer, but also achieve a higher piezoelectric coefficient and improve the detection sensitivity.
[0028] 3. Compared with the traditional magnetron sputtering and vapor deposition methods for preparing zinc oxide, the hydrothermal method for preparing zinc oxide has simple steps, less time consumption, and low cost. It uses microfluidics and peristaltic pump control to flexibly adjust the formula and local concentration of the reaction solution to achieve control of the morphology of nano-zinc oxide.
[0029] 4. The flexible ultrasonic sensors proposed in the present invention are all prepared using micro-nano processing technology, which is mature, highly repeatable, and suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Flow chart of the preparation of flexible ultrasonic sensors based on zinc oxide nanowire composites;
[0031] Figure 2 Schematic diagram of a flexible ultrasonic sensor based on zinc oxide nanowire composite material;
[0032] Figure 3 Schematic diagram of the device for growing nano zinc oxide using the hydrothermal method using microfluidics and peristaltic pumps;
[0033] Figure 4 Schematic diagram of a flexible ultrasonic sensor based on zinc oxide nanocone composite material;
[0034] Figure 5 Flow chart of the preparation of flexible ultrasonic sensors based on ZnO nanocone composites;
[0035] Figure 6 Schematic diagram of the device for growing nano zinc oxide using the hydrothermal method in a chemical reactor.
[0036] Among them, 1 is a flexible substrate, 2 is a bottom electrode, 3 is a top electrode, 4 is a nano zinc oxide structure, 5 is a filled flexible colloid, 6 is an acoustic matching layer, 7 is a lead of the electrode, and 8 is an electrically insulating sealed package. DETAILED DESCRIPTION
[0037] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail in conjunction with the following specific examples and drawings.
[0038] Example 1
[0039] The ultrasonic sensor in this embodiment is used for ophthalmic photoacoustic imaging. To balance detection resolution and detection depth, the central operating frequency of the sensor is 30 MHz. The sensor is flexible and can be attached to the surface of the eyeball with coupling fluid.
[0040] like Figure 2 As shown, a flexible ultrasonic sensor based on zinc oxide nanowire composite material includes a flexible substrate, a nano zinc oxide composite material, an acoustic matching layer and an electrode; the nano zinc oxide composite material is composed of a nano zinc oxide structure and a flexible colloid; the nano zinc oxide composite material is placed between two electrode layers and is placed on the flexible substrate as a whole; the acoustic matching layer is located above the top electrode. The flexible substrate is a polyimide with a thickness of 300um and an area of 2cm×2cm, the top electrode and the bottom electrode are both 100nm thick gold films, and the piezoelectric layer is a 40um thick zinc oxide nanowire filled with SU-8 colloid.
[0041] like Figure 1 As shown, the preparation method of the flexible ultrasonic sensor based on zinc oxide nanowire composite material is as follows:
[0042] Step 1: Select a polyimide flexible substrate with a thickness of 300um and an area of 2cm×2cm, and clean the substrate. Use acetone, alcohol, and deionized water to ultrasonically clean the polyimide substrate for 10 minutes in sequence, and then use nitrogen to blow clean the polyimide surface for later use.
[0043] Step 2: Prepare the bottom electrode on the flexible substrate. Use magnetron sputtering to evenly sputter a 100nm thick gold film on the substrate. The sputtering target is a pure gold target with a purity of more than 99.90%. The vacuum degree of the substrate is less than 1×10 -3 Pa, ignition gas pressure 10Pa, sputtering power 50W, and the bottom electrode thickness is controlled by controlling the sputtering time.
[0044] Step 3: Prepare a piezoelectric layer on the bottom electrode. First, a 100nm thick zinc oxide seed layer is prepared on the bottom electrode using magnetron sputtering. The sputtering target is a zinc oxide target with a purity of more than 99.9%, and the base vacuum is less than 1×10 -3 Pa, ignition pressure 10Pa, sputtering power 100W, argon to oxygen flow ratio 8:1, the thickness of zinc oxide is controlled by controlling the sputtering time. The hydrothermal growth of zinc oxide thick film adopts micro-channel and peristaltic pump mode to ensure that the local concentration of zinc oxide remains constant during the growth process to obtain a rod-shaped nanowire structure. The experimental device is as follows Figure 3 As shown. The reaction solution includes ammonia water and zinc nitrate solution, the molar ratio of zinc ions to hydroxide ions is 1:6, the growth temperature is 80 degrees Celsius, and the thickness of the synthesized zinc oxide is controlled by controlling the reaction time. The synthesized zinc oxide crystals grow along the C axis, and there are certain gaps between the crystals.
[0045] Step 4: After the growth is completed, fill the gaps between the zinc oxide crystals with SU-8 colloid by spin coating. Take 4 ml of SU-8 colloid, set the speed of the glue machine to 500 rpm, spin coat for 60 seconds, then 4000 rpm, spin coat for 200 seconds, and ensure that a flat and dense filling surface is obtained. Let it stand for half an hour after the spin coating is completed.
[0046] Step 5: Prepare the top electrode on the piezoelectric layer. Use magnetron sputtering to evenly sputter a 100nm thick gold film on the filled flat surface. The sputtering target is a gold target with a purity of more than 99.90%, and the base vacuum is less than 1×10 -3 Pa, ignition gas pressure 10Pa, sputtering power 50W, and the top electrode thickness is controlled by controlling the sputtering time.
[0047] Step 6: Prepare an acoustic matching layer on the top electrode. The center frequency of the ultrasonic wave is 30 MHz, the transmission wavelength in the acoustic matching layer is about 50 μm, and the thickness of the acoustic matching layer is selected to be 12.5 μm using the quarter-wavelength matching theory.
[0048] According to the traditional theory, the piezoelectric material and the target medium to be detected are regarded as semi-infinite, and the impedance of the piezoelectric material and the target to be detected are Z p and Z m , the acoustic impedance of the i-th matching layer is Z i , then the acoustic impedance of the matching layer satisfies the following formula when the single layer is matched: Here, the ZnO nanocomposite material p About 15×10 6 Kg / (m 2 ·s), Z inside the eyeball m About 1.5×10 6 Kg / (m 2 ·s), according to the calculation, epoxy resin with titanium oxide nanoparticles added is selected as the acoustic matching layer, and its acoustic impedance Z i 4.74×10 6 Kg / (m 2 ·s). The acoustic matching layer is directly bonded to the top electrode and acts as an electrical insulating layer and a sealing layer at the same time.
[0049] Step 7: Lead out the upper and lower electrodes, perform electrical insulation and sealing packaging on the sensor as a whole, and obtain a completed flexible ultrasonic sensor.
[0050] The flexible ultrasonic sensor is flexible and bendable, and as a contact lens-like wearable device, it is easy to use in ophthalmic photoacoustic imaging. Its central operating frequency is about 30 MHz, the response bandwidth is about 20 MHz, and the detection sensitivity is good, filling the gap in wearable ultrasonic sensors in ophthalmology.
[0051] Example 2
[0052] The ultrasonic sensor in this embodiment is used for body surface photoacoustic imaging. In order to balance detection resolution and detection depth, the central operating frequency of the sensor is 50 MHz. The sensor is flexible and can be attached to the skin surface with coupling fluid.
[0053] like Figure 4 As shown, a flexible ultrasonic sensor based on zinc oxide nanocone composite material has a structure similar to that of Example 1, except that 4 is a conical structure; the conical structure is formed by placing a zinc oxide seed layer in a chemical reactor for hydrothermal growth, and the reactive ions are continuously consumed during the growth process, so the reaction concentration in the local area of the chemical reactor will continue to decrease, and eventually the synthesized zinc oxide crystal rod will form a nanoconical structure with a thick bottom and a thin top. The substrate is a PDMS with a thickness of 100um and an area of 2cm×2cm, the top electrode and the bottom electrode are both 100nm thick gold films, and the piezoelectric layer is a 30um thick zinc oxide nanocone filled with polyimide colloid.
[0054] like Figure 5 As shown, the preparation method of the flexible ultrasonic sensor based on zinc oxide nanocone composite material is as follows:
[0055] Step 1: Select a flexible PDMS substrate with a thickness of 100um and an area of 2cm×2cm, and clean the substrate. Use acetone, alcohol, and deionized water to ultrasonically clean the PDMS substrate for 10 minutes, and then use nitrogen to blow the surface clean for later use.
[0056] Step 2: Prepare the bottom electrode on the flexible substrate. Use magnetron sputtering to evenly sputter a 100nm thick gold film on the substrate. The sputtering target is a pure gold target with a purity of more than 99.90%. The vacuum degree of the substrate is less than 1×10 -3 Pa, ignition gas pressure 10Pa, sputtering power 50W, and the bottom electrode thickness is controlled by controlling the sputtering time.
[0057] Step 3: Prepare a piezoelectric layer on the bottom electrode. First, a 200nm thick zinc oxide seed layer is prepared on the bottom electrode using magnetron sputtering. The sputtering target is a zinc oxide target with a purity of more than 99.9%, and the base vacuum is less than 1×10 -3 Pa, ignition pressure 10Pa, sputtering power 100W, flow ratio of argon to oxygen 8:1, and the thickness of zinc oxide is controlled by controlling the sputtering time. After the seed layer is grown, the substrate is placed in a high-pressure reactor and a zinc oxide film is grown using a hydrothermal method. The experimental apparatus is as follows: Figure 6As shown. As the concentration of the reaction reagents is continuously consumed during the growth process, the diameter of the synthesized zinc oxide crystal rod will gradually decrease, and finally form a nano-cone structure with a diameter of thick bottom and thin top. The reaction solution includes ammonia water and zinc nitrate solution, the molar ratio of zinc ions to hydroxide ions is 1:7, the growth temperature is 85 degrees Celsius, and the thickness of the synthesized zinc oxide is controlled by controlling the reaction time. The synthesized zinc oxide crystal grows along the C axis, and there are gaps of different sizes between the crystals.
[0058] Step 4: After the growth is completed, the gaps between the zinc oxide crystals are filled with polyimide colloid by spin coating. Take 4 ml of polyimide colloid, set the speed of the glue machine to 500 rpm, spin coat for 60 seconds, then 4000 rpm, spin coat for 180 seconds, to ensure that a flat and dense filling surface is obtained. After spin coating, let it stand for half an hour.
[0059] Step 5: Prepare the top electrode on the piezoelectric layer. Use magnetron sputtering to evenly sputter a 100nm thick gold film on the filled flat surface. The sputtering target is a gold target with a purity of more than 99.90%, and the base vacuum is less than 1×10 -3 Pa, ignition gas pressure 10Pa, sputtering power 50W, and the top electrode thickness is controlled by controlling the sputtering time.
[0060] Step 6: Prepare an acoustic matching layer on the top electrode. The center frequency of the ultrasound wave is 50 MHz, and the transmission wavelength in the acoustic matching layer is about 30 μm. Using the quarter-wavelength matching theory, the thickness of the acoustic matching layer is selected to be 7.5 μm. According to the traditional theory, the piezoelectric material and the target medium to be detected are regarded as semi-infinite, and the impedance of the piezoelectric material and the target to be detected are Z p and Z m , the acoustic impedance of the i-th matching layer is Z i , then the acoustic impedance of the matching layer satisfies the following formula when the single layer is matched: Here, the ZnO nanocomposite material p About 15×10 6 Kg / (m 2 ·s), Z inside the skin m About 1.5×10 6 Kg / (m 2 ·s), according to the calculation, SU-8 glue with titanium oxide nanoparticles added is selected as the acoustic matching layer, and its acoustic impedance Z i 4.74×10 6 Kg / (m 2 ·s). The acoustic matching layer is directly bonded to the top electrode and acts as an electrical insulating layer and a sealing layer at the same time.
[0061] Step 7: Lead out the upper and lower electrodes, perform electrical insulation and sealing packaging on the sensor as a whole, and obtain a completed flexible ultrasonic sensor.
[0062] The flexible ultrasonic sensor is flexible and bendable, and is easy to use as a wearable device in photoacoustic imaging of the body surface. Its central operating frequency is about 50 MHz, the response bandwidth is about 30 MHz, and the detection sensitivity is good, filling the gap in wearable high-resolution ultrasonic sensors on the body surface.
[0063] The examples described above are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A flexible ultrasonic sensor based on nano zinc oxide composite material, comprising a flexible substrate, an acoustic matching layer and an electrode; characterized in that: It also includes a nano zinc oxide composite material; the nano zinc oxide composite material is composed of a nano zinc oxide structure and a flexible colloid; the nano zinc oxide composite material is placed between two electrode layers and is placed on a flexible substrate as a whole; the acoustic matching layer is located above the top electrode; The processing and preparation method of the flexible ultrasonic sensor based on the nano zinc oxide composite material is as follows: Step 1: Select a flexible substrate and clean it; use acetone, alcohol, and deionized water to ultrasonically clean the substrate in sequence, and then use nitrogen to blow clean the surface; Step 2: prepare a bottom electrode on a flexible substrate; use magnetron sputtering to uniformly deposit one or more layers of metal material on the substrate, and the vacuum degree of the substrate is less than 1×10 -3 Pa, ignition gas pressure 5-10Pa, sputtering power 50-250W, the thickness of the bottom electrode is controlled by controlling the sputtering time; Step 3: Prepare a piezoelectric layer on the bottom electrode. First, a zinc oxide seed layer is prepared on the bottom electrode by magnetron sputtering. The thickness of the seed layer does not exceed 800 nm. The vacuum degree of the substrate is less than 1×10 -3 Pa, ignition pressure 5-10Pa, sputtering power 50-100W, flow ratio of argon to oxygen 5-8:1, and thickness of zinc oxide is controlled by controlling sputtering time; then a layer of nano zinc oxide thick film is prepared on the seed layer by hydrothermal growth method; the reaction solution includes alkali solution and zinc nitrate solution, the molar ratio of zinc ions to hydroxide ions in the reaction solution is 1:4-8, the growth temperature is 60-100 degrees Celsius, and thickness of synthesized zinc oxide is controlled by controlling reaction time; synthesized zinc oxide crystals grow along C axis, with certain gaps between crystals; Step 4: Fill the gaps between zinc oxide crystals with flexible colloid to ensure that a smooth and dense filling surface is obtained in the end; Step 5: prepare a top electrode on the piezoelectric layer; use magnetron sputtering to uniformly deposit one or more layers of metal material on the substrate; the vacuum degree of the substrate is less than 1×10 -3 Pa, ignition gas pressure 5-10Pa, sputtering power 50-250W, the thickness of the top electrode is controlled by controlling the sputtering time; Step 6: preparing an acoustic matching layer on the top electrode; Step 7: Lead out the upper and lower electrodes, and perform electrical insulation and sealing packaging on the prepared sensor as a whole to obtain a flexible ultrasonic sensor.
2. A flexible ultrasonic sensor based on nano zinc oxide composite material as claimed in claim 1, characterized in that: The nano zinc oxide structure is prepared by a hydrothermal growth method, and its nanoscale linear structure ensures that the zinc oxide material will not undergo destructive deformation under large deformation bending conditions; the flexible colloid is filled in the nano zinc oxide structure, ensuring that the entire sensor has good robustness and is conducive to achieving close contact between the double-sided electrodes.
3. A flexible ultrasonic sensor based on nano zinc oxide composite material as claimed in claim 2, characterized in that: The method for preparing the nano zinc oxide structure by the hydrothermal growth method is as follows: placing the sample in a chemical reaction kettle for thick film growth; Alternatively, the sample is placed in a microchannel for thick film growth; the filling method of the flexible colloid includes: spin coating, spray coating and sputtering.
4. A flexible ultrasonic sensor based on nano zinc oxide composite material as claimed in claim 2, characterized in that: The nano zinc oxide structure includes: nano wires, nano rods, nano needles and nano cones, with a thickness of 1 to 100 μm and a top diameter of less than 1 μm.
5. The flexible ultrasonic sensor based on nano zinc oxide composite material according to claim 1, characterized in that: Flexible colloids include: polyimide, polystyrene, SU-8 and PDMS.
6. The flexible ultrasonic sensor based on nano zinc oxide composite material according to claim 1, characterized in that: The flexible substrate includes: polyimide, PDMS, polyethylene terephthalate and polystyrene, and its thickness is not less than 50 μm, its tensile strength is not less than 10 MPa, and its bending strength is not less than 10 MPa.
7. The flexible ultrasonic sensor based on nano zinc oxide composite material according to claim 1, characterized in that: The electrodes include a top electrode and a bottom electrode. The bottom electrode is located between the flexible substrate and the piezoelectric layer, and the top electrode is located between the piezoelectric layer and the matching layer. The electrode materials include gold, chromium, titanium, aluminum, silver and copper, and the thickness thereof is not less than 100 nm.
8. The flexible ultrasonic sensor based on nano zinc oxide composite material according to claim 1, characterized in that: The acoustic matching layer is one or more layers of material. The material and thickness of the acoustic matching layer are designed according to the acoustic impedance of the piezoelectric material and the detected object, so that the acoustic impedance value of the acoustic matching layer is between the impedance values of the piezoelectric material and the detected target. According to the traditional theory, the piezoelectric material and the detected target medium are regarded as semi-infinite, and the impedances of the piezoelectric material and the detected target are respectively Z p and Z m , the acoustic impedance of the i-th matching layer is Z i , then the acoustic impedance of the matching layer satisfies the following formula when the single layer is matched: