Preparation method of composite thermite and application of composite thermite in 5, 5 '-bistetrazole-1, 1'-dihydroxylammonium diformate

By etching the surface of aluminum powder in liquid metal and assembling it with nanometal oxides, the problem of intimate contact in existing composite aluminum thermal agents is solved, the energy density and combustion performance are improved, and catalyzed by multi-stage assembly to achieve the TKX-50 More efficient explosive performance.

CN118930391APending Publication Date: 2024-11-12BEIJING INST OF TECH

Patent Information

Application Number
CN202411207813.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing composite aluminum thermal agents are not in close contact with aluminum powder at the microscopic level, resulting in limited energy density improvement, and dihydroxyammonium 5,5′-bistetrazol-1,1′-dicarboxylate ( TKX-50) has insufficient research on modification technology and cannot fully demonstrate its advantages in high-energy explosives.

Method used

The surface of aluminum powder is etched by introducing liquid metal and ball milling process is used to perform multi-stage assembly of liquid metal and nanometal oxide with TKX-50, which promotes close contact between aluminum powder and oxide and improves combustion and heat transfer efficiency.

Benefits of technology

It significantly improves the thermal and combustion performance of aluminum powder, enhances the energy density, and catalyzes TKX-50 through liquid metal modified aluminum thermal agents, reducing its decomposition temperature and improving the overall performance of the explosives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930391A_ABST
    Figure CN118930391A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a composite thermite and application of the composite thermite in 5, 5 '-bistetrazole-1, 1'-dihydroxylammonium diformate, and relates to the technical field of catalytic materials. Liquid metal is prepared through a dissolving and mixing technology and serves as a modification medium of aluminum powder, and liquid metal modified aluminum powder (LM-Al) is obtained; the composite material is compounded with a nano metal oxide, and the thermal performance of the composite material is tested by using a synchronous thermal analyzer (TG-DSC). Results show that the composite thermite modified by the liquid metal has good thermal performance, the high-temperature thermal oxidation stage of the aluminum powder can be remarkably improved to be close to the melting point of the aluminum powder through Fe2O3 and WO3, and the thermal performance of the aluminum powder is greatly improved. On the basis, a liquid metal modified thermite is compounded with TKX-50, and the catalytic activity of the LM-Al at oxide composite material on thermal decomposition of TKX-50 is researched.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of catalytic materials technology, specifically to a method for preparing a composite aluminothermic agent and its application in 5,5′-bis(tetrazole-1,1′-dicarboxylic acid dihydroxyammonium). Background Technology

[0002] In recent years, highly reactive metal powders have been widely used in explosives to improve their combustion and detonation performance. Aluminum powder, due to its high calorific value, good compatibility, and low cost, has become the most commonly used energetic metal powder. However, aluminum powder is easily oxidized, forming a dense alumina film on its surface. This alumina film has poor chemical activity and a high melting point, affecting the heat and mass transfer process during operation and thus reducing the energy release efficiency of the explosive. Current research generally involves adding nano-metal oxides to micro / nano aluminum powder systems and preparing composite thermite agents through physical mixing methods to improve the thermal and ignition / combustion properties of aluminum powder. While this method can improve the thermal properties of aluminum powder, the effect is limited. At the microscopic level, the nano-metal oxides are not in close contact with the aluminum powder, leaving significant room for improvement in the system's energy density.

[0003] Dihydroxyammonium 5,5′-bis(hexazolium-1,1′-diacidate) (TKX-50) is a novel high-energy material that has attracted much attention since its successful synthesis due to its excellent explosive and safety properties. TKX-50 has a high nitrogen content, resulting in high energy density and low mechanical sensitivity. Furthermore, its simple preparation method makes it suitable for replacing widely used explosives such as CL-20, RDX, and HMX in high-energy composite solid propellants, thereby improving the energy level of solid propellants and reducing sensitivity and environmental hazards. However, current research on TKX-50 modification techniques is scarce. Typically, TKX-50 is physically blended with aluminum powder without establishing a bridge between the composite thermite system and TKX-50. Insufficient process exploration also prevents the full realization of TKX-50's advantages as a high-energy explosive.

[0004] To address the above problems, this invention provides a method for preparing a composite thermite and applies it to 5,5′-bistetrazole-1,1′-dicarboxylic acid dihydroxyammonium. Summary of the Invention

[0005] The purpose of this invention is to provide a method for preparing a composite thermite and its application in 5,5′-bis(tetrazole-1,1′-dicarboxylic acid dihydroxyammonium). By introducing liquid metal to etch the surface of aluminum powder and using a ball milling process to multi-stage assemble the prepared composite thermite and explosive (TKX-50), the contact between the explosive (TKX-50) and the aluminum powder is promoted, thereby improving combustion, detonation and heat transfer efficiency.

[0006] To achieve the above objectives, the present invention provides a method for preparing a composite thermite, specifically comprising the following steps:

[0007] (1) Preparation of liquid metal (LM)

[0008] Galinstan eutectic liquid metal with a mass ratio of Ga:In:Sn of 68:22:10 was prepared by taking three metal raw materials: Ga, In and Sn.

[0009] (2) Preparation of aluminum powder / liquid metal aluminothermic agent (LM-Al)

[0010] Aluminum powder and the liquid metal obtained in step (1) were mixed and ultrasonically stirred, then vacuum filtered and dried to obtain LM-Al;

[0011] (3) Preparation of aluminum powder / liquid metal / nano metal oxide composite aluminothermic agent (LM-Al@oxide)

[0012] The LM-Al and nano-metal oxides obtained in step (2) were added to n-hexane, ultrasonically stirred, and then dried to obtain a composite aluminothermic agent.

[0013] Preferably, in step (2), the liquid metal accounts for one of 5%, 10%, and 15% of the mass of the aluminum powder.

[0014] Preferably, in step (2), the ultrasonic power is 200W and the ultrasonic frequency is 40kHz.

[0015] Preferably, in step (2), the drying conditions are: drying in an oven at 50°C for 12 hours.

[0016] Preferably, in step (3), the nano-metal oxide is one of Fe2O3, Bi2O3, Cr2O3, and WO3.

[0017] Preferably, in step (3), the mass ratio of LM-Al to nano-metal oxide is one of 4:1, 4:2, 4:3, 4:4, or 4:5.

[0018] Preferably, in step (3), the ultrasonic power is 200W and the ultrasonic frequency is 40kHz.

[0019] Preferably, in step (3), the drying conditions are: drying in an oven at 50°C for 12 hours.

[0020] The present invention also provides a composite aluminothermic agent prepared by any of the above preparation methods.

[0021] The present invention also provides the application of the above-mentioned composite thermite in 5,5′-bistetrazole-1,1′-dicarboxylic acid dihydroxyammonium explosive.

[0022] Therefore, the present invention provides a method for preparing a composite thermite and its application in 5,5′-bis(tetrazole-1,1′-dicarboxylic acid dihydroxyammonium). Compared with the prior art, the specific beneficial effects are as follows:

[0023] (1) The composite thermite prepared by the present invention involves introducing liquid metal to etch the surface of aluminum powder, thereby destroying the dense oxide film layer on the surface of aluminum powder and embrittles the surface of aluminum powder. This is beneficial to the contact between the aluminum core and the external oxygen environment, thereby improving the thermal performance of aluminum powder.

[0024] (2) In this invention, nano-metal oxides are mixed with aluminum powder and a core-shell structured thermite is prepared by ultrasonic melting process, which improves the energy density of aluminum powder (the common method is mechanical mixing, while the process obtained by this method is a core-shell structure. Compared with other methods, the contact between aluminum powder and oxide in the product is closer, so the energy density is improved).

[0025] (3) In this invention, aluminum powder catalyzed by liquid metal and nano metal oxide are prepared into core-shell structured composite particles. Then, the particles are mixed with explosive (TKX-50) by ball milling to obtain multi-stage assembled aluminum powder / liquid metal / metal oxide / TKX-50 energetic composite particles, which have significantly enhanced thermal and combustion properties.

[0026] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0027] Figure 1 The graph shows the thermal weight gain curves of aluminum powder with different proportions of liquid metal obtained in Example 1.

[0028] Figure 2 Here are schematic diagrams and microstructure images of Raw-Al and LM-Al, where (a) shows the process of LM modifying raw aluminum powder; (b) shows the microstructure of raw aluminum powder; (c) shows the microstructure of LM-Al; and (d) shows the elemental surface scan diagram of LM-Al.

[0029] Figure 3 SEM images of LM-Al powder stored in air for one year;

[0030] Figure 4 The images shown are SEM images of LM-Al@Fe2O3 with different ratios obtained in Example 2, where (a) is 4:1; (b) is 4:2; (c) is 4:3; (d) is 4:4; (e) is 4:5; and (f) and (g) are EDS-Mapping images of composite particles when LM-Al:Fe2O3 = 4:4.

[0031] Figure 5The images shown are SEM images of LM-Al@Bi2O3 with different ratios obtained in Example 3, where (a) is 4:1; (b) is 4:2; (c) is 4:3; (d) is 4:4; (e) is 4:5; and (f) and (g) are EDS-Mapping images of composite particles when LM-Al:Bi2O3 = 4:4.

[0032] Figure 6 The images shown are SEM images of LM-Al@Cr2O3 with different ratios obtained in Example 4, where (a) is 4:1; (b) is 4:2; (c) is 4:3; (d) is 4:4; (e) is 4:5; and (f) and (g) are EDS-Mapping images of composite particles when LM-Al:Cr2O3 = 4:4.

[0033] Figure 7 The images shown are SEM images of LM-Al@WO3 with different ratios obtained in Example 5, where (a) is 4:1; (b) is 4:2; (c) is 4:3; (d) is 4:4; (e) is 4:5; and (f) and (g) are EDS-Mapping images of composite particles when LM-Al:WO3 = 4:4.

[0034] Figure 8 The images are SEM images of Raw-Al@Fe2O3 with different ratios obtained in Comparative Example 1, where (a) is 4:1; (b) is 4:2; (c) is 4:3; (d) is 4:4; and (e) is 4:5.

[0035] Figure 9 The images are SEM images of Raw-Al@Bi2O3 with different ratios obtained in Comparative Example 2, where (a) is 4:1; (b) is 4:2; (c) is 4:3; (d) is 4:4; and (e) is 4:5.

[0036] Figure 10 The images are SEM images of Raw-Al@Cr2O3 with different ratios obtained in Comparative Example 3, where (a) is 4:1; (b) is 4:2; (c) is 4:3; (d) is 4:4; and (e) is 4:5.

[0037] Figure 11 The images shown in Comparative Example 4 are Raw-Al@WO3SEM images with different aspect ratios, where (a) is 4:1; (b) is 4:2; (c) is 4:3; (d) is 4:4; and (e) is 4:5.

[0038] Figure 12SEM images of Raw-Al and LM-Al composites with nano-metal oxides at a mass ratio of 4:3 are shown. (a) Raw-Al@Fe2O3; (b) Raw-Al@Bi2O3; (c) Raw-Al@Cr2O3; (d) Raw-Al@WO3; (e) LM-Al@Fe2O3; (f) LM-Al@Bi2O3; (g) LM-Al@Cr2O3; (h) LM-Al@WO3.

[0039] Figure 13 The XRD patterns of LM-Al@oxide composite aluminothermic agents are shown, where (a) is LM-Al@Fe2O3; (b) is LM-Al@Bi2O3; (c) is LM-Al@Cr2O3; and (d) is LM-Al@WO3.

[0040] Figure 14 XPS spectra of LM-Al@oxide composite aluminothermic agents, where (a) represents LM-Al@Fe2O3; (b) represents LM-Al@Bi2O3; (c) represents LM-Al@Cr2O3; and (d) represents LM-Al@WO3.

[0041] Figure 15 TG-DSC image of LM-Al@oxide composite aluminothermic agent.

[0042] Figure 16 DSC curves for TKX-50, TKX-50+LM-Al@Fe2O3, TKX-50+LM-Al@Bi2O3, KX-50+LM-Al@Cr2O3, and TKX-50+LM-Al@WO3;

[0043] Figure 17 Arrhenius plots of TKX-50 catalyzed by LM-Al@Fe2O3, LM-Al@Bi2O3, LM-Al@Cr2O3, and LM-Al@WO3. Detailed Implementation

[0044] The present invention will be further described below with reference to the accompanying drawings and specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the invention should be considered equivalent substitutions and are included within the scope of protection of the present invention. Furthermore, it should be understood that after reading the contents of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims and are all within the scope of protection of the present invention.

[0045] In this document, the term "embodiment" means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The term "embodiment" appearing in various places throughout the specification does not necessarily refer to the same embodiment, nor does it specifically limit its independence or connection with other embodiments. In principle, in this application, as long as there are no technical contradictions or conflicts, the technical features mentioned in each embodiment can be combined in any way to form corresponding implementable technical solutions.

[0046] Unless otherwise defined, the technical terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the use of related terms herein is merely for the purpose of describing particular embodiments and is not intended to limit this application.

[0047] Unless otherwise specified, the reagents, instruments, and equipment used in this invention are all commonly used by those skilled in the art.

[0048] The materials used in the following examples are: micron-sized aluminum powder with a particle size of 5 μm and a purity of 99.9%; iron oxide Fe2O3 (30 nm, spherical, Aladdin); chromium oxide Cr2O3 (60 nm, spherical, Maclean); bismuth oxide Bi2O3 (80-200 nm, spherical, ThermoScientific); tungsten oxide WO3 (<100 nm, spherical, Maclean); high-purity gallium (99.99%, Zancheng (Tianjin) Technology Co., Ltd.); indium (99.99%, Zancheng (Tianjin) Technology Co., Ltd.); tin (99.99%, Zancheng (Tianjin) Technology Co., Ltd.); and n-hexane (Beijing Mairuida Technology Co., Ltd.).

[0049] Example 1

[0050] This embodiment provides the preparation of an aluminum powder / liquid metal composite thermite, including the following steps:

[0051] (1) Preparation of liquid metal

[0052] Galinstan eutectic liquid metal with a mass ratio of Ga:In:Sn of 68:22:10 was prepared by taking three metal raw materials: Ga, In and Sn.

[0053] (2) Preparation of aluminum powder / liquid metal aluminothermic agent

[0054] According to different proportions, aluminum powder and liquid metal obtained in step (1) are mixed, stirred under ultrasonic conditions with a power of 200W and a frequency of 40kHz, vacuum filtered, and then placed in an oven at 50℃ for 12h to obtain LM-Al with liquid metal contents of 5%, 10%, and 15%.

[0055] Thermal weight gain curves of aluminum powder with different proportions of liquid metal are shown below. Figure 1 As shown. By Figure 1 It can be seen that when the proportion of liquid metal reaches 10%, the degree of thermal oxidation of aluminum powder is the highest, which is reflected in the largest increase in weight and the fastest rate of heat release.

[0056] Example 2

[0057] This embodiment provides a method for preparing LM-Al@Fe2O3 composite aluminothermic agent, and the specific steps are as follows:

[0058] The 10% LM-Al and Fe2O3 obtained in Example 1 were added to n-hexane at mass ratios of 4:1, 4:2, 4:3, 4:4, and 4:5, respectively. The mixture was stirred under ultrasonic conditions at 200W and 40kHz. The high-intensity ultrasound generated a strong flow effect, which helped break up the nanoparticle clusters of the oxides. Simultaneously, mechanical stirring was performed to prevent the nanoparticles from re-aggregating. The mixture was then dried in an oven at 50°C for 12 hours to obtain the LM-Al@Fe2O3 composite aluminothermic agent.

[0059] Example 3

[0060] This embodiment provides a method for preparing LM-Al@Bi2O3 composite aluminothermic agent, and the specific steps are as follows:

[0061] LM-Al and Bi₂O₃, each in a mass ratio of 10%, obtained in Example 1, were added to n-hexane at mass ratios of 4:1, 4:2, 4:3, 4:4, and 4:5, respectively. The mixture was stirred under ultrasonic conditions at a power of 200W and a frequency of 40kHz. The high-intensity ultrasound generated a strong flow effect, which helped break up the nanoparticle clusters of the oxides. Simultaneously, mechanical stirring was performed to prevent the nanoparticles from re-aggregating. The mixture was then dried in an oven at 50°C for 12 hours to obtain the LM-Al@Bi₂O₃ composite aluminothermic agent.

[0062] Example 4

[0063] This embodiment provides a method for preparing LM-Al@Cr2O3 composite aluminothermic agent, and the specific steps are as follows:

[0064] The 10% LM-Al and Cr2O3 obtained in Example 1 were added to n-hexane at mass ratios of 4:1, 4:2, 4:3, 4:4, and 4:5, respectively. The mixture was stirred under ultrasonic conditions at 200W and 40kHz. The high-intensity ultrasound generated a strong flow effect, which helped break up the nanoparticle clusters of the oxides. Simultaneously, mechanical stirring was performed to prevent the nanoparticles from re-aggregating. The mixture was then dried in an oven at 50°C for 12 hours to obtain the LM-Al@Cr2O3 composite aluminothermic agent.

[0065] Example 5

[0066] This embodiment provides a method for preparing LM-Al@WO3 composite thermite, and the specific steps are as follows:

[0067] LM-Al and WO3, each at a mass ratio of 10% obtained in Example 1, were added to n-hexane at mass ratios of 4:1, 4:2, 4:3, 4:4, and 4:5, respectively. The mixture was stirred under ultrasonic conditions at a power of 200W and a frequency of 40kHz. The high-intensity ultrasound generated a strong flow effect, which helped break up the nanoparticle clusters of the oxides. Simultaneously, mechanical stirring was performed to prevent the re-agglomeration of the nanoparticles. The mixture was then dried in an oven at 50°C for 12 hours to obtain the LM-Al@WO3 composite aluminothermic agent.

[0068] Comparative Example 1

[0069] This comparative example provides a method for preparing Raw-Al@Fe2O3 composite thermite, the specific steps of which are as follows:

[0070] Raw aluminum powder (Raw-Al) and Fe₂O₃ were added to n-hexane at mass ratios of 4:1, 4:2, 4:3, 4:4, and 4:5, respectively. The mixture was stirred under ultrasonic conditions at 200W and 40kHz. The high-intensity ultrasound generated a strong flow effect, which helped break up the nanoparticle clusters of the oxides. Simultaneously, mechanical stirring was performed to prevent the nanoparticles from re-agglomerating. The mixture was then dried in an oven at 50℃ for 12 hours to obtain the Raw-Al@Fe₂O₃ composite aluminothermic agent.

[0071] Comparative Example 2

[0072] This embodiment provides a method for preparing Raw-Al@Bi2O3 composite thermite, and the specific steps are as follows:

[0073] Raw aluminum powder (Raw-Al) and Bi₂O₃ were added to n-hexane at mass ratios of 4:1, 4:2, 4:3, 4:4, and 4:5, respectively. The mixture was stirred under ultrasonic conditions at 200W and 40kHz. The high-intensity ultrasound generated a strong flow effect, which helped break up the nanoparticle clusters of the oxides. Simultaneously, mechanical stirring was performed to prevent the nanoparticles from re-aggregating. The mixture was then dried in an oven at 50℃ for 12 hours to obtain the Raw-Al@Bi₂O₃ composite aluminothermic agent.

[0074] Comparative Example 3

[0075] This embodiment provides a method for preparing Raw-Al@Cr2O3 composite thermite, the specific steps of which are as follows:

[0076] Raw aluminum powder (Raw-Al) and Cr2O3 were added to n-hexane at mass ratios of 4:1, 4:2, 4:3, 4:4, and 4:5, respectively. The mixture was stirred under ultrasonic conditions at 200W and 40kHz. The high-intensity ultrasound generated a strong flow effect, which helped break up the nanoparticle clusters of the oxides. Simultaneously, mechanical stirring was performed to prevent the nanoparticles from re-agglomerating. The mixture was then dried in an oven at 50℃ for 12 hours to obtain the Raw-Al@Cr2O3 composite aluminothermic agent.

[0077] Comparative Example 3

[0078] This embodiment provides a method for preparing Raw-Al@WO3 composite thermite, and the specific steps are as follows:

[0079] Raw aluminum powder (Raw-Al) and WO3 were added to n-hexane at mass ratios of 4:1, 4:2, 4:3, 4:4, and 4:5, respectively. The mixture was stirred under ultrasonic conditions at 200W and 40kHz. The high-intensity ultrasound generated a strong flow effect, which helped break up the oxide nanoparticle clusters. Simultaneously, mechanical stirring was performed to prevent the nanoparticles from re-aggregating. The mixture was then dried in an oven at 50℃ for 12 hours to obtain the Raw-Al@WO3 composite aluminothermic agent.

[0080] The morphology, structure and thermal properties of the materials in the above embodiments and comparative examples were characterized. The LM-Al mentioned below refers to LM-Al with a liquid metal content of 10%.

[0081] I. Morphological Structure Characterization

[0082] The microstructures of Raw-Al, LM-Al, LM-Al@oxide, and Raw-Al@oxide were studied using a scanning electron microscope (SEM, ZEISG GeminiSEM300, Germany). The test conditions were: accelerating voltage 10V and probe beam current 3pA-20nA.

[0083] The phase compositions of LM-Al, LM-Al@oxide, and Raw-Al@oxide were obtained using X-ray diffraction (XRD, Rigaku Ultima IV, Japan). The test conditions were as follows: wavelength... Voltage 40kV, current 40mA.

[0084] The elemental composition and relative content of LM-Al, LM-Al@ oxide, and Raw-Al@ oxide were studied using an X-ray photoelectron spectroscopy analyzer (XPS, Thermo Scientific K-Alpha, USA). The test conditions were: excitation source: AlKα rays (1486.6 eV), beam spot: 400 μm.

[0085] Results analysis:

[0086] 1. For example Figure 2 Schematic diagrams and microstructure images of Raw-Al and LM-Al are shown. Figure 2 a is a schematic diagram of the process of modifying raw aluminum powder using liquid metal (LM). Figure 2 b represents the microstructure of the original aluminum powder. It can be seen that the original aluminum powder has a size of approximately 5 μm, a smooth surface, and good sphericity. Figure 2 c represents the microstructure of liquid metal-modified aluminum powder (LM-Al). It can be seen that after surface treatment with liquid metal, the surface of the aluminum powder particles exhibits an uneven texture, indicating that the liquid metal disrupts the dense oxide film present on the surface of the aluminum powder. Figure 2 Image d shows the elemental surface scan of LM-Al, confirming that the modified aluminum powder is coated with a thin film of liquid metal. LM-Al was then placed in room temperature air for one year. Figure 3 ),Depend on Figure 3 The SEM image shows that the particle surface is still uneven, indicating that the presence of the liquid metal film can inhibit the oxidation process on the aluminum powder surface and improve the heat transfer and energy release efficiency of the aluminum powder.

[0087] 2. For example Figure 4-7 The images show SEM images of LM-Al@oxides prepared in different proportions as described in Examples 2-5. As can be seen from the figures, with the increase of oxide content, the surface coating of aluminum powder gradually increases, which is reflected in the decrease of the exposed area of ​​the aluminum powder surface.

[0088] 3. For example Figure 8-11 The images show SEM images of the Raw-Al@oxides prepared in different proportions as shown in Examples 1-4. As can be seen from the figures, with the increase of oxide content, the surface coating of the aluminum powder gradually increases, which is reflected in the decrease of the exposed area of ​​the aluminum powder surface.

[0089] 4. For example Figure 12 The images show SEM images of the original aluminum powder and the product after LM-Al was combined with nano-metal oxides. The Al:oxide ratio before and after modification was 4:3. As can be seen from the images, under the modification process used in this work, different oxides can form a core-shell structure with the aluminum powder before and after modification with liquid metal. This structure allows for sufficient contact between the aluminum core and the oxide, which is beneficial for improving the complete combustion of aluminum powder and thus enhancing its energy release efficiency.

[0090] 5. For example Figure 13The X-ray diffraction (XRD) spectra of the products obtained by LM-Al and metal oxides under different modification ratios are shown. The XRD patterns show that even after introducing Fe2O3, Bi2O3, Cr2O3, and WO3 into LM-Al, characteristic peaks of Al and oxides are still detected, and no impurity peaks are present. This indicates that the phase structure of the composite particles modified with different coating ratios remains unchanged, and the relationship between LM-Al and nano-metal oxides is a physical composite.

[0091] 6. Figure 14 The X-ray photoelectron spectroscopy (XPS) spectra of the products obtained by LM-Al and metal oxides at different modification ratios are shown. It can be seen that the surface of the aluminum powder particles is covered with liquid metal (Ga, In, Sn), which explains why LM-Al did not show significant oxidation after one year of storage. Figure 3 This means that the liquid metal coating on the surface of aluminum powder particles can suppress the formation of the Al2O3 passivation layer. Furthermore, no obvious Al characteristic peaks were detected in the composite particles formed by LM-Al and oxides. As discussed above, LM-Al and oxides are modified in this process to form a tightly packed core-shell structure, and XPS cannot detect the aluminum core beneath the oxides; therefore, the Al characteristic peaks are extremely weak.

[0092] II. Thermal Performance Characterization

[0093] The thermal properties of the samples were studied using thermogravimetric-differential scanning calorimetry (TG-DSC, Netzsch STA449F3, Germany), with a temperature range of 50 to 1200 °C and a heating rate of 20 °C / min. -1 The nitrogen flow rate is 50 mL / min. -1 .

[0094] The thermal properties of four thermite agents were characterized using simultaneous thermal analysis (TG-DSC), such as... Figure 15 As shown in the figure, except for Bi₂O₃, the other three oxides can advance the high-temperature thermal oxidation stage of aluminum powder after coating and modification. Specifically, when Fe₂O₃ is used as a metal oxide and forms an aluminothermic agent with aluminum powder, the high-temperature thermal oxidation stage of the aluminum powder occurs immediately after reaching the melting point (660℃) when the mass ratio (Al:Fe₂O₃) ≤ 4:3. This means that after the aluminum powder reaches its melting point, the internal active aluminum breaks through the shell and enters the system, reacting with Fe₂O₃ in a short time and releasing a large amount of heat. Figure 15-a). When the ratio is 1:1, the peak temperature of thermal oxidation is the lowest (664.45℃), which is consistent with the melting temperature of aluminum powder (660℃). This indicates that the melting reaction of aluminum powder and the high-temperature thermal oxidation reaction occur simultaneously at this time. That is, after the aluminum powder reaches its melting point, due to the change in surface load, the molten active aluminum reacts with Fe2O3 in the system the instant it breaks through the aluminum shell. This phenomenon helps to improve the reaction degree of aluminum powder in the high-temperature thermal oxidation stage and reduce the ignition delay time of aluminum powder.

[0095] WO3 and Fe2O3 have similar effects, but molten active aluminum cannot react fully with WO3. Even at a ratio of 4:5, a small amount of active aluminum still undergoes high-temperature thermal oxidation around 1100℃. Figure 15 -d). When LM-Al and Cr2O3 form an aluminothermic agent, the peak temperature of high-temperature thermal oxidation of aluminum powder is directly proportional to the amount of Cr2O3 added. When the ratio of Cr2O3 added is increased to 4:5, the peak temperature of thermal decomposition of aluminum powder decreases to 941.7℃, but this temperature is still much higher than the peak temperature of thermal oxidation of aluminum powder under Fe2O3 catalysis (664-702℃). Further increasing the amount of Cr2O3 is a potential solution, but there are safety concerns when nano-oxides are combined with aluminum powder. An excessively high proportion of oxides can affect the stability of energetic materials and is detrimental to their storage and transportation. The worst performing aluminothermic agent is Bi2O3 combined with aluminum powder. As the proportion of Bi2O3 increases, the high-temperature thermal oxidation temperature of aluminum powder decreases slightly after a brief increase. When the ratio exceeds 4:3, the exothermic heat release of high-temperature thermal oxidation of aluminum powder decreases significantly, reflected in a weak high-temperature exothermic peak. This indicates that the presence of Bi2O3 hinders the participation of molten aluminum in high-temperature thermal oxidation and reduces its thermal properties.

[0096] In summary, when the four oxides are combined with modified aluminum powder to form thermite, Fe2O3 and WO3 can significantly enhance the high-temperature thermal oxidation stage of aluminum powder to occur near the melting point of aluminum powder, greatly improving the thermal properties of aluminum powder. However, the reaction between WO3 and aluminum powder is incomplete, and its performance is slightly inferior to that of Fe2O3. Bi2O3 has the worst performance; a small amount of Bi2O3 can increase the heat release of aluminum powder in the high-temperature thermal oxidation stage, but as the proportion increases, it hinders the high-temperature thermal oxidation of aluminum powder and is not suitable as a catalytic component for aluminum-based propellants.

[0097] The modified composite aluminothermic agents prepared in Examples 2-5 were used in TKX-50 to study their effect on thermal decomposition catalytic performance.

[0098] 1. The effect of thermite on the peak temperature of the thermal decomposition of TKX-50

[0099] To investigate the effects of LM-Al@Fe2O3, LM-Al@Bi2O3, LM-Al@Cr2O3, and LM-Al@WO3 on the thermal decomposition catalytic performance of TKX-50, LM-Al@Fe2O3, LM-Al@Bi2O3, LM-Al@Cr2O3, and LM-Al@WO3 powders were added to TKX-50, respectively, and their thermal properties were tested. The results are as follows: Figure 16 As shown, the decomposition of TKX-50 involves two consecutive exothermic stages: low-temperature exothermic and high-temperature exothermic, with peak temperatures of 239.36℃ and 267.51℃, respectively. After adding LM-Al@Fe2O3, LM-Al@Bi2O3, LM-Al@Cr2O3, and LM-Al@WO3, the first decomposition peak of TKX-50 decreased by 55.57℃, 13.6℃, ​​20.4℃, and 28.46℃, respectively. LM-Al@Fe2O3 exhibited the best catalytic activity, possibly due to the different pore size distributions of the different oxides. Fe2O3 has a larger pore size, which is beneficial for the adsorption of gaseous products and the mass transfer of intermediate products, thus resulting in superior catalytic performance.

[0100] 2. To further explore the dynamic thermal parameters of different samples, the Kissinger method was used to calculate the apparent activation energy (Ea), pre-exponential factor (A), and linear correlation coefficient (r), as shown in the following formulas:

[0101]

[0102] In the formula, β is the heating rate, and T is the temperature rise rate. P1 The temperature of the first exothermic peak is given by [value], and R is the gas constant. E is analyzed using the Kissinger method. a See Table 1, Kissinger fitting plots are shown below. Figure 17 Linear correlation coefficient R 2 A value greater than 0.99 indicates high reliability of the results. The calculated Ea for TKX-50+LM-Al@Cr2O3 is 149.73 kJ·mol⁻¹. -1 It is significantly lower than TKX-50 (176.86 kJ·mol⁻¹). -1 It is also lower than TKX-50+LM-Al@Fe2O3 (157.30kJ·mol⁻¹). -1 ), TKX-50+LM-Al@Bi2O3(168.79kJ·mol -1 ), TKX-50+LM-Al@WO3(158.15kJ·mol -1 This indicates that LM-Al@Cr2O3 has better thermal decomposition catalytic activity than other catalysts.

[0103] The non-isothermal kinetic parameters of the exothermic reaction of TKX-50 with LM-Al@Fe2O3, LM-Al@Bi2O3, LM-Al@Cr2O3, and LM-Al@WO3 are shown in Table 1 below.

[0104] Table 1

[0105]

[0106] In summary, liquid metal was selected as the surface modification medium for aluminum powder, resulting in modified aluminum powder (LM-Al) after liquid metal embrittlement. Based on this, liquid metal-modified thermite agents LM-Al@Fe2O3, LM-Al@Bi2O3, LM-Al@Cr2O3, and LM-Al@WO3 were prepared using a solution-mixing process. Structural characterization confirmed that the composite particles prepared by this process possess a core-shell structure. Thermal performance tests showed that the high-temperature thermal oxidation initiation temperature of the aluminum powder after being combined with nano-metal oxides was significantly increased compared to the original aluminum powder.

[0107] Liquid metal-modified aluminothermic agents were used as catalysts for TKX-50. Thermal analysis confirmed that the addition of four modified aluminothermic agents significantly reduced the decomposition temperature of TKX-50, with LM-Al@Fe2O3 exhibiting the highest catalytic activity for the thermal decomposition of TKX-50. This work demonstrates the catalytic effect of liquid metal-modified aluminothermic agents on TKX-50, providing a new approach for the modification of TKX-50-based energetic materials.

[0108] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.

Claims

1. A method for preparing a composite thermite, characterized in that: The specific steps include: (1) Preparation of liquid metal Take three metal raw materials of Ga, In and Sn to prepare Galinstan eutectic liquid metal with a mass ratio of Ga:In:Sn of 68:22:10; (2) Preparation of aluminum powder / liquid metal thermite The aluminum powder and the liquid metal obtained in step (1) are mixed and ultrasonically stirred, and then vacuum filtered and dried to obtain LM-Al; (3) Preparation of aluminum powder / liquid metal / nanometallic oxide composite thermite The LM-Al and nano-metal oxide obtained in step (2) are added into n-hexane, and then dried after ultrasonic stirring to obtain a composite thermite.

2. The method for preparing a composite thermite according to claim 1, characterized in that: In the step (2), the liquid metal accounts for one of 5%, 10% and 15% of the mass of the aluminum powder.

3. The method for preparing a composite thermite according to claim 1, characterized in that: In the step (2), the ultrasonic power is 200 W and the ultrasonic frequency is 40 kHz.

4. The method for preparing a composite thermite according to claim 1, characterized in that: In the step (2), the drying condition is: drying in an oven at 50° C. for 12 hours.

5. The method for preparing a composite thermite according to claim 1, characterized in that: In the step (3), the nano metal oxide is one of Fe2O3, Bi2O3, Cr2O3, and WO3.

6. The method for preparing a composite thermite according to claim 1, characterized in that: In the step (3), the mass ratio of LM-Al to the nano-metal oxide is one of 4:1, 4:2, 4:3, 4:4, and 4:

5.

7. The method for preparing a composite thermite according to claim 1, characterized in that: In the step (3), the ultrasonic power is 200 W and the ultrasonic frequency is 40 kHz.

8. The method for preparing a composite thermite according to claim 1, characterized in that: In the step (3), the drying condition is: drying in an oven at 50° C. for 12 hours.

9. A composite thermite, characterized in that: The composite thermite is prepared by the preparation method according to any one of claims 1 to 8.

10. The composite thermite according to claim 9, characterized in that: The composite thermite is applied to 5,5'-bistetrazole-1,1'-dihydroxyammonium dicarboxylate explosive.

Citation Information

Patent Citations

  • Aluminum-based energetic MOFs and preparation method thereof

    CN112939707A

  • Core-shell structure thermite as well as preparation method and application thereof

    CN113105298A

  • Method for improving metal acceleration capacity of composite explosive

    CN117945819A

  • Methods for preparing dihydroxyammonium 5,5'-bistetrazole-1,1'diolate

    US20240425466A1

  • Energetic active composition comprising a dihydroxylammonium salt or diammonium salt of a bistetrazolediol

    WO2013026768A1

Cited By

  • Fluoride modified liquid metal medium thermite and preparation method thereof

    CN119591461A

  • Fluoride-modified liquid metal medium aluminized agent and preparation method thereof

    CN119591461B