Interference-resistant solid-state reference electrode

By introducing solid ion exchange materials and a polymer matrix with high loading of solid inorganic salts into the solid reference electrode, the problem of potential instability of traditional electrodes in acidic or abrasive environments is solved, achieving higher anti-interference and long-term stability. sex.

CN114667448BActive Publication Date: 2024-10-11COMMONWEALTH SCI & IND RES ORG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080077609.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-08
Filing Date
2020-11-06
Publication Date
2024-10-11
Estimated Expiration
2040-11-06

AI Technical Summary

Technical Problem

Traditional solid-state reference electrodes are prone to degradation when faced with acidic or abrasive analytes, and are sensitive to interfering ions in competitive redox reactions, resulting in unstable potential and difficulty in maintaining long-term stability in complex environments.

Method used

Solid ion exchange materials are introduced to intercept and immobilize interfering ions in the analyte, reduce the potential for redox reactions by exchanging with non-interfering ions, and provide stability through the high loading and water permeability of the solid inorganic salt and polymer matrix the reference potential.

Benefits of technology

Significantly improves the anti-interference ability and long-term stability of the electrode, ensuring potential stability and electrode life in acidic or abrasive analytes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114667448B_ABST
    Figure CN114667448B_ABST
Patent Text Reader

Abstract

The present invention provides a solid-state reference electrode, which includes: a reference element ionically connected to a composite material, the composite material including a water-permeable polymer matrix loaded with a solid inorganic salt including a reference anion; an electrode surface for contacting an analyte; and a solid ion exchange material located between the electrode surface and the reference element, the solid ion exchange material including one or more non-interfering ions, wherein in use, the solid ion exchange material is fixed to dissolve the one or more interfering ions when present in the analyte by exchanging with the non-interfering ions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a solid-state reference electrode. In particular, the electrode comprises a reference element ionically connected to a polymer composite material loaded with an inorganic salt including a reference anion, and a solid ion exchange material located between the electrode surface and the reference element. In use, the solid ion exchange material fixes interfering ions present in the analyte by exchanging with non-interfering ions present in the material. The present invention also relates to a system for electrochemical analysis of an analyte comprising the solid-state reference electrode, and a method for electrochemical analysis of an analyte using the solid-state reference electrode. Background Art

[0002] Electroanalytical techniques (including potentiometric and voltammetric electroanalytical measurements) rely on both an indicating (sensing) electrode and a reference electrode, the performance of which is equally important for the accuracy of the measurement. Therefore, it is critical that the reference electrode provides a stable and reproducible potential that is substantially independent of the concentration of species in the analyte, including the target species for the analysis.

[0003] To provide a constant reference potential, reference electrodes traditionally include a reference element immersed in a reservoir of a liquid or gel electrolyte of known salt concentration contained within a housing. Silver / silver chloride (Ag / AgCl) and calomel (Hg / Hg 2 Cl 2 ) reference element is common. Although the electrolyte is substantially isolated from the analyte by the housing, a liquid junction (liquid junction) (salt bridge) between the analyte and the internal electrolyte is required to provide ionic communication to complete the electrochemical cell. The liquid junction typically comprises a small opening or porous plug in the housing.

[0004] Although conventional reference electrodes are suitable for many applications, they also have significant disadvantages. These include leakage of electrolyte through the liquid junction, potentially contaminating the analyte with the reference electrolyte salt, and penetration of the analyte into the internal electrolyte, affecting the electrolyte salt concentration and introducing foreign species that interfere with the reference half-cell reaction. Although the junction and electrolyte can be designed to alleviate these problems, there is an inherent trade-off between the necessity (imperative) of minimizing liquid communication between the electrolyte and the analyte and maintaining an acceptable junction potential (which is a source of error in analytical measurements). In addition, conventional electrodes are difficult to miniaturize due to the electrolyte volume and complex structure, and are generally location-dependent, fragile, costly, and maintenance-intensive.

[0005] Many previous efforts have been made to address one or more of these challenges using solid-state reference electrodes that lack an internal liquid electrolyte reservoir and a corresponding liquid-liquid junction. Vonau et al., DE 10305005, describe a sintered Ag / AgCl reference element embedded in a solidified melt of KCl. The KCl is encapsulated in a ceramic layer and an outer housing, where the ceramic is exposed at a small opening in the housing, forming a junction to regulate ion connectivity and limit KCl dissolution into the analyte. These electrodes still rely on a porous junction between the internal salt and the analyte, resulting in a brittle and complex structure.

[0006] A promising approach is to embed a reference element in a composite material in the form of a water-permeable polymer matrix loaded with an inorganic salt including a reference anion. When immersed in an aqueous analyte, the composite material is hydrated until a saturated concentration of the reference anion is provided at the reference element. Thus, for example, Vonau et al., DE 195 33 059, reported a reference electrode comprising an Ag / AgCl reference element embedded in a polyester resin composite loaded with KCl. Mousavi et al., Analyst 2013 (138) 5216 and Journal of Solid State Electrochemistry 2014 (18) 607, prepared a reference electrode comprising an Ag / AgCl reference element embedded in a polyvinyl acetate (PVAc) homopolymer loaded with granular KCl. If suitably designed, the polymer matrix prevents rapid leaching of salts while still allowing sufficient ionic conductivity between the reference element and the analyte.

[0007] However, in many applications, the analytes of interest contain components that degrade the composite material or otherwise interfere with the long-term stability of the measured reference potential. For example, highly acidic or abrasive analytes can degrade polymer composite electrodes to the point of loss of dimensional stability and leaching of inorganic salts. In the applicant's co-pending PCT application published as WO2018 / 201200, this problem is addressed by using a composite material having a cross-linked vinyl polymer matrix.

[0008] However, solid-state reference electrodes including polymer composites loaded with reference salts are still sensitive to interference by soluble ionic species that can participate in competitive redox reactions at the reference element. These undesirable reactions lead to drifts away from the expected electrode potential. In particular, anionic species such as sulfide, bromide, iodide and cyanide can interfere with reference electrodes that rely on chloride or sulfate as reference anions.

[0009]

[0006] Therefore, there is a continuing need to provide a solid-state reference electrode that at least partially addresses one or more of the above-mentioned disadvantages or provides a useful alternative.

[0010] The reference herein to a patent document or other matter as prior art is not to be taken as an admission that the document or matter was known or that the information it contains was part of the common general knowledge as at the priority date of any claim. Summary of the invention

[0011] The inventors have discovered that a polymer composite reference electrode having improved resistance to redox interferences of ionic species present in the analyte can be obtained by introducing a solid ion exchange material with exchangeable non-interfering ions. In use, the solid ion exchange material intercepts one or more interfering ions that diffuse from the analyte into the electrode, thereby reducing the likelihood of undesirable redox reactions at the reference element. The ion exchange reaction fixes the interfering ions and releases non-interfering ions that have no substantial effect on the measured reference potential.

[0012] According to a first aspect, the present invention provides a solid-state reference electrode comprising: a reference element ionically connected to a composite material, the composite material comprising a water-permeable polymer matrix loaded with a solid inorganic salt including a reference anion; an electrode surface for contacting an analyte; and a solid ion exchange material located between the electrode surface and the reference element, the solid ion exchange material comprising one or more non-interfering ions, wherein in use, the solid ion exchange material is fixed to dissolve the one or more interfering ions when present in the analyte by exchanging with the non-interfering ions.

[0013] In some embodiments, the solid ion exchange material comprises a metal salt or an ion exchange resin. In some embodiments, the solid ion exchange material comprises a metal salt having a lower water solubility than a solid inorganic salt.

[0014] In some embodiments, one or more non-interfering ions are non-interfering anions, and one or more interfering ions are interfering anions. Non-interfering anions may include reference anions. In some embodiments, the solid ion exchange material includes a metal salt including cations selected from silver, mercury, and lead. In some embodiments, the solid ion exchange material includes a metal salt including a metal present in a reference element. In some embodiments, the interfering anions are selected from sulfide, iodide, bromide, and cyanide. In some embodiments, the interfering anions include sulfide.

[0015] In some embodiments, the solid ion exchange material is a granular material.

[0016] In some embodiments, the solid ion exchange material is supported in the polymer matrix of the composite or in an additional polymer composite located between the electrode surface and the reference element. The additional polymer composite may include a solid anion exchange material dispersed in a hydratable polymer.

[0017] In some embodiments, the solid ion exchange material is supported in the polymer matrix of the composite material.The solid ion exchange material may be present in an amount of at least 1 wt %, such as at least 3 wt %, of the composite material.

[0018] In some embodiments, the solid ion exchange material is supported in a water permeable layer of an additional polymer composite located between the electrode surface and the composite.

[0019] In some embodiments, the reference anion is chloride. In some embodiments, the reference element is selected from Ag / AgCl and calomel.

[0020] In some embodiments, the water-permeable polymer matrix comprises a vinyl polymer of a vinyl monomer containing a heteroatom. The vinyl polymer may be cross-linked. The cross-linked vinyl polymer may be a copolymer of i) at least one vinyl monomer selected from vinyl esters, vinyl amides, and acrylates and ii) a cross-linking agent comprising at least two copolymerizable vinyl functional groups. If present, the hydratable polymer may similarly be a vinyl polymer of a vinyl monomer containing a heteroatom.

[0021] In some embodiments, the composite material includes at least 30 mass % solid inorganic salt.

[0022] According to a second aspect, the present invention provides a system for electrochemical analysis of an analyte, the system comprising: a solid-state reference electrode according to any embodiment of the first aspect; a second electrode selected from an ion-selective electrode and a working electrode; and a device for measuring the potential difference between the second electrode and the reference electrode.

[0023] According to a third aspect, the present invention provides a method for electrochemical analysis of an analyte, the method comprising: contacting i) a solid-state reference electrode according to any embodiment of the first aspect and ii) a second electrode selected from an ion-selective electrode and a working electrode with the analyte; and measuring the electrochemical potential difference between the second electrode and the reference electrode.

[0024] In some embodiments, the analyte includes one or more interfering ions of dissolution. In some such embodiments, the interfering ion is an interfering anion. The interfering anion can be selected from sulfide, iodide, bromide and cyanide. In some embodiments, the interfering anion includes sulfide.

[0025] When the term "comprising" is used in the specification (including claims), it is interpreted as specifying stated features, integers, steps or components, but not excluding the presence of one or more other features, integers, steps or components, or groups thereof.

[0026] As used herein, the terms "first," "second," "third," etc., in connection with various features of the disclosed apparatus are arbitrarily designated and are intended only to distinguish between two or more such features that may be incorporated into the apparatus in various embodiments. The terms themselves do not imply any particular orientation or order. Furthermore, it will be understood that the presence of a "first" feature does not imply the presence of a "second" feature, the presence of a "second" feature does not imply the presence of a "first" feature, and so on.

[0027] Other aspects of the invention appear from the following detailed description of the invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Embodiments of the present invention will be described herein by way of example only with reference to the accompanying drawings, in which:

[0029] Figure 1 A solid-state reference electrode according to one embodiment of the present invention is schematically depicted, wherein a solid-state ion exchange material is dispersed in a composite material.

[0030] Figure 2 A printed solid-state reference electrode according to another embodiment of the invention is schematically depicted, wherein a solid ion exchange material is dispersed within a printed composite material layer.

[0031] Figure 3 A solid-state reference electrode according to another embodiment of the invention is schematically depicted, wherein the solid-state ion exchange material is present in a water-permeable layer between the electrode surface and the composite material.

[0032] Figure 4 is a graph of the potentiometric response of electrodes, including an electrode comprising AgCl as a solid ion exchange material and a comparative electrode lacking a solid ion exchange material, when exposed to an analyte comprising a sulfide anion for 140 days, as measured in Example 2.

[0033] Figure 5 is a graph of the potentiometric response of an electrode when exposed to an analyte comprising a sulfide anion, including an electrode comprising chloride-loaded ion exchange resin particles as a solid ion exchange material and a comparative electrode lacking a solid ion exchange material, as measured in Example 3.

[0034] Figure 6is a graph of the potentiometric response of an electrode, including an electrode comprising AgCl as a solid ion exchange material and a comparative electrode lacking a solid ion exchange material, when exposed to a highly acidic analyte comprising a sulfide anion, as measured in Example 5. DETAILED DESCRIPTION

[0035] Solid state reference electrode

[0036] The present invention relates to a solid reference electrode. The electrode comprises a reference element in ionic communication with a composite material. The composite material comprises a water-permeable polymer matrix loaded with a solid inorganic salt comprising a reference anion. The electrode has an electrode surface for contacting an analyte, and a solid ion exchange material is located between the electrode surface and the reference element. The solid ion exchange material comprises one or more non-interfering ions. In use, the solid ion exchange material is fixed to dissolve one or more interfering ions when present in the analyte by exchanging with the non-interfering ions.

[0037] Reference element

[0038] The solid state reference electrode comprises a reference element.As used herein, a reference element is an electrical conductor which comprises or forms in situ a redox couple (couple) capable of providing a reference potential when exposed to a reference electrolyte in use.

[0039] The reference element may be any suitable reference element capable of providing a stable potential when in contact with a reference electrolyte having a constant concentration of a reference anion. Such reference elements include reference elements having silver-silver chloride (Ag / AgCl), calomel (Hg / Hg 2 Cl 2 ), silver-silver sulfate (Ag / Ag 2 SO 4 ) and mercury-mercuric sulfate (Hg / Hg 2 SO 4 ) redox pairs. In some embodiments, the reference element is an Ag / AgCl or calomel reference element, which provides a reference potential when exposed to a reference electrolyte comprising a stable chloride concentration. Ag / AgCl reference elements are particularly preferred, at least in part for environmental and safety reasons.

[0040] Ag / AgCl reference element can include silver wire or other silver metal body, it is coated with silver chloride, typically electrochemically or by chemical oxidation. In some embodiments, the reference element includes a mesh or woven metal structure to increase the surface area in contact with the composite material. Ag / AgCl reference element can also be manufactured by a variety of other methods, including by sintering a mixture of Ag and AgCl powders. Printed Ag / AgCl reference element can be obtained by printing a silver layer onto a substrate, then using a chlorinating agent (such as hypochlorite) to chemically oxidize the layer. Alternatively, an ink including both Ag and AgCl particles in a carrier (carrier) can be used.

[0041] In use, the reference element is electrically connected to the other electrodes via an external circuit. Therefore, the reference element is typically provided with suitable electrical terminals for connection to the circuit. For example, in the case of a silver wire reference electrode, the electrical terminal may be the uncoated end of the wire.

[0042] The reference potential relative to the sensing electrode is measured by electrical conduction through the electrical conductor of the reference element. Because the reference electrode is configured for potentiometric, voltammetric and amperometric electrochemical analysis, the potential of the reference element should be measured without significant impedance between the active redox pair on the reference element and the potential measuring instrument. Therefore, the electrode is generally configured for low-impedance measurement of the reference potential, wherein the total impedance of the electrode is mainly attributable to the limitation of the ionic conductivity between the reference element and the analyte, rather than the limitation of the conductivity of the reference element. In particular, the electrode does not include a resistor coupled to the reference element through which the reference potential is measured. Also therefore, the electrode is generally configured to provide a single reference potential for measurement, which is different from the electrode that determines the reference potential by combining the ion-sensitive potentials established at two different electrode portions separated by a resistor.

[0043] Composite Materials

[0044] The reference element is in ionic communication with the composite material. The effect of the composite material is to provide a substantially stable solution concentration of reference anions at the reference element when the electrode is in contact with and hydrated by the aqueous analyte, while also allowing sufficient ionic conductivity between the reference element and the analyte. If in contact with or close to an electrolyte, the reference element will be appropriately in ionic communication with the composite material, provided that these criteria are met in use. In some embodiments, the reference element is in direct contact with the composite material. In some embodiments, the composite material is at least partially located between the electrode surface and the reference element.

[0045] The composite material comprises a water-permeable polymer matrix loaded with a solid inorganic salt including a reference anion. Thus, the composite material is typically a solid material without an internal liquid electrolyte reservoir. However, it is necessary that the composite material is sufficiently permeable to water to allow the composite material to be hydrated in use and to provide satisfactory ionic conductivity between the reference element and the analyte. In addition, the leaching rate of the inorganic salt into the analyte should preferably be low. For some applications, it is also preferred that the composite material is resistant to degradation in strongly acidic or abrasive analytes.

[0046] The composite material is preferably dimensionally stable in the expected aqueous analyte for the desired life of the device, which may be more than one week, or more than one month. Dimensional stability is an important mechanical requirement for many applications. Thus, in some embodiments, the composite material does not swell significantly when immersed in an aqueous analyte, as this would result in leaching of solid inorganic salts. Any swelling may be less than about 10% of the initial volume.

[0047] The composite material may define the physical body of the solid-state reference electrode. However, in some embodiments, the reference electrode includes a housing surrounding the composite material. The housing may be made of a suitable insulating and durable material for the envisioned application, such as poly(methyl methacrylate). If used, the housing will typically include a window to expose the composite material to the analyte, either directly or through an intermediate water-permeable layer, as described below.

[0048] The polymer matrix of composite material is loaded with solid inorganic salt comprising reference anion.Inorganic salt is sufficiently soluble in water so that the hydration of composite material will produce a constant saturated solution concentration of reference anion at the reference element.Solid inorganic salt can be dispersed in polymer matrix, typically as granular solid.Although solid inorganic salt is typically dispersed throughout polymer matrix, it is not excluded that the non-uniform distribution of inorganic salt is present in composite material.In some embodiments, the distribution of inorganic salt is produced by the gravity settling of granular salt in monomer mixture before polymerization.

[0049] High loading of solid inorganic salts can be beneficial because it can extend the life of the reference electrode. In some embodiments, the composite material includes at least 10 mass %, preferably at least 30 mass %, more preferably at least 50 mass % of solid inorganic salts. However, the loading should not be too high so as to damage the physical integrity of the composite material. Suitable loading can be achieved by allowing the inorganic salt in the form of granular solids (i.e. powder) to settle by gravity in the monomer mixture before polymerization.

[0050] The solid inorganic salt includes a reference anion. As used herein, a reference anion is an anion that participates in the desired redox half-reaction at the reference element. For example, Ag / AgCl and Ag / Ag 2 SO4 The reference electrode requires chloride and sulfate reference anions, respectively. In use, the reference anions should be provided in the composite material at a constant solution concentration to obtain a constant reference potential. This is evident, for example, from the half-cell potential of the Ag / AgCl reference electrode given by the applicable Nernst equation (1):

[0051]

[0052] where E is the half-cell reduction potential, E 0 is the standard half-cell reduction potential, R is the universal gas constant, T is the temperature, and α Cl- is the activity of the chloride ion (related to concentration).

[0053] In some embodiments, the solid inorganic salt is a sulfate, such as for Ag / Ag 2 SO 4 Potassium sulfate for the reference electrode. In other embodiments, the solid inorganic salt is a chloride salt, such as potassium chloride (KCl), sodium chloride (NaCl) or lithium chloride (LiCl), preferably KCl. When the reference electrode is, for example, an Ag / AgCl or calomel electrode, a chloride reference anion is required.

[0054] In some embodiments, the inorganic salt is composed of an inorganic cation and an inorganic anion, i.e., it lacks a coordinating ligand or any other organic component. The inorganic salt is not covalently bonded to the polymer matrix of the composite material because the polymer matrix and the inorganic salt are chemically distinct components of the composite material. In contrast, the ionic polymer charge-balanced with the reference ion is not a composite material loaded with an inorganic salt, and it itself provides insufficient amounts of readily soluble reference ions for establishing a persistent and constant saturated solution concentration at the reference element.

[0055] The inorganic salt may be a particulate solid. In some embodiments, the particulate solid has an average particle size of less than 1 mm, preferably less than 500 microns. The particles may be small enough to form a well-dispersed distribution throughout the polymer matrix.

[0056] Composite material comprises a water-permeable polymer matrix loaded with an inorganic salt including a reference anion, and in some embodiments also comprises a solid ion exchange material. As used herein, a polymer matrix is ​​a polymer phase of a composite material in which an inorganic salt is loaded. In at least some embodiments, the composite material comprises a polymer matrix as a continuous phase and an inorganic salt as a discontinuous phase. The polymer of the polymer matrix should therefore have a suitable hydrophobic-hydrophilic balance. Water permeability should be sufficient to allow composite material hydration and provide ionic conductivity through the polymer matrix between the reference element and the analyte. Therefore, the impedance of the electrode is acceptably low, and when placed in the analyte, the electrode can achieve a stable potential (that is, become adjusted) within an acceptable time. However, it is also preferred that the composite material should not be too hydrophilic, because this can lead to the substantial swelling of the polymer, the loss of the physical integrity of the electrode body and / or the rapid leaching of inorganic salts and / or solid ion exchange materials into the analyte. The polymer matrix is ​​generally electrically insulating, and is particularly not composed of intrinsic conductive polymers (such as polypyrrole). Reference element and ion exchange material are therefore electrically isolated from each other in use.

[0057] The type of polymer is not considered to be limited, provided that the polymer matrix is ​​suitably water permeable, taking into account the above considerations. Thus, in some embodiments, the polymer may be a vinyl polymer, an epoxy resin, a polyester resin, a polysiloxane, a polyurethane, a polysaccharide. Specific examples of suitable polymers may include propoxylated diglycidyl ether, methyl methacrylate glycidyl methacrylate-tetrahydrofurfuryl acrylate copolymer, cellulose acetate, ethyl cellulose, cellulose, etc. as disclosed in WO2012074356A1, silicone rubber, polyvinyl chloride, polystyrene, polyhydroxyethyl methacrylate, polyvinylidene chloride and polyurethane as disclosed in WO1996035116A1, cellulose acetate, cellulose acetate butyrate, cellulose triacetate, nitrocellulose and combinations thereof as disclosed in US6793789B2, vinyl fluoride, hexafluoropropylene, vinylidene fluoride as disclosed in US4908117A. , trifluoroethylene, chlorotrifluoroethylene polymers, such as the epichlorohydrin epoxy resin disclosed in DE102010050481A1, polymethyl methacrylate, polyacrylonitrile, polybutyl acrylate, etc. disclosed in US8486246B2, N-acrylamide disclosed in DE10354100A1, acrylate polymers disclosed in WO2006032284A1, polymers or copolymers of N-acryloylaminoethoxyethanol disclosed in US7790323B2, and copolymers of cationic monomers and anionic monomers including quaternary amines as disclosed in DE102011089707A1.

[0058] In some embodiments, the polymer matrix of the composite material includes a vinyl polymer. As used herein, a vinyl polymer is an addition polymer of one or more vinyl monomers, including an extended alkane (...-CCCCC-...) backbone chain. A wide range of vinyl polymers may be suitable, although achieving the optimal hydrophobic-hydrophilic balance for low impedance and high electrochemical stability while also providing excellent chemical resistance and mechanical stability may require an appropriate combination of monomers, crosslinking groups, and the degree of crosslinking in the polymer matrix, as will be further described below.

[0059] Vinyl polymers can be polymers containing heteroatoms, optionally containing at least one vinyl monomer containing more than one heteroatom. Heteroatoms can be selected from oxygen and nitrogen. Such heteroatom-containing vinyl monomers can impart hydrophilicity to the polymer backbone chain, allowing hydration and ion conductivity through the composite material. In some embodiments, the heteroatom-containing vinyl monomer is selected from vinyl esters, vinyl amides, acrylates, acrylonitrile and vinyl ethers. In some embodiments, the vinyl monomer includes a carbonyl group and can be selected from vinyl esters, vinyl amides and acrylates. Suitable vinyl monomers can include vinyl acetate, vinyl caprolactam, methyl (meth) acrylate, ethyl (meth) acrylate, butyl (meth) acrylate and hexyl (meth) acrylate.

[0060] In some embodiments, the vinyl polymer includes a vinyl monomer containing a heteroatom as the only monofunctional monomer. In other embodiments, the vinyl polymer is a copolymer of a vinyl monomer containing a heteroatom and a less polar vinyl monomer lacking a heteroatom. Suitable monomer compositions for the vinyl polymer can be selected by the skilled artisan without undue burden in consideration of the principles disclosed herein.

[0061] In some embodiments, the vinyl polymer is a cross-linked vinyl polymer. Such a polymer can be obtained, for example, by copolymerizing a mixture comprising a vinyl monomer containing a heteroatom and a copolymerizable cross-linking agent. In some embodiments, cross-linking of the vinyl polymer can enhance the resistance of the electrode to degradation caused by chemical attack, such as under strong acidic and / or high temperature use conditions. In some embodiments, cross-linking can enhance the resistance of the electrode to mechanical degradation, such as under abrasive use conditions.

[0062] In some embodiments, the vinyl polymer is cross-linked with a hydrophilic cross-linking group. As used herein, a hydrophilic cross-linking group is a group that imparts hydrophilic properties to the polymer matrix. The hydrophilic cross-linking group is typically an organic linking group containing one or more hydrophilic functional groups such as carboxyl, ether, amide and amine groups, preferably carboxyl and / or ether groups. In other embodiments, the vinyl polymer is cross-linked with a more hydrophobic cross-linking group. It will be appreciated that in this case, a more hydrophilic backbone may be desirable to achieve a desired overall hydrophilic-hydrophobic balance.

[0063] The crosslinked vinyl polymer may be a copolymer of a vinyl monomer including a heteroatom and a crosslinking agent having at least two copolymerizable vinyl functional groups, such as an acrylate or methacrylate. The crosslinking agent may be a hydrophilic crosslinking agent, such as ethylene glycol di(meth)acrylate, oligoethylene glycol di(meth)acrylate, or polyethylene glycol di(meth)acrylate. In other embodiments, the crosslinking agent may have hydrophobic properties, such as an aliphatic crosslinking agent 1,6-hexanediol di(meth)acrylate.

[0064] In some embodiments, the crosslinking agent is selected from ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, poly(ethylene glycol) dimethacrylate (e.g., Mn=330-20,000), poly(ethylene glycol) diacrylate (e.g., Mn=250-20,000), N,N'-methylenebisacrylamide, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, bisphenol A glycerol di(meth)acrylate. di(meth)acrylate), diurethane di(meth)acrylate, divinylbenzene, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, glycerol propoxylate triacrylate (e.g., Mn=428), trimethylolpropane ethoxylate triacrylate, and trimethylolpropane propoxylate triacrylate. As used herein, "(meth)acrylate" refers to acrylate or methacrylate. In some embodiments, the crosslinking agent is selected from ethylene glycol di(meth)acrylate, poly(ethylene glycol) di(meth)acrylate.

[0065] Crosslinked vinyl polymers include suitable crosslinking density. If the crosslinking density is too low, the resistance or long-term stability of the reference electrode to chemical and or mechanical degradation may be lower than desired. However, if the crosslinking density is too high, the permeability or mechanical properties of the polymer may be unsatisfactory. In embodiments where the vinyl polymer is a copolymer of a vinyl monomer and a crosslinking agent containing heteroatoms, the vinyl polymer may include 0.5 to 7% by mass of a crosslinking agent, for example 1 to 4% by mass of a crosslinking agent or 1.5 to 3.5% by mass of a crosslinking agent.

[0066] Solid ion exchange materials

[0067] The solid-state reference electrode comprises a solid-state ion exchange material, which comprises one or more non-interfering ions. The material is located between the electrode surface for contacting the analyte and the reference element. In use, the solid ion exchange material is fixed to dissolve one or more interfering ions when present in the analyte by exchanging with the non-interfering ions. Therefore, the role of the solid ion exchange material is to react sacrificially by ion exchange with the interfering ions that penetrate the electrode, thereby fixing them and preventing, suppressing or delaying them from reaching the reference element. The ions released in the ion exchange reaction are non-interfering anions, and therefore have little or no harmful effect on the potential stability of the electrode.

[0068] As used herein, an interfering ion is capable of participating in a competing redox reaction at the reference element, which results in a deviation from the expected electrode potential. In contrast, a non-interfering ion is an ion that does not significantly affect the measured electrode potential.

[0069] In some embodiments, the solid ion exchange material comprises non-interfering anions. The ion exchange material can therefore protect the electrode from one or more interfering anions present in the analyte by anion exchange. Without wishing to be bound by any theory, the inventors believe that for a given electrode system, possible interfering and non-interfering anions can be distinguished by comparing the standard reduction potential of the relevant redox reaction expected at the reference electrode. Taking the Ag / AgCl reference electrode as an example, the standard reference reduction potential (at 25°C, 1atm) for the selection of anions is as shown in Table 1. Anions reacting at the reference element at a standard reference potential more negative than the reference electrode reaction can be expected to interfere with the measured potential. In contrast, anions involved in the reaction with the same or more positive standard reference potential are expected not to interfere with the measured potential.

[0070] Table 1

[0071]

[0072] Thus, anionic species such as sulfide, bromide, iodide, and cyanide can interfere with reference electrodes that rely on chloride or sulfate as reference anions. When sulfate is the reference anion, chloride can also be an interfering anion. In particular, sulfide has been found to be of great significance to the long-term stability of composite reference electrodes, consistent with the substantial differences between the standard reduction potentials of redox reactions involving sulfide compared to those for chloride or sulfate.

[0073] Therefore, the range of suitable non-interfering anions that the ion exchange material may include will depend on the redox couple that forms the basis for the reference potential measurement. For Ag / AgCl or saturated calomel reference elements, the solid ion exchange material may include anions selected from chloride, sulfate or nitrate.

[0074] In some embodiments, the solid ion exchange material includes the reference anion itself as an exchangeable anion. This is particularly preferred because the resulting ion exchange reaction simply releases additional reference anion into the environment in which it is already present in solution. Thus, for Ag / AgCl or saturated calomel reference elements, the solid ion exchange material preferably includes exchangeable chloride. For Ag / Ag 2 SO 4 The reference element, the solid ion exchange material may include exchangeable sulfate groups.

[0075] In some embodiments, the solid ion exchange material includes non-interfering cations that are capable of ion exchange with one or more interfering cations present in the analyte.

[0076] Solid ion exchange materials can generally be any solid material that can fix interfering anions and release non-interfering ions through an ion exchange mechanism. In some embodiments, solid ion exchange materials include metal salts or ion exchange resins. Solid ion exchange materials can be granular materials, for example, having an average particle size of less than 10 mm, or less than 5 mm, or less than 1 mm, or less than 500 microns. Therefore, granular ion exchange materials can be dispersed throughout the polymer matrix of composite materials or in an additional protective layer between composite materials and electrode surfaces, so as to provide good protection effects.

[0077] Metal Salts as Solid Ion Exchange Materials

[0078] In some embodiments, the solid ion exchange material is a metal salt. The metal salt need not be completely insoluble in water, but preferably has a lower solubility in water than the solid inorganic salt comprising the reference anion. Therefore, it is unlikely to leach out of the composite material during the service life of the electrode. In addition, relative insolubility can help to fix interfering ions during use, because the product salt is also expected to be relatively insoluble.

[0079] As discussed above, the present invention may be used to protect an electrode from one or more interfering anions and therefore the metal salt may be a metal salt of a suitable non-interfering anion.Most preferably, the metal salt comprises the reference anion itself.

[0080] The selection of the metal in the metal salt can depend on the interfering anion expected in the analyte, because the target is to precipitate the product salt of the ion exchange reaction as an insoluble salt. In addition, the metal salt should preferably have a strong affinity to the interfering anion, thereby providing good selectivity and fast ion exchange kinetics in the salt metathesis reaction. For the fixing of the sulfide anion, it can be suitable to include a wide range of metal cations, because most of the metals except some alkali metals and alkaline earth metals form insoluble sulfides. For other interfering anions such as bromide, iodide and chloride, the scope of the metal forming an insoluble salt is narrower, including for example silver, mercury and lead.

[0081] In some embodiments, the metal salt comprises a metal present in the reference element and participating in the reference redox reaction. Thus, any dissolution of the metal salt within the electrode does not release metal species participating in the competitive redox reaction at the reference element. In some embodiments, the metal salt comprises a cation selected from silver and mercury, and an anion selected from chloride and sulfate. In particular, AgCl may be a preferred ion exchange metal salt for the Ag / AgCl reference element, Ag 2 SO 4 Can be for Ag / Ag 2 SO 4 The preferred ion exchange metal salts of the reference element, and Hg 2 Cl 2 May be the preferred ion exchange metal salt for the saturated calomel reference element.

[0082] Ion exchange resins as solid ion exchange materials

[0083] In some embodiments, the solid ion exchange material is an ion exchange resin. Ion exchange resins are believed to work in a similar manner to metal salts by exchanging interfering ions with ions of the exchange resin, thereby immobilizing the interfering ions and preventing them from interacting with the reference element.

[0084] Ion exchange resins are polymers, such as cross-linked polystyrene, with ionic functional groups balanced by exchangeable ionic charges. Both cation exchange resins and anion exchange resins are known, and either can be selected depending on whether it is necessary to intercept and fix cationic or anionic interfering ions. In some embodiments, the ion exchange resin is an anion exchange resin, such as a strongly basic or weakly basic ion exchange resin. Basic ion exchange resins typically include side chain quaternized amine functional groups, wherein exchangeable anionic charge balance cationic amine groups. The ion exchange resin included in the electrode can therefore initially be loaded with suitable non-interfering anions, such as chloride. The affinity of the basic ion exchange resin for the non-interfering anions initially loaded therein can be lower than the interfering anions present in the analyte, thereby facilitating the interfering anions to be fixed on the resin.

[0085] It is preferred to use a resin whose exchange ion matches the exchange ion of the redox pair in the reference element. In the case of an Ag / AgCl reference, possible candidates include chloride-based exchange resins such as Amberjet 4200 Cl, Amberlite IRA410 Cl, Dowex 1X8 chloride form and Dowex Marathon A chloride form.

[0086] Location of solid ion exchange materials

[0087] At least a portion of the solid ion exchange material is located between the analyte contacting surface of the electrode and the reference element. As described above, the role of the solid ion exchange material is to intercept and immobilize interfering anions as they diffuse into the electrode and thereby reduce the likelihood of undesirable interactions at the reference element. Therefore, the solid ion exchange material should be located and dispersed in the electrode in a manner suitable for performing this function.

[0088] It is also clear to the skilled person that the ion exchange material actually involved in the sacrificial ion exchange reaction should not be in electrical communication with the reference element, otherwise the reaction would adversely affect the measured reference potential. Therefore, at least the sacrificially reactive portion of the solid ion exchange material is physically separated from the reference element, for example by an insulating polymer matrix of the composite material. The reference element is electrically insulated from at least the sacrificially reactive portion of the solid ion exchange material.

[0089] Solid ion exchange material can be loaded in the polymer composite material in the electrode.It can be loaded in the polymer matrix of the same composite material of solid inorganic salt, and / or it can be loaded in the different polymer composite materials between the electrode surface and the reference element, such as discrete electrode layer.Solid ion exchange material and solid inorganic salt are loaded in the polymer composite material in the electrode, such as the same composite material, can provide many advantages, including simple manufacture, for the control of electrode hydration and effective interception and fixed interfering ion.It can also provide excellent electrode life and reliability, be included in abrasive or corrosive analyte, because solid component can be embedded and optionally dispersed throughout polymer matrix (or multiple matrix), and described polymer matrix can be customized (adjustment, tailor) for its compatibility with such analyte.This structure also provides by removing the surface layer of composite electrode to renew the electrode used, such as the opportunity of the electrode with surface dirt, and can not lose the protection ability of electrode.

[0090] In some embodiments, the solid ion exchange material is present in a polymer matrix of the same composite material in which the solid inorganic salt is loaded. The solid ion exchange material and the solid inorganic salt comprising the reference anion can thus be co-dispersed in the polymer matrix, for example as a granular material. The solid ion exchange material can be present in an amount of at least 1 wt %, for example at least 3 wt %, of the composite material.

[0091] In such a configuration, the composite material can be exposed, for example, through a window in the electrode housing, thereby forming an electrode surface for contacting an analyte. In use, the electrode is immersed in the analyte and hydrated due to water penetration into the composite material. The interfering ions diffused into the composite material react with the solid ion exchange material through an ion exchange reaction, thereby being fixed in the composite material before reaching the reference element. The inventor has found through experiments that sulfide anions are fixed in a thin surface layer of a composite material comprising 5 or 10 wt % of AgCl dispersed in the matrix, and do not penetrate into a depth that may interfere with the reference element. Therefore, the reference element should be located at a sufficiently deep position below the composite surface so that the interfering ions are fixed before reaching it, while still allowing sufficient ionic conductivity between the reference element and the analyte. In some embodiments, the reference element is between 1mm and 10mm from the surface.

[0092] Figure 1Describe one such embodiment of the present invention.Electrode 100 includes a reference element 102 embedded in a composite material 104. Reference element 102 includes a silver wire having a proximal end 106 coated with silver chloride and in contact with composite material 104. Distal end 108 extends out of the composite material and can therefore be electrically connected to a potentiometer. Composite material 104 includes a matrix of polyvinyl acetate crosslinked with about 2% by weight of ethylene glycol dimethacrylate (EGDMA). The matrix is ​​loaded with granular potassium chloride (KCl) present in an amount greater than 50% by weight of the composite material and granular silver chloride (AgCl) present in an amount of about 5% by weight of the composite material. Granular components are dispersed throughout the composite material. Impermeable polymer shell 110 encapsulates the composite material except at window 112, where the surface 114 of the composite material is exposed to contact with the analyte.

[0093] In use, the electrode 100 is immersed in an aqueous analyte that includes one or more target species for analysis and one or more interfering anions including sulfur. The composite material hydrates via the window 112, dissolving some of the KCl and establishing a saturated concentration of chloride ions at the reference element 102. Thus, the electrode 100 provides a stable Ag / AgCl reference potential against which the potential of the ion selective or working electrode can be measured, as will be explained in more detail below.

[0094] Interfering anions present in the analyte will penetrate the composite material during the initial hydration process and will penetrate the composite material by diffusion during the continued use of the reference electrode. However, according to the principles disclosed herein, the interfering anions are fixed on the granular AgCl particles located between the surface 114 and the reference element 102, such as at position 116. The ion exchange reaction that is believed to fix the sulfur anions is a salt metathesis reaction shown by Equation 2:

[0095] S 2- (aq)+2AgCl(s)→Ag 2 S(s)+2Cl - (aq) (2)

[0096] Considering that the interior of the composite material 104 already has a saturated concentration of chloride and the reference element is electrically insulated from the AgCl particles that intercept and fix the sulfide ions, the release of chloride anions by the ion exchange reaction has no effect on the measured reference potential.

[0097] Figure 2Another embodiment is depicted in FIG. Electrode 200 is a printed electrode formed on substrate 201 by printing techniques such as screen printing or inkjet printing. Substrate 201 can be any of a wide range of substrates, including polymer substrates (e.g., polyethylene terephthalate, polyimide), paper substrates, glass substrates, ceramic substrates, or any of these substrates with a film coating (including indium tin oxide). Reference element 202 is a printed layer including silver and silver chloride, and can be printed with commercially available Ag / AgCl ink. A layer of composite material 204 is printed on the reference element, except at distal end 208, which is left exposed and can therefore be electrically connected to a potentiometer. Composite material 204 includes a polymer matrix, such as polyvinyl acetate (PVAc), in which both KCl and AgCl particles are dispersed. The layer can be printed with an ink including PVAc and the particles dispersed in acetone, and cured after printing. Composite material 204 can also include multiple printed layers. The surface 214 of the composite material is exposed to contact with the analyte. Optionally, the electrode 200 may further include an insulating printed layer (not shown) on a portion of the composite material 204, but a portion of the composite material surface 214 remains exposed to contact with the analyte. In use, the composite material is hydrated through the surface 214, thereby establishing a reference potential for the electrode 100 as described herein. However, interfering anions such as sulfur radicals are fixed on the AgCl particles in the polymer matrix by ion exchange reactions before reaching the reference element 202.

[0098] In other embodiments, the solid ion exchange material is present in a water-permeable composite material layer between the electrode surface and the composite material loaded with a solid inorganic salt. The water-permeable layer may include a solid ion exchange material dispersed in a hydratable polymer. The water-permeable layer may also optionally include a solid inorganic salt including a reference anion, but this is not necessary for the function of the electrode or to provide protection.

[0099] The hydration of composite material and the ionic conductivity between reference element and analyte are provided via water permeable layer, thus, it will be clear that, for the polymer matrix of composite material, similar considerations about the property of hydratable polymer are applicable. Therefore hydratable polymer should show the hydrophilic-hydrophobic balance suitable for allowing rapid adjustment and low impedance, and dimensional stability and maintenance of solid ion exchange material are provided. Therefore, although hydratable polymer can be the same or different with the polymer matrix of composite material, its composition can be described as for suitable composite material polymer matrix herein usually. Water permeable layer should have enough thickness to allow interference with the interception and fixing of anion, but can not be too thick, because this can increase impedance. In some embodiments, the thickness of water permeable layer is between 1 and 5mm.

[0100] In the embodiment that solid ion exchange material is present in the water permeable layer, composite material is usually not directly exposed to analyte.On the contrary, it is covered by the water permeable layer, completely or at least at its position (local), such as the window area of ​​electrode housing, otherwise it will be expected to contact with analyte.The exposed surface of water permeable layer can then provide the electrode surface for contacting analyte.In use, because water penetrates through the water permeable layer into composite material, electrode immerses analyte and hydrates.The interfering ions diffused through the water permeable layer react with solid ion exchange material via ion exchange reaction, thereby being fixed in the water permeable layer before reaching composite material or reference element.

[0101] It is of course not excluded that a further water-permeable layer may be present between the composite material loaded with inorganic salts and the layer comprising solid ion exchange material, or as an outer layer forming the analyte contacting surface of the electrode.

[0102] Figure 3 One embodiment of the present invention is depicted in Figure 1 1. The electrode 100 depicted in FIG. 100 is described. In the electrode 300, the reference element 102 is embedded in a composite material 304, which includes a polyvinyl acetate matrix cross-linked with EGDMA in which particulate KCl is dispersed. However, the particulate ion exchange material is not present in the composite material, but instead is present in a water-permeable layer 318 arranged directly against the composite material 304. Layer 318 includes a polyvinyl acetate matrix cross-linked with EGDMA in which particulate AgCl is dispersed, and has a thickness of about 1-5 mm. The surface 314 of the water-permeable layer is exposed to contact with the analyte in the window 112 of the housing 110.

[0103] In use, electrode 300 is immersed in aqueous analyte, and the aqueous analyte comprises one or more target species for analysis and one or more interfering anions comprising sulfur radical. Water permeable layer and composite material are hydrated via window 112, dissolve some of KCl and set up the chloride ion of saturation concentration at reference element 108. Therefore electrode 100 provides stable Ag / AgCl reference potential. Interfering anions present in analyte will infiltrate water permeable layer in initial hydration process, and infiltrate water permeable layer by diffusion during the continuous use of reference electrode. However, according to principle disclosed herein, interfering anions are fixed on granular AgCl particles in water permeable layer, for example, at position 316 between surface 314 and reference element 102.

[0104] Method for manufacturing solid-state reference electrode

[0105] It is clear from the above discussion that many different electrode configurations fall within the scope of the present invention. Accordingly, the method of manufacturing the solid-state reference electrode will also vary.

[0106] The method generally comprises making a composite material, the composite material comprising a water-permeable polymer matrix loaded with a solid inorganic salt comprising a reference anion. In some embodiments, a solid ion exchange material is also dispersed in the polymer matrix. Solid inorganic salts and solid ion exchange materials have been described herein.

[0107] In some embodiments, solid inorganic salts and optionally solid ion exchange materials are combined with polymer precursors, such as polymerizable compositions (polymerizable ingredients) including one or more monomers, crosslinkable polymers or curable resins. The polymer precursors are then polymerized, crosslinked and / or cured to form a water-permeable polymer matrix loaded with inorganic salts and optionally solid ion exchange materials.

[0108] When the water-permeable polymer matrix includes a vinyl polymer, the method may include combining a solid inorganic salt and optionally a solid ion exchange material with a polymerizable composition including one or more vinyl monomers. The polymerizable composition may optionally include a crosslinker comprising at least two copolymerizable vinyl functional groups. Suitable vinyl monomers and crosslinkers have been described herein. The composite material is then manufactured by polymerizing the composition, typically in the presence of a free radical initiator or catalyst. The polymerizable composition may therefore include a photoinitiator, such as 2,2-dimethoxy-2-phenylacetophenone. The method may then include irradiating the mixture with UV light for a time sufficient to initiate and satisfactorily complete the polymerization. Alternatively, the mixture may include a thermally activated initiator, such as 2,2'-azobis(2-methylpropionitrile). The method may then include heating the mixture to a temperature and time sufficient to initiate and satisfactorily complete the polymerization. It is also envisioned that a composite material with a crosslinked polymer matrix may be manufactured by combining a solid inorganic salt and optionally a solid ion exchange material with an uncrosslinked vinyl polymer and then crosslinking the polymer.

[0109] Composite material is made to be in ionic communication with reference element. Suitable reference element has also been described. In some embodiments, reference element is therefore contacted with a polymer precursor containing inorganic salt and optionally solid ion exchange material before completion of polymerization, crosslinking or curing. For example, reference element can be inserted into polymer precursor, or polymer precursor can be cast or printed on reference element. Then, polymerization or curing can be initiated to manufacture an electrode in which reference element contacts or adheres to composite material.

[0110] In embodiments where the solid ion exchange material is dispersed in the composite material, the method may include providing a surface of the composite material as an electrode surface to contact the analyte in use. For example, if a polymer precursor is polymerized or cured in the housing, a window of suitable size may then be created in the housing to expose the surface of the composite material.

[0111] In the embodiment that solid ion exchange material is present in the water permeable layer of polymer composite material between the composite material that is located at electrode surface and load has solid inorganic salt that comprises reference ion, method of the present invention can comprise providing water permeable layer.Water permeable layer can be provided, and makes it comprise solid ion exchange material and optionally comprise the solid inorganic salt of reference anion that are dispersed in hydratable polymer.Hydrable polymer has been described in this article.Therefore, it can be manufactured in the similar mode of polymer matrix with composite material, for example, by solid ion exchange material is dispersed in polymer precursor and make precursor polymerize, crosslink or solidify to form the water permeable layer with necessary properties.

[0112] The water permeable layer may be formed on the composite material. This may involve forming the composite material on the water permeable layer or forming the water permeable layer on the composite material. For an example of the first alternative, Figure 3 The electrode 300 depicted in Figure 1 can be manufactured by placing a mixture of vinyl acetate, EGDMA, granular AgCl and a free radical initiator in a layer at the bottom of the housing 110 (before the window 112 is opened). The mixture is then polymerized to form a water-permeable layer 318, which includes a cross-linked polyvinyl acetate with dispersed AgCl. The mixture of vinyl acetate, EGDMA, granular KCl and a free radical initiator is then transferred to the housing, and the reference element 102 is inserted into the mixture to the desired depth. The mixture is then polymerized to form a composite material 304 on top of the water-permeable layer. Finally, a window 112 is created in the housing to expose the surface 314.

[0113] In an example of a second alternative, a printed electrode can be manufactured on a substrate by successively printing and curing i) a conductive reference element layer comprising Ag and AgCl, ii) a composite material layer comprising KCl dispersed in a water-permeable polymer matrix on a portion of the reference element, and ii) a water-permeable layer comprising AgCl dispersed in a hydratable polymer covering the composite layer.

[0114] In embodiments where the solid ion exchange material is dispersed in a water permeable layer, the method may include providing a surface of the water permeable layer as an electrode surface to contact the analyte in use. For example, if the electrode is prepared in a housing, a window of suitable size may be created in the housing to expose the surface of the water permeable layer.

[0115] Systems and methods for electrochemical analysis of analytes

[0116] The solid-state reference electrode of the present invention can be used in electrochemical analysis, including potentiometric, voltammetric and amperometric measurements. In potentiometric analysis, the potential difference between a reference electrode in contact with the analyte and an ion-sensitive electrode is measured passively. In three-electrode voltammetric analysis, a working electrode and a counter electrode are in contact with the analyte, the potential between these electrodes varies according to a predetermined pattern, and the resulting current transfer to the analyte is measured. The reference electrode is coupled to the working electrode and thus allows the working potential to be measured and controlled in the analysis. A similar arrangement is used in amperometric analysis, except that the current flow is controlled and the resulting potential difference between the working electrode and the reference electrode is measured.

[0117] The present invention therefore relates to a system for electrochemical analysis of an analyte. The system comprises a solid-state reference electrode as described herein, an ion selective electrode or a working electrode (depending on the type of analysis to be performed), and a device for measuring the potential difference between the ion selective electrode or the working electrode and the reference electrode, such as a voltmeter or a potentiostat.

[0118] In some embodiments, the system is a potentiometric system for determining the concentration of ions in an analyte. The system includes a solid-state reference electrode as described herein, an ion selective electrode, and a device for measuring the potential difference between the ion selective electrode and the reference electrode, such as a voltmeter or a potentiostat.

[0119] The present invention also relates to a method for electrochemical analysis of an analyte. The method comprises contacting a solid reference electrode and an ion selective electrode or a counter electrode as described herein with the analyte and measuring the electrochemical potential difference between the reference electrode and the ion selective electrode or the working electrode. The two electrodes may be contacted with the analyte by immersion in the analyte. The analyte may be an aqueous analyte. The electrochemical potential difference may be measured with a voltmeter or a potentiostat.

[0120] In some embodiments, the method is a method of determining the concentration of an ion in an analyte. The method comprises contacting a solid-state reference electrode and an ion selective electrode as described herein with the analyte, and measuring the electrochemical potential difference between the ion selective electrode and the reference electrode.

[0121] In systems and methods for determining ion concentration, the ion selective electrode is not considered to be particularly limited and will depend on the target application. For example, the ion selective electrode can be a potentiometric sensor for pH, oxidation reduction potential (ORP), cyanide, metal ions, or a biosensor. In some embodiments, the ion selective electrode is sensitive to hydrogen ions, so that the system is a pH meter. In some embodiments, the ion selective electrode is a solid state electrode, such as a polymer composite electrode. An example of such an electrode is a composite hydrogen ion selective sensor, which includes Ta dispersed in a polymer matrix. 2 O 5 and RuO 2 A mixture of as described in WO2016 / 033632.

[0122] Interfering ions are expected in analytes undergoing electrochemical analysis in many applications including environmental monitoring, process monitoring in the mining and chemical industries, oil and gas related monitoring systems, biological systems, wastewater treatment and pipelines.

[0123] In some embodiments, the analyte is an acidic and / or abrasive analyte, where interfering ions present additional challenges to maintaining a stable reference potential. Examples of such analytes are found in the mining and mineral processing industries. In some embodiments, the analyte is a leachate and leach slurry, such as from a heap leaching operation, or an acid mine drainage stream.

[0124] In some embodiments, the analyte includes one or more interfering ions. The interfering ions can be interfering anions, such as sulfide, iodide, bromide, and cyanide. In some embodiments, the analyte includes sulfide.

[0125] Example

[0126] The present invention is described with reference to the following examples. It will be understood that these examples are illustrative rather than limiting of the invention described herein.

[0127] Material

[0128] All starting materials were purchased from Sigma Aldrich or other commercial suppliers. The KCl used was of analytical quality (VWR AnalaR) to avoid a shift in the reference potential due to any inorganic contaminants. The monomers, crosslinkers, and initiators used were 98% pure or higher. Silver particles (99.9%, 5-8 microns) and silver chloride coarse powder (99.997%) were purchased from AlfaAesar. Amberjet TM 4200 Cl (strong base (Type I) ion exchange resin in chloride form, with a particle size of 600-800 μm) was purchased commercially.

[0129] Example 1. Preparation of electrodes

[0130] Silver wires (1.5 mm thick, 99.95% Ag) were polished with fine sandpaper and washed with ethanol. Each wire was inserted into a 1M KCl solution and connected to a potentiostat. The wires were coated with a silver chloride coating by passing a small current (7 mA, 100 seconds) between a silver electrode (anode) and a platinum counter electrode (cathode).

[0131] A mixture of vinyl acetate and ethylene glycol dimethacrylate (EGDMA) was prepared, wherein EGDMA accounted for 2 wt% of the total monomers. A small amount of 2,2'-azobis(2-methylpropionitrile) (≤ 2 wt%) was added to the mixture as a thermal initiator.

[0132] Dry KCl powder was added to each mixture and the settled slurry was transferred to a glass vial (1-10 mL volume) by pipette such that the vial was filled with KCl powder and the monomer mixture filled the inter-particle spaces. TM 4200 Cl ion exchange resin) was dispersed in some of the mixture, as shown in Table 1. In the subsequent polymerization process, a small amount (0.1-0.5 mL) of additional monomer mixture was transferred to the vial to form a salt-free seal layer on the top of the vial. The mass ratio of KCl to monomer in the mixture was about 2:1.

[0133] Then silver chloride coated silver wire (2-5cm length, depending on vial size) is inserted into each vial, and then the vial is sealed. The monomers are copolymerized by heating the mixture to about 50°C for about 18 hours. After the polymerization is complete, the bottom portion of the vial is removed by grinding to expose a solid composite material comprising a matrix of EGDMA cross-linked polyvinyl acetate (PVAc) loaded with both solid KCl and solid particulate additives. The electrode is then ready for use.

[0134] Table 1

[0135]

[0136] Example 2. Electrochemical testing of electrodes with metal salt additives

[0137] 1 g / L Na in pH 9 buffer 2The electrochemical performance of the electrodes E1-E5 prepared in Example 1 was evaluated in S solution (1.5 mL vial volume). The potential response of the electrodes was measured against a saturated calomel electrode (SCE) obtained from Koslow Scientific Company (which was regularly maintained during the electrochemical testing to ensure stable performance). The open circuit potential (OCP) signal of the electrodes was recorded using a multichannel potentiostat (Biologic VMP3 potentiostat).

[0138] Figure 4 The potential response for the electrodes is depicted. The control electrode E1 was initially stable in potential relative to SCE, but began to drift after about 30 days of exposure to the analyte. After 120 days online, the potential was -132 mV relative to SCE, compared to a theoretical potential of -45 mV relative to SCE. Figure 4 The time period indicated by "X" in corresponds to the time period in which maintenance (maintenance) of the SCE fails.

[0139] In contrast, the inclusion of 5 wt% (E2) or 10 wt% (E3) AgCl particles dispersed throughout the composite resulted in a stable reference potential throughout the experiment, despite the presence of sulfide anions in the analyte. After 120 days online, the potential was -44 mV relative to SCE, compared to a theoretical potential of -45 mV relative to SCE. The potentials were nearly identical for electrodes E2 and E3 throughout the experiment. After the experiment was completed, a discolored layer was observed at the composite interface with the analyte; however, no discoloration was apparent deeper in the composite.

[0140] It is believed that the protection of the electrode potential is due to the fixation of the sulfur anions in this layer, thereby preventing them from diffusing through the composite to reach the Ag / AgCl wire. The sulfur anions exchange with the chloride anions on the AgCl particles to form insoluble Ag 2 S and releases free chloride anions.

[0141] Including Ag metal particles at 5 wt% (E4) or 10 wt% (E5) was not effective in protecting the electrode from drift caused by sulfide anion interference. For electrode E4 with 5 wt% Ag metal particles, the potential was stable for the first 20 days, but then severe drift was observed.

[0142] Example 3. Electrochemical testing of electrodes with ion exchange resin additives

[0143] 1 g / L Na in pH 9 buffer 2The electrochemical performance of electrodes E1 and E6 prepared in Example 1 was evaluated in triplicate in S solution (1.5 mL vial volume). The potential response of the electrode was measured against a saturated calomel electrode (SCE) obtained from Koslow Scientific Company (which was regularly maintained during the electrochemical testing to ensure stable performance). The open circuit potential (OCP) signal of the electrode was recorded using a multichannel potentiostat (Biologic VMP3 potentiostat).

[0144] Figure 5 The potential response for the electrodes is depicted, where the potential shown is the average of three electrodes. The control electrode E1 without any additive and the electrode E6 with the ion exchange resin additive initially provided very similar results, plateauing close to the theoretical potential of -45 mV relative to SCE. By about 30 days, there was an indication that the standard electrode E1 was drifting due to interference from sulfur radicals, as was also seen in Example 2 at about this time. In contrast, the electrode E6 containing the ion exchange resin loaded with chloride radicals continued to show a highly stable potential.

[0145] After 24 days online, an E1 and an E6 electrode were removed, the shell was removed, and the electrode was longitudinally cross-sectioned with a razor blade. Visual inspection of the electrode interior confirmed that the ion exchange resin beads were distributed throughout the composite material. The electrode was then subjected to XRF analysis. The elemental mapping (map) (20mmx10mm) of the dry cross section was collected in air at 20 mbar using a Bruker M4 Tornado high-performance μXRF spectrometer equipped with a Rh x-ray tube, polycapillary optics, and a silicon drift detector. The polycapillary optics allow for the collection of mappings with a spot diameter of 25 μm for Mo Kα. The pixel spacing was 25 μm with a 20ms pixel. -1 The XRF images were mapped with an acquisition time of 50 kV and 599 μA using a 12.5 μM Al filter. It is clear from the XRF imaging that sulfur selectively accumulates on the resin beads dispersed in the composite of the E6 electrode. In contrast, no sulfur accumulation is visible in the D1 electrode composite.

[0146] Example 4. Accelerated poisoning test

[0147] Electrodes E1 (no additive) and E2 (5 wt % AgCl additive) were placed in 1 mmol / L sodium sulfide (Na 2 The electrodes were then subjected to longitudinal cross-sectioning and XRF analysis in the same manner as in Example 3. The elemental mapping results showed that less sulfur and bromine entered the interior of the E1 electrode compared to the E2 electrode.

[0148] Example 5. Electrochemical testing of electrodes with metal salt additives under highly acidic conditions

[0149] In 1000ppmNa acidified to pH 2.6 2 The electrochemical performance of electrodes E1 (no additive) and E2 (5 wt % AgCl additive) prepared as in Example 1 was evaluated in aqueous S solution. Five identical electrodes of each type were tested in parallel. The potential response of the electrode was measured against a commercial Ag / AgCl reference electrode with 3 mol / liter KCl internal electrolyte (which was regularly maintained during the electrochemical testing to ensure stable performance).

[0150] Figure 6 Describe the potential response for the electrode. Three of the control electrode E1 provide an initial response close to the theoretical potential difference of -9mV, but all fail when online for 7 days. In contrast, the five electrodes E2 containing AgCl are all stable for nearly 50 days. After that, their performances differ, with two of them drifting significantly, but three continue to provide reliable reference potentials for more than 200 days online.

[0151] Those skilled in the art will appreciate that the invention described herein is susceptible to variations and modifications other than those specifically described. It is understood that the invention includes all such variations and modifications that fall within the spirit and scope of the invention.

Claims

1. Solid-state reference electrode, including: a reference element in ionic communication with a composite material, the composite material comprising an electrically insulating, water-permeable polymer matrix loaded with a solid inorganic salt comprising a reference anion, wherein the solid inorganic salt is a particulate solid dispersed in the polymer matrix, wherein the solid inorganic salt is sufficiently soluble in water such that hydration of the composite material will produce a constant saturated solution concentration of the reference anion at the reference element, and wherein the reference anion is capable of participating in a desired redox half-reaction at the reference element to provide a reference potential; an electrode surface for contacting the analyte; as well as a solid ion exchange material between the electrode surface and the reference element, the solid ion exchange material comprising one or more non-interfering anions, wherein the reference element is electrically insulated from the solid ion exchange material, wherein in use, said solid ion exchange material is immobilized to solubilize one or more interfering anions when present in the analyte by exchange with said non-interfering anions, Whereas interfering ions are able to participate in competing redox reactions at the reference element, which results in deviations from the expected electrode potential, non-interfering ions are ions that do not significantly affect the measured electrode potential.

2. The solid-state reference electrode of claim 1, wherein the solid ion exchange material comprises a metal salt or an ion exchange resin.

3. The solid-state reference electrode of claim 1, wherein the solid ion exchange material comprises a metal salt having a lower water solubility than the solid inorganic salt.

4. A solid-state reference electrode according to claim 1, wherein the non-interfering anion comprises the reference anion.

5. The solid state reference electrode of claim 1, wherein the solid ion exchange material comprises a metal salt comprising a cation selected from the group consisting of silver, mercury, and lead.

6. The solid state reference electrode of claim 1, wherein the solid ion exchange material comprises a metal salt comprising a metal present in the reference element.

7. The solid-state reference electrode according to claim 1, wherein the interfering anion is selected from the group consisting of sulfur, iodide, bromide and cyanide.

8. The solid-state reference electrode of claim 1, wherein the solid ion exchange material is a granular material.

9. A solid-state reference electrode according to any one of claims 1 to 8, wherein the solid ion exchange material is supported in a polymer matrix of the composite material or in a further polymer composite material located between the electrode surface and the reference element.

10. A solid-state reference electrode according to claim 9, wherein the further polymer composite comprises a solid anion exchange material dispersed in a hydratable polymer.

11. The solid-state reference electrode of claim 9, wherein the solid ion exchange material is supported in a polymer matrix of the composite material.

12. The solid-state reference electrode of claim 11, wherein the solid ion exchange material is present in an amount of at least 1% by weight of the composite material.

13. The solid-state reference electrode of claim 9, wherein the solid ion exchange material is supported in a water-permeable layer of an additional polymer composite material located between the electrode surface and the composite material.

14. A solid state reference electrode according to any one of claims 1 to 8, wherein the reference anion is chloride.

15. The solid-state reference electrode according to claim 14, wherein the reference element is selected from Ag / AgCl and calomel.

16. The solid-state reference electrode according to any one of claims 1 to 8, wherein the water permeable polymer matrix comprises a vinyl polymer of a vinyl monomer comprising a heteroatom.

17. The solid-state reference electrode of claim 16, wherein the vinyl polymer is cross-linked.

18. The solid-state reference electrode according to claim 17, wherein the cross-linked vinyl polymer is a copolymer of i) at least one vinyl monomer selected from vinyl esters, vinyl amides and acrylates and ii) a cross-linking agent comprising at least two copolymerizable vinyl functional groups.

19. The solid-state reference electrode according to any one of claims 1 to 8, wherein the composite material comprises at least 30% by mass of solid inorganic salt.

20. A system for electrochemical analysis of an analyte, the system comprising: The solid-state reference electrode according to any one of claims 1 to 8; a second electrode selected from an ion selective electrode and a working electrode; as well as means for measuring the potential difference between said second electrode and said reference electrode.

21. A method for electrochemical analysis of an analyte, the method comprising: contacting i) a solid reference electrode according to any one of claims 1 to 8 and ii) a second electrode selected from an ion selective electrode and a working electrode with an analyte; and The electrochemical potential difference between the second electrode and the reference electrode is measured.

22. The method of claim 21, wherein the analyte comprises dissolved one or more interfering anions, wherein the one or more interfering anions are capable of participating in a competitive redox reaction at the reference element, which results in a deviation from an expected electrode potential.

23. The method of claim 22, wherein the interfering anion is selected from the group consisting of sulfide, iodide, bromide and cyanide.

24. The method of claim 22, wherein the interfering anion comprises sulfide.

25. The method of claim 22, wherein the solid state ion exchange material immobilizes the one or more interfering anions by exchange with the non-interfering anions.