A low-cost, high-performance multi-phase rare earth permanent magnetic material and its preparation method

By using multi-main phase alloys and grain boundary reconstruction technology in rare earth permanent magnet materials, a multi-core shell structure and continuous non-ferromagnetic grain boundary phases are formed, which solves the problem of insufficient coercivity and high cost of rare earth permanent magnet materials in high temperature environments. Problem, high-performance and low-cost rare earth permanent magnet materials have been prepared, which are suitable for new energy fields.

CN114678182BActive Publication Date: 2024-10-29ZHEJIANG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210393709.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-14
Publication Date
2024-10-29
Estimated Expiration
2042-04-14

AI Technical Summary

Technical Problem

Existing rare earth permanent magnet materials have insufficient coercivity in high-temperature environments, resulting in an increase in the content of heavy rare earth elements, magnetic dilution effects and high production costs. Moreover, the traditional process is complex and not suitable for large-size magnets.

Method used

Using low-cost and high-performance multi-main phase rare earth permanent magnet materials, through main phase alloys without heavy rare earths, main phase alloys with added heavy rare earths and grain boundary reconstruction auxiliary alloys, combined with rapid solidification casting technology and nitrogen or argon gas protection Mixing and sintering under conditions form a multi-core shell structure and a continuous non-ferromagnetic grain boundary phase, optimizing the coercive force and magnetic properties of the magnet.

Benefits of technology

It greatly improves the coercivity and magnetic energy product of rare earth permanent magnet materials, reduces the amount of heavy rare earth and raw material costs, is suitable for magnets of different sizes, has a simple process and is suitable for large-scale production, and meets the high performance requirements in the new energy field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114678182B_ABST
    Figure CN114678182B_ABST
Patent Text Reader

Abstract

The invention discloses a low-cost, high-performance multi-main-phase rare-earth permanent magnet material and a preparation method thereof. The multi-main-phase sintered magnet is prepared based on the multi-main-phase alloy technology and the grain boundary reconstruction technology. By reducing the content of the B element in the main-phase alloy and increasing the content of at least one metal element such as Ga, Cu, Al, etc., the rare earth element content in the main-phase alloy component is relatively low, thereby providing a characteristic main-phase alloy with low rare earth content and low cost. The grain boundary reconstruction auxiliary alloy component is innovatively designed, and the mass fraction of the grain boundary phase in the magnet is significantly increased during the sintering and heat treatment process, and the distribution and morphology of the grain boundary phase are optimized to form a continuous non-ferromagnetic grain boundary phase, which more effectively isolates the short-range magnetic exchange between adjacent main-phase grains. At the same time, an uneven heavy rare earth multi-core-shell structure of the multi-main-phase magnet is constructed, and the enrichment of the heavy rare earth element in the grain boundary region is reduced, thereby efficiently utilizing the heavy rare earth element, greatly improving the coercive force of the magnet, and improving the comprehensive magnetic properties of the magnet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of rare earth permanent magnets, and in particular to a low-cost, high-performance multi-main-phase rare earth permanent magnet material and a preparation method thereof. Background Art

[0002] Sintered rare earth permanent magnets are currently the most powerful and widely used permanent magnet materials. They are widely used in energy, transportation, information, medical care, and national defense, and have developed into strategic functional materials in the fields of national economic construction and national defense technology. Globally, the continued growth in demand for sintered rare earth permanent magnets has led to an increasingly tight supply of rare earth raw materials, and rare earth prices have continued to fluctuate. The global rare earth industry has begun to face severe cost control challenges. In particular, the wind power generation and new energy vehicle industries have flourished in recent years. The application of these high-temperature fields has also put forward higher requirements on the performance of sintered rare earth permanent magnets, especially the coercive force.

[0003] At present, heavy rare earth elements Dy and Tb are commonly added to increase the intrinsic magnetocrystalline anisotropy field H of magnets. A The coercivity of sintered rare earth permanent magnets is improved by using a method. The higher the working environment temperature, the higher the room temperature coercivity required for the service magnet, and the higher the content of heavy rare earth elements required for the corresponding magnet. In the traditional process, heavy rare earth metals are directly added during the smelting process. After Dy and Tb elements uniformly replace Nd inside the main phase grains, the coercivity of the magnet is improved. However, the antiferromagnetic coupling between Dy, Tb and Fe elements will cause serious magnetic dilution effect, resulting in a significant reduction in remanence and magnetic energy product. The grain boundary diffusion process coats a heavy rare earth diffusion source on the surface of the magnet, and diffuses the heavy rare earth elements into the interior of the magnet through long-term heat treatment, forming a heavy rare earth-rich hard magnetic shell layer in the epitaxial layer of the main phase grains, avoiding the magnetic dilution effect and maintaining the remanence. However, the grain boundary diffusion method is limited by the diffusion depth and is only applicable to small-sized magnets. In addition, the process is complicated, and long-term high-temperature diffusion heat treatment increases the production cost.

[0004] Studies have shown that the coercive force of sintered rare earth permanent magnets is not only related to the intrinsic magnetocrystalline anisotropy field, but also closely related to the distribution of rare earth-rich grain boundary phases. The rare earth-rich grain boundary phases in traditional sintered magnets come from the excess rare earth elements in the composition design. In addition to forming a 2:14:1 main phase, the redundant rare earth elements act as liquid phase sintering aids during sintering and heat treatment. Blindly reducing the content of rare earth elements will lead to defects such as poor density of the magnet, discontinuity of the grain boundary phase, and reduce the coercive force of the magnet. How to redesign the main phase alloy composition, introduce new grain boundary phases, combine new technologies, and take into account the composition and microstructure optimization of the main phase and grain boundary phases is an important challenge in the preparation of high-performance rare earth permanent magnet materials. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a low-cost, high-performance multi-phase rare earth permanent magnet material and a preparation method thereof.

[0006] The present invention provides a low-cost, high-performance multi-phase rare earth permanent magnet material, characterized by comprising a main phase alloy I without heavy rare earth, one or more main phase alloys II with heavy rare earth added, and a grain boundary reconstruction auxiliary alloy. The main phase alloy I without heavy rare earth has a composition of RE in terms of mass percentage. x1 Q bal M y1 M' z1 B w1 , wherein RE is one or more of the other lanthanide rare earth elements except the heavy rare earth elements Dy and Tb, Q is one or more of the elements Fe, Co, and Ni, M is one or more of the elements Cr, Mn, Mo, N, Nb, P, Pb, Si, Ta, Ti, V, and Zr, M' is one or more of the elements Ga, Al, and Cu, and B is a boron element, wherein x1, y1, z1, and w1 satisfy the following relationship: 22≤x1≤30, 0≤y1≤2, 0.2≤z1≤1.0, and 0.8≤w1≤1.0; the main phase alloy II with the addition of heavy rare earth elements has an average composition of (RE in percentage by mass) 1-a HRE a ) x2 Q bal M y2 M' z2 B w2 , wherein RE is one or more of the other lanthanide rare earth elements except the heavy rare earth elements Dy and Tb, HRE is one or two of the heavy rare earth elements Dy and Tb, Q is one or more of the elements Fe, Co, and Ni, M is one or more of the elements Cr, Mn, Mo, N, Nb, P, Pb, Si, Ta, Ti, V, and Zr, M' is one or more of the elements Ga, Al, and Cu, and B is the boron element, wherein a, x2, y2, z2, and w2 satisfy the following relationship: 0.2≤a≤0.8, 22≤x2≤29, 0≤y2≤2, 0.2≤z2≤1.1, and 0.8≤w2≤0.95; the grain boundary reconstruction auxiliary alloy is calculated in mass percentage, and its composition is RE m TM 100-m , wherein RE is one or more of the rare earth La, Ce, Pr, Nd, Sm, Gd, Dy, Tb, Ho, Y, and contains at least one heavy rare earth element Dy or Tb; TM is one or more of H, O, F, Fe, Ga, Ti, Cu, Al, Co, Nb, Zr, Ta, Si, V, Mo, Mn, Ag, Mg, Zn, wherein 0 <m<100。

[0007] The present invention provides a method for preparing a low-cost, high-performance multi-phase rare earth permanent magnetic material, which is characterized by comprising the following steps:

[0008] 1) According to the designed main phase components, the ingredients are prepared separately, and the vacuum degree is ≤10 -2 Different main phase alloys were melted in a vacuum medium frequency induction furnace at 1000 Pa, and main phase alloy flakes with a thickness of 0.2-0.6 mm were obtained by rapid solidification casting technology. Main phase alloy powders with an average particle size of 2-4 μm were prepared by hydrogen crushing and air flow grinding.

[0009] 2) The ingredients are prepared according to the designed grain boundary reconstruction auxiliary alloy composition, and the grain boundary reconstruction auxiliary alloy powder with an average particle size of 0.5 to 3 μm is prepared through smelting, coarse crushing and ball milling;

[0010] 3) Under nitrogen or argon protection, the main phase alloy powders of different components are uniformly mixed according to a proportion, and then uniformly mixed with the grain boundary reconstruction auxiliary alloy powder; wherein the grain boundary reconstruction auxiliary alloy powder accounts for 0.1 to 10% of the total powder mass; and mixed alloy powders with different heavy rare earth addition amounts are obtained;

[0011] 4) Orienting and pressing the obtained mixed alloy powder in a magnetic field of 1.5 to 2.0 T to obtain a green body;

[0012] 5) The obtained green body is vacuum packaged, cold isostatically pressed at 150-250 MPa, and then sintered and heat treated in a high vacuum positive pressure sintering furnace to obtain a low-cost, high-performance multi-phase magnet.

[0013] It is characterized in that, in step 5), the sintering temperature is 980-1080° C. and the sintering time is 2-5 hours.

[0014] It is characterized in that the heat treatment system in step 5) is to carry out primary heat treatment at 800-950°C for 2-3 hours and secondary heat treatment at 450-700°C for 2-5 hours.

[0015] The invention is characterized in that the main phase alloy composition has a low rare earth content, 22≤x1≤30, 22≤x2≤29, thereby reducing material cost.

[0016] It is characterized in that the main phase grains of the final multi-main phase magnet present a core-shell structure, including two or more main phase grain cores with low heavy rare earth content n1 and main phase grain cores with high heavy rare earth content n2, and hard magnetic shells of main phase grains with high heavy rare earth content n3, wherein n1<n3<n2; its grain boundary phase includes a Q-rich grain boundary phase and a traditional rare earth-rich grain boundary phase, and the mass percentage of Q in the Q-rich grain boundary phase is 40% to 60%, and the mass percentage of M' is 1% to 9%.

[0017] The characteristic is that the Q-rich grain boundary phase and the traditional rare earth-rich grain boundary phase together form a continuous thin layer grain boundary surrounding adjacent main phase grains, thereby ensuring the high coercive force of the magnet.

[0018] It is characterized in that the total rare earth element content in the Q-rich grain boundary phase is lower than that in the traditional rare earth-rich grain boundary phase, wherein the heavy rare earth content n4 is lower than the hard magnetic shell layer of the main phase grains with high heavy rare earth content n3, that is, n4<n3.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1) The present invention synergistically innovates grain boundary reconstruction technology and multi-main phase alloy technology. Based on the phase formation laws and physical and chemical properties of different systems of heavy rare earth Dy / Tb-Fe-B and light rare earth Nd-Fe-B, a variety of main phase alloys and grain boundary reconstruction alloys are redesigned to form a hard magnetic shell layer in the epitaxial layer of the main phase grains to efficiently utilize the heavy rare earth, and give play to the multi-scale magnetic coupling and high squareness advantages of the multi-main phase magnet, greatly improving the coercive force of the multi-main phase magnet while maintaining the remanence and magnetic energy product; and reducing the rare earth element content in the main phase alloy, reducing the amount of heavy rare earth, and greatly reducing the cost of raw materials; by reducing the content of B element in the main phase alloy and increasing the metal Ga , Al, Cu and other at least one element, an additional Q-rich grain boundary phase, that is, Fe, Co, Ni-rich grain boundary phase, is introduced into the sintered permanent magnet, wherein the mass percentage of Fe, Co and Ni is 40% to 60%, and the mass percentage of Ga, Al and Cu is 1% to 9%; on this basis, combined with the grain boundary reconstruction auxiliary alloy and the key preparation technology innovation, additional rare earth elements and grain boundary phases are provided during the sintering and heat treatment process, which is more conducive to optimizing the grain boundary phase distribution, constructing a continuous non-ferromagnetic grain boundary phase, effectively isolating the magnetic coupling between adjacent grains, greatly improving the coercive force of the magnet, and improving the comprehensive magnetic properties of the magnet.

[0021] 2) The low-cost, high-performance multi-main-phase rare earth permanent magnet material prepared by the present invention presents a multi-core-shell structure, wherein the core includes two or more different heavy rare earth contents, typically a low heavy rare earth content n1 main phase grain core and a high heavy rare earth content n2 main phase grain core, and a high heavy rare earth content n3 main phase grain hard magnetic shell, satisfying n1<n3<n2. This uneven heavy rare earth multi-core-shell structure is different from the uniform distribution of heavy rare earth elements in traditional smelting and adding heavy rare earth sintered magnets, and is also different from the grain boundary and shell distribution of heavy rare earth elements in grain boundary diffusion magnets. It is suitable for various types of magnets of different sizes, and also ensures the multi-scale coupling and high squareness of the magnet, thereby improving the coercive force and the utilization efficiency of heavy rare earth. In addition, the total rare earth element content in the formed Q-rich grain boundary phase is lower than that in the traditional rare earth-rich grain boundary phase, among which the heavy rare earth content n4 is lower than the hard magnetic shell of the main phase grains with high heavy rare earth content n3, that is, n4<n3, which further avoids the enrichment of heavy rare earth elements in the grain boundary phase and improves the utilization efficiency of heavy rare earths.

[0022] 3) In summary, the present invention provides a way to efficiently utilize heavy rare earth elements, forming a continuous non-ferromagnetic grain boundary phase while constructing a heavy rare earth multi-core shell structure with an uneven multi-phase magnet. Under the synergistic effect of the two, the coercive force of the magnet is further improved, and the amount of heavy rare earth used in the magnet and the cost of raw materials are greatly reduced. The preparation method provided by the present invention has a simple process and is suitable for large-scale production. At the same time, it ensures high magnetic properties and can meet the stringent requirements of high heat-resistant and high magnetic energy product permanent magnet motors in emerging technology fields such as wind power generation and new energy vehicles. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a typical microstructure model diagram of a low-cost, high-performance multi-phase rare earth permanent magnet material. As can be seen from the figure, in the permanent magnet material, there are multiple core-shell structures, low heavy rare earth content n1 main phase grain core and high heavy rare earth content n2 main phase grain core, and high heavy rare earth content n3 main phase grain hard magnetic shell, where n1<n3<n2; at the same time, there are continuous Q-rich grain boundary phase and traditional rare earth-rich phase, and the heavy rare earth content n4 in the Q-rich grain boundary phase is lower than the high heavy rare earth content n3 main phase grain hard magnetic shell, that is, n4<n3. DETAILED DESCRIPTION

[0024] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments:

[0025] Embodiment 1:

[0026] 1) The main phase components are prepared according to the designed main phase components. In terms of mass percentage, the main phase alloy I without heavy rare earth is composed of (Pr 0.2 Nd 0.8 ) 28.8 Fe bal Co 0.2 Zr 0.2 Ga 0.45 Al 0.35 Cu 0.2 B 0.92 The main phase alloy II with heavy rare earth addition has a composition of [(Pr 0.2 Nd 0.8 ) 0.25 Dy 0.75 ] 26.8 Fe bal Co 0.2 Zr 0.2 Ga 0.45 Al 0.35 Cu 0.2 B 0.92 , at vacuum degree ≤10 -2Different main phase alloys were melted in a vacuum medium frequency induction furnace at 10000 Pa, and main phase alloy flakes with a thickness of 0.35 mm were obtained by rapid solidification casting technology. Main phase alloy powders with an average particle size of 3.1 μm were prepared by hydrogen crushing and air flow grinding.

[0027] 2) According to the designed grain boundary reconstruction auxiliary alloy composition, the composition is Pr 10 Dy 70 Fe 20 , preparing grain boundary reconstruction auxiliary alloy powder with an average particle size of ~2μm through smelting, coarse crushing and ball milling;

[0028] 3) Under nitrogen protection, the main phase alloy I and II powders with different compositions are uniformly mixed in a mass ratio of 19:1, and then uniformly mixed with the grain boundary reconstruction auxiliary alloy powder; wherein the grain boundary reconstruction auxiliary alloy powder accounts for 2% of the total powder mass; in terms of mass percentage, the composition of Pr 5.63 Nd 21.72 Dy 2.4 Fe bal Co 0.2 Zr 0.2 Ga 0.44 Al 0.34 Cu 0.2 B 0.9 Mixed alloy powder;

[0029] 4) Orienting and pressing the obtained mixed alloy powder in a magnetic field of 1.7 T to obtain a green body;

[0030] 5) The obtained green body is vacuum packaged, cold isostatically pressed at 200MPa, and then sintered and heat treated in a high vacuum positive pressure sintering furnace. The sintering temperature is 1065℃, the sintering time is 3h, the primary heat treatment is carried out at 890℃ for 3h, and the secondary heat treatment is carried out at 490℃ for 4h to obtain a low-cost, high-performance multi-phase magnet. The test results of the AMT-4 permanent magnet property measuring instrument show that the magnetic properties of the magnet are B r =13.6kG, H cj =25.9kOe, (BH) max =45.7MGOe, reaching the performance of commercial N48UH brand magnets.

[0031] Comparative Example 1:

[0032] The difference from Example 1 is that the magnet is prepared by a conventional single-phase process, and the actual composition is the same as that of the magnet prepared in Example 1, which is Pr 5.63 Nd 21.72 Dy 2.4 Fe bal Co 0.2 Zr 0.2 Ga0.44 Al 0.34 Cu 0.2 B 0.9 The test results of AMT-4 permanent magnetic property measuring instrument show that the magnetic properties of the magnet are B r =13.3kG, H cj =21.4kOe, (BH) max =43.0MGOe, both lower than Example 1.

[0033] Comparative Example 2:

[0034] The difference from Example 1 is that the magnet is prepared by a conventional single-phase process, and the composition of the single-phase alloy is Pr 5.63 Nd 21.72 Dy 2.4 Fe bal Co 0.2 Zr 0.2 Ga 0.3 Al 0.3 Cu 0.2 B 1.0 , which is different from the composition of the mixed alloy powder in step 3) of Example 1 (the content of B is increased to 1.0wt.%, the content of Ga is reduced to 0.3wt.%, and the content of Al is reduced by 0.3wt.%). The test results of AMT-4 permanent magnetic property measuring instrument show that the magnetic properties of the magnet are B r =13.1kG, H cj =19.5kOe, (BH) max =40.8MGOe, both lower than Example 1.

[0035] Embodiment 2:

[0036] 1) The main phase components are prepared according to the designed main phase components. In terms of mass percentage, the main phase alloy I without heavy rare earth is composed of (Pr 0.2 Nd 0.8 ) 25.6 Fe bal Co 0.4 Nb 0.2 Ga 0.25 Al 0.35 Cu 0.2 B 0.9 The main phase alloy II with heavy rare earth addition has a composition of [(Pr 0.2 Nd 0.8 ) 0.25 Tb 0.75 ] 25.2 Fe bal Co 0.4 Nb 0.2 Ga 0.25 Al 0.35 Cu0.2 B 0.9 , at vacuum degree ≤10 -2 Different main phase alloys were melted in a vacuum medium frequency induction furnace at 10000 Pa, and main phase alloy flakes with a thickness of 0.32 mm were obtained by rapid solidification casting technology. Main phase alloy powders with an average particle size of 3.0 μm were prepared by hydrogen crushing and air flow grinding.

[0037] 2) According to the designed grain boundary reconstruction auxiliary alloy composition, the composition is Pr 20 Tb 60 Cu 10 Ga 10 , preparing grain boundary reconstruction auxiliary alloy powder with an average particle size of ~1.3μm through smelting, coarse crushing and ball milling;

[0038] 3) Under argon protection, the main phase alloy I and II powders with different compositions are uniformly mixed in a mass ratio of 15:1, and then uniformly mixed with the grain boundary reconstruction auxiliary alloy powder; wherein the grain boundary reconstruction auxiliary alloy powder accounts for 3.5% of the total powder mass; in terms of mass percentage, the composition of Pr 5.41 Nd 19.52 Tb 3.28 Fe bal Co 0.4 Nb 0.2 Ga 0.54 Al 0.34 Cu 0.49 B 0.87 Mixed alloy powder;

[0039] 4) Orienting and pressing the obtained mixed alloy powder in a magnetic field of 2.0 T to obtain a green body;

[0040] 5) The obtained green body is vacuum packaged, cold isostatically pressed at 200 MPa, and then sintered and heat treated in a high vacuum positive pressure sintering furnace at a sintering temperature of 1070°C for 3 hours, and a primary heat treatment at 900°C for 2.5 hours and a secondary heat treatment at 480°C for 3 hours to obtain a low-cost, high-performance multi-phase magnet. The test results of the AMT-4 permanent magnet property measuring instrument show that the magnetic properties of the magnet are B r =13.2kG, H cj =31.8kOe, (BH) max =43.1MGOe, reaching the performance of commercial N42EH brand magnets.

[0041] Comparative Example 3:

[0042] The difference from Example 2 is that the magnet is prepared by a conventional single-phase process, and the actual composition is the same as that of the magnet prepared in Example 2, which is Pr 5.41 Nd 19.52Tb 3.28 Fe bal Co 0.4 Nb 0.2 Ga 0.54 Al 0.34 Cu 0.49 B 0.87 The test results of AMT-4 permanent magnetic property measuring instrument show that the magnetic properties of the magnet are B r =12.8kG, H cj =25.4kOe, (BH) max =40.1MGOe, both lower than Example 2.

[0043] Comparative Example 4:

[0044] The difference from Example 2 is that the magnet is prepared by a conventional single-phase process, and the composition of the single-phase alloy is Pr 5.41 Nd 19.52 Tb 3.28 Fe bal Co 0.4 Nb 0.2 Ga 0.1 Al 0.2 Cu 0.2 B 1.05 , which is different from the composition of the mixed alloy powder in step 3) of Example 2 (the content of B is increased to 1.05wt.%, the content of Ga is reduced to 0.1wt.%, the content of Al is reduced to 0.2wt.%, and the content of Cu is reduced to 0.2wt.%). The test results of AMT-4 permanent magnetic property measuring instrument show that the magnetic properties of the magnet are B r =12.7kG, H cj =23.5kOe, (BH) max =38.9MGOe, both lower than Example 2.

[0045] Embodiment 3:

[0046] 1) The main phase components are prepared according to the designed main phase components. In terms of mass percentage, the main phase alloy I without heavy rare earth is composed of (Pr 0.2 Nd 0.8 ) 27.8 Fe bal Co 0.2 Zr 0.15 Ga 0.5 Al 0.25 Cu 0.2 B 0.88 The main phase alloy II with heavy rare earth addition has a composition of [(Pr 0.2 Nd 0.8 ) 0.25 Dy 0.75 ] 26.8Fe bal Co 0.2 Zr 0.15 Ga 0.5 Al 0.25 Cu 0.2 B 0.88 , at vacuum degree ≤10 -2 Different main phase alloys were melted in a vacuum medium frequency induction furnace at 1000 Pa, and main phase alloy flakes with a thickness of 0.37 mm were obtained by rapid solidification casting technology. Main phase alloy powders with an average particle size of 3.3 μm were prepared by hydrogen crushing and air flow grinding.

[0047] 2) According to the designed grain boundary reconstruction auxiliary alloy composition, the composition is Pr 20 Dy 20 Tb 40 Co 20 , preparing grain boundary reconstruction auxiliary alloy powder with an average particle size of ~1.5μm through smelting, coarse crushing and ball milling;

[0048] 3) Under nitrogen protection, the main phase alloy I and II powders with different compositions are uniformly mixed in a mass ratio of 19:1, and then uniformly mixed with the grain boundary reconstruction auxiliary alloy powder; wherein the grain boundary reconstruction auxiliary alloy powder accounts for 2% of the total powder mass; in terms of mass percentage, the composition of Pr 5.64 Nd 21.43 Dy 1.4 Tb 0.8 Fe bal Co 0.6 Zr 0.15 Ga 0.44 Al 0.34 Cu 0.2 B 0.86 Mixed alloy powder;

[0049] 4) Orienting and pressing the obtained mixed alloy powder in a magnetic field of 2 T to obtain a green body;

[0050] 5) The obtained green body is vacuum packaged, cold isostatically pressed at 200 MPa, and then sintered and heat treated in a high vacuum positive pressure sintering furnace. The sintering temperature is 1075°C, the sintering time is 4 hours, the primary heat treatment is carried out at 880°C for 2 hours, and the secondary heat treatment is carried out at 475°C for 4 hours to obtain a low-cost, high-performance multi-phase magnet. The test results of the AMT-4 permanent magnet property measuring instrument show that the magnetic properties of the magnet are B r =13.7kG, H cj =26.8kOe, (BH) max =46.8MGOe, reaching the performance of commercial N48UH brand magnets.

[0051] Embodiment 4:

[0052] 1) The main phase components are prepared according to the designed main phase components. In terms of mass percentage, the main phase alloy I without heavy rare earth is composed of (Pr 0.2 Nd 0.8 ) 28.8 Fe bal Co 0.2 Zr 0.2 Ga 0.2 Al 0.35 Cu 0.15 B 0.85 The main phase alloy II with heavy rare earth addition has a composition of [(Pr 0.2 Nd 0.8 ) 0.5 Dy 0.5 ] 26.4 Fe bal Co 0.2 Zr 0.2 Ga 0.2 Al 0.35 Cu 0.15 B 0.85 , at vacuum degree ≤10 -2 Different main phase alloys were melted in a vacuum medium frequency induction furnace at 10000 Pa, and main phase alloy flakes with a thickness of 0.35 mm were obtained by rapid solidification casting technology. Main phase alloy powders with an average particle size of 3.2 μm were prepared by hydrogen crushing and air flow grinding.

[0053] 2) The ingredients are prepared according to the designed grain boundary reconstruction auxiliary alloy composition, which is Dy in mass percentage. 20 Tb 60 Fe 10 Ga 10 , preparing grain boundary reconstruction auxiliary alloy powder with an average particle size of ~1.8μm through smelting, coarse crushing and ball milling;

[0054] 3) Under nitrogen protection, the main phase alloy I and II powders with different compositions are uniformly mixed in a mass ratio of 5:1, and then uniformly mixed with the grain boundary reconstruction auxiliary alloy powder; wherein the grain boundary reconstruction auxiliary alloy powder accounts for 3% of the total powder mass; in terms of mass percentage, the composition of Pr 4.88 Nd 19.50 Dy 2.74 Tb 1.8 Fe bal Co 0.2 Zr 0.2 Ga 0.5 Al 0.34 Cu 0.15 B 0.83 Mixed alloy powder;

[0055] 4) Orienting and pressing the obtained mixed alloy powder in a magnetic field of 1.8 T to obtain a green body;

[0056] 5) The obtained green body is vacuum packaged, cold isostatically pressed at 200 MPa, and then sintered and heat treated in a high vacuum positive pressure sintering furnace. The sintering temperature is 1060°C, the sintering time is 5 hours, the primary heat treatment is carried out at 890°C for 2 hours, and the secondary heat treatment is carried out at 490°C for 4 hours to obtain a low-cost, high-performance multi-phase magnet. The test results of the AMT-4 permanent magnet property measuring instrument show that the magnetic properties of the magnet are B r =13.2kG, H cj =31.4kOe, (BH) max =42.2MGOe, reaching the performance of commercial N42EH brand magnets.

Claims

1. A low-cost, high-performance multi-phase rare earth permanent magnet material. It is characterized in that The invention comprises a main phase alloy I without heavy rare earth, one or more main phase alloys II with heavy rare earth, and a grain boundary reconstruction auxiliary alloy; the main phase alloy I without heavy rare earth has a composition of RE in terms of mass percentage. x1 Q bal M y1 M' z1 B w1 , wherein RE is one or more of the other lanthanide rare earth elements except the heavy rare earth elements Dy and Tb, Q is one or more of the elements Fe, Co, and Ni, M is one or more of the elements Cr, Mn, Mo, N, Nb, P, Pb, Si, Ta, Ti, V, and Zr, M' is one or more of the elements Ga, Al, and Cu, and B is a boron element, wherein x1, y1, z1, and w1 satisfy the following relationship: 22≤x1≤30, 0≤y1≤2, 0.2≤z1≤1.0, and 0.8≤w1≤1.0; the main phase alloy II with the addition of heavy rare earth elements has an average composition of (RE in percentage by mass) 1-a HRE a ) x2 Q bal M y2 M' z2 B w2 , wherein RE is one or more of the other lanthanide rare earth elements except the heavy rare earth elements Dy and Tb, HRE is one or two of the heavy rare earth elements Dy and Tb, Q is one or more of the elements Fe, Co, and Ni, M is one or more of the elements Cr, Mn, Mo, N, Nb, P, Pb, Si, Ta, Ti, V, and Zr, M' is one or more of the elements Ga, Al, and Cu, and B is the boron element, wherein a, x2, y2, z2, and w2 satisfy the following relationship: 0.2≤a≤0.8, 22≤x2≤29, 0≤y2≤2, 0.2≤z2≤1.1, and 0.8≤w2≤0.95; the grain boundary reconstruction auxiliary alloy is calculated in mass percentage, and its composition is RE m TM 100-m , wherein RE is one or more of the rare earth La, Ce, Pr, Nd, Sm, Gd, Dy, Tb, Ho, Y, and contains at least one heavy rare earth element Dy or Tb; TM is one or more of H, O, F, Fe, Ga, Ti, Cu, Al, Co, Nb, Zr, Ta, Si, V, Mo, Mn, Ag, Mg, Zn, wherein 0 <m<100; Main phase alloy composition with low rare earth content, 22≤x1≤30, 22≤x2≤29, reducing material cost; The main phase grains of the final multi-main phase magnet present a core-shell structure, including two or more low heavy rare earth content n1 main phase grain cores and high heavy rare earth content n2 main phase grain cores, and high heavy rare earth content n3 main phase grain hard magnetic shells, wherein n1<n3<n2; its grain boundary phase includes a Q-rich grain boundary phase and a traditional rare earth-rich grain boundary phase, and the mass percentage of Q in the Q-rich grain boundary phase is 40% to 60%, and the mass percentage of M' is 1% to 9%; The Q-rich grain boundary phase and the traditional rare earth-rich grain boundary phase together form a continuous thin layer of grain boundary surrounding the adjacent main phase grains, ensuring the high coercivity of the magnet; The total rare earth element content in the Q-rich grain boundary phase is lower than that in the traditional rare earth-rich grain boundary phase, wherein the heavy rare earth content n4 is lower than the hard magnetic shell layer of the main phase grains with high heavy rare earth content n3, that is, n4<n3.

2. A method for preparing the low-cost, high-performance multi-phase rare earth permanent magnetic material as claimed in claim 1, It is characterized in that The following steps are involved: 1) According to the designed main phase components, the ingredients are prepared separately, and the vacuum degree is ≤10 -2 Different main phase alloys were melted in a vacuum medium frequency induction furnace at 1000 Pa, and main phase alloy flakes with a thickness of 0.2-0.6 mm were obtained by rapid solidification casting technology. Main phase alloy powders with an average particle size of 2-4 μm were prepared by hydrogen crushing and air flow grinding. 2) The ingredients are prepared according to the designed grain boundary reconstruction auxiliary alloy composition, and the grain boundary reconstruction auxiliary alloy powder with an average particle size of 0.5 to 3 μm is prepared through smelting, coarse crushing and ball milling; 3) Under nitrogen or argon protection, the main phase alloy powders of different components are uniformly mixed according to a proportion, and then uniformly mixed with the grain boundary reconstruction auxiliary alloy powder; wherein the grain boundary reconstruction auxiliary alloy powder accounts for 0.1 to 10% of the total powder mass; and mixed alloy powders with different heavy rare earth addition amounts are obtained; 4) Orienting and pressing the obtained mixed alloy powder in a magnetic field of 1.5 to 2.0 T to obtain a green body; 5) The obtained green body is vacuum packaged, cold isostatically pressed at 150-250 MPa, and then sintered and heat treated in a high vacuum positive pressure sintering furnace to obtain a low-cost, high-performance multi-phase magnet.

3. The method for preparing the low-cost, high-performance multi-phase rare earth permanent magnetic material according to claim 2, It is characterized in that In step 5), the sintering temperature is 980-1080° C. and the sintering time is 2-4 hours.

4. The method for preparing the low-cost, high-performance multi-phase rare earth permanent magnetic material according to claim 2, It is characterized in that In step 5), the heat treatment system is to carry out primary heat treatment at 800-950°C for 2-3 hours and secondary heat treatment at 450-700°C for 2-5 hours.

Citation Information

Patent Citations

  • Low-cost double-main phase Ce permanent-magnet alloy and preparation method thereof

    CN102800454A

  • (Nd,Y)-Fe-B rare earth permanent magnet and preparation method thereof

    CN107195414A

  • A preparation method of high-performance sintered Nd-Fe-B permanent magnet material

    CN109192493A

  • Lanthanum-cerium-yttrium-rich multi-principal-phase fine-grain rare earth permanent magnet material and preparation method thereof

    CN111091944A